Cellulose membrane as well as preparation method and application thereof

By using porous polystyrene microspheres and organic solvent treatment technology in cellulose membranes, the problem of insufficient breathability and wettability of lithium battery separators is solved, and a high-performance, degradable cellulose membrane preparation is achieved, suitable for lithium-ion batteries application.

CN118970360AActive Publication Date: 2024-11-15SENIOR (NANTONG) NEW MATERIAL TECH CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411007327.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-15
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

While taking into account both mechanical properties and heat resistance, the existing lithium battery separators have poor breathability and wetting properties, making it difficult to degrade in a natural environment.

Method used

Porous polystyrene microspheres are used as pore-forming agent and mixed with cellulose. Through specific organic solvent treatment and molding processes, the mass ratio between cellulose and pore-forming agent is controlled to form a uniform micropore structure and improve the pores of cellulose membrane. Rate and breathability.

Benefits of technology

While maintaining mechanical properties and heat resistance, the breathability and wetting properties of the cellulose film are significantly improved. It is suitable for the electrolyte infiltration and transmission of lithium ions in lithium-ion batteries, and has degradable properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970360A_ABST
    Figure CN118970360A_ABST
Patent Text Reader

Abstract

The invention provides a cellulose membrane and a preparation method and application thereof, the preparation method comprises the following steps: (1) mixing and dispersing cellulose and a first pore forming agent to obtain a dispersion; (2) molding the dispersion obtained in the step (1) to obtain a first membrane material; and (3) mixing the first membrane material obtained in the step (2) with a second organic solvent to obtain the cellulose membrane, wherein the first pore forming agent comprises porous polystyrene microspheres; on the basis of solid mass, the mass ratio of the cellulose to the first pore-forming agent is 1: (0.5-1.6); the first pore-forming agent can be dissolved in the second organic solvent. According to the invention, the cellulose membrane obtained by adopting a specific process has good heat resistance, air permeability and wettability, and is beneficial to transmission of lithium ions and infiltration of electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of diaphragm materials, and in particular relates to a cellulose membrane and a preparation method and application thereof. Background Art

[0002] At present, the mainstream lithium battery separators in the market are mainly polyolefin separators. Polyolefin separators are mainly made of petrochemical raw materials and are difficult to degrade in the natural environment. At the same time, the existing production process is difficult to take into account the mechanical properties and heat resistance of the separator. Therefore, it is necessary to find a separator with degradable properties and high performance as a substitute. Cellulose is widely distributed in nature and has biodegradable properties. Pure fiber-coated separators have the characteristics of light weight and high heat resistance. However, since the surface of cellulose contains rich hydroxyl functional groups, hydrogen bonding forces will be formed in water. During the drying process, due to capillary action, nanofibers are easy to form a dense network, which hinders the migration of lithium ions and leads to poor air permeability and wetting properties of the separator.

[0003] Therefore, developing a method for preparing a cellulose membrane having excellent mechanical properties, heat resistance, air permeability and wettability is an urgent problem to be solved in the art. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention aims to provide a cellulose film and a preparation method and application thereof. The cellulose film obtained by the specific preparation method of the present invention can improve the air permeability and wettability of the cellulose film while retaining the mechanical properties, heat resistance and lightness of the cellulose film.

[0005] To achieve this object, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a method for preparing a cellulose film, the method comprising the following steps:

[0007] (1) Mixing and dispersing cellulose and a first pore-forming agent to obtain a dispersion; (2) Molding the dispersion obtained in step (1) to obtain a first membrane material; (3) Mixing the first membrane material obtained in step (2) with a second organic solvent to obtain the cellulose membrane; wherein the first pore-forming agent comprises porous polystyrene microspheres (porous PS microspheres); based on solid mass, the mass ratio of the cellulose to the first pore-forming agent is 1:(0.5-1.6); and the first pore-forming agent can be dissolved in the second organic solvent.

[0008] In the present invention, the porous polystyrene microspheres have a large specific surface area and a high porosity, and can be more evenly embedded in the cellulose matrix. The porous polystyrene microspheres are then removed by a second organic solvent, thereby leaving a large number of evenly distributed microporous structures in the cellulose matrix, improving the porosity of the cellulose membrane, and while ensuring the mechanical properties and heat resistance of the cellulose membrane, the air permeability and wettability of the cellulose membrane can be improved; at the same time, controlling the mass ratio of cellulose to the first pore-forming agent within a specific range can further improve the air permeability, heat resistance and wettability of the cellulose membrane; the cellulose membrane obtained by the specific method of the present invention has good mechanical properties, heat resistance, air permeability and wettability, is more conducive to the infiltration of electrolytes and the transmission of lithium ions, and is light in weight.

[0009] In the present invention, based on solid mass, the mass ratio of the cellulose to the first pore-forming agent is 1:(0.5-1.6), wherein the specific value of (0.5-1.6) can be, for example, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1, 1.1, 1.2, 1.3, 1.4, 1.5, etc.

[0010] Preferably, the cellulose in step (1) comprises nanocellulose.

[0011] Preferably, the cellulose comprises at least one of cellulose nanocrystals (CNC), nanofiber filaments (CNF) or bacterial cellulose (BC).

[0012] In the present invention, the diameter of the nanocellulose is 5-20 nm and the length is 50-100 nm.

[0013] Preferably, the cellulose and / or the first membrane material is treated with a first organic solvent, the polarity of the first organic solvent is less than that of water, and the boiling point of the first organic solvent is less than 100°C, for example, it can be 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 98°C, etc.

[0014] In the present invention, by treating cellulose and / or the first membrane material with an organic solvent of low polarity and low boiling point, the capillary action of cellulose during the drying process can be reduced, the distance between cellulose chains becomes relatively larger, and the pore structure of the cellulose membrane is increased, thereby further improving the air permeability and wettability of the cellulose membrane.

[0015] In the present invention, the cellulose is in the form of a cellulose dispersion having a solid content of 3-5%, for example, 3%, 3.2%, 3.4%, 3.6%, 3.8%, 4%, 4.2%, 4.4%, 4.6%, 4.8%, 5%, etc.

[0016] In the present invention, the solvent of the cellulose dispersion includes water.

[0017] Preferably, the raw materials for preparing the porous polystyrene microspheres include styrene monomers, a second pore-forming agent, a dispersant, an initiator and a solvent.

[0018] Preferably, the mass ratio of the second pore-forming agent to the styrene monomer is (1-3):1, wherein the specific values ​​of 1-3 can be, for example, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3, etc.; further preferably, it is (1-2):1.

[0019] In the present invention, the content of the second pore-forming agent affects the porosity, pore size and specific surface area of ​​the porous polystyrene microspheres; when the content of the second pore-forming agent is low, the porosity of the porous polystyrene microspheres decreases, the pore size decreases, and the specific surface area decreases; when the content is high, the porosity is not significantly improved, and the porous polystyrene microspheres are easily broken. The reasons are: the content of the second pore-forming agent is high, the relative concentration of the monomer decreases, and the viscosity is too low during the polymerization process; and it is easy to cause pore formation failure, and the obtained polystyrene microspheres have low porosity and small pore size.

[0020] Preferably, the second pore forming agent comprises polyethylene glycol.

[0021] Preferably, the mass percentage of the dispersant in the preparation raw material is 0.5-0.8%, for example, it can be 0.5%, 0.52%, 0.54%, 0.56%, 0.58%, 0.6%, 0.62%, 0.64%, 0.66%, 0.68%, 0.7%, 0.72%, 0.74%, 0.76%, 0.78%, 0.8%, etc.

[0022] In the present invention, the dispersant affects the D50 particle size of the porous polystyrene microspheres; when the amount of the dispersant is too low, the D50 particle size of the porous polystyrene microspheres increases; when the amount of the dispersant is too high, the D50 particle size of the porous polystyrene microspheres decreases; when the amount of the dispersant is within the above range, porous polystyrene microspheres with a suitable D50 particle size can be obtained, thereby obtaining a cellulose film with good wettability and air permeability.

[0023] In the present invention, the mass percentage of the dispersant is 0.5-0.8%, which refers to the mass percentage of the solid mass of the dispersant in the entire system, including the solvent.

[0024] Preferably, the dispersant includes any one of polyvinyl alcohol, sodium dodecylbenzene sulfonate, glycerol, and polymethyl acrylate, or a mixture of at least two of them.

[0025] In the present invention, by making the polystyrene microspheres porous, that is, adding a specific content of a second pore-forming agent and a specific content of a dispersant, the particle size, porosity and pore size of the polystyrene microspheres can be controlled within an appropriate range, so that the polystyrene microspheres are evenly dispersed in the cellulose matrix, the porosity of the cellulose membrane is increased, and a cellulose membrane with high air permeability, high wettability, heat resistance and good mechanical properties is obtained.

[0026] Preferably, the styrene monomer includes styrene and / or divinylbenzene.

[0027] Preferably, the styrene monomers include styrene and divinylbenzene, and the mass ratio of styrene to divinylbenzene is (40-60):1, wherein the specific value of (40-60) can be, for example, 40, 42, 44, 46, 48, 50, 52, 54, 56, 58, 60, etc.

[0028] Preferably, the amount of the initiator is 1-5% of the mass of styrene, for example, 1%, 1.2%, 1.4%, 1.6%, 1.8%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, etc.

[0029] In the present invention, the initiator includes but is not limited to benzoyl peroxide; the solvent includes water.

[0030] Preferably, the method for preparing the porous polystyrene microspheres comprises:

[0031] The styrene monomer, the second pore-forming agent, the dispersant, the initiator and the solvent are mixed and reacted, and the second pore-forming agent is removed to obtain the porous polystyrene microspheres.

[0032] In the present invention, the dispersant can reduce the surface tension of the liquid, so that the monomer liquid is more dispersed, and can also increase the viscosity of the polymer medium, thereby hindering the collision and bonding between the monomer droplets. It can also form a protective film on the surface of the monomer droplets to prevent the droplets from condensing and play a steric role; the second pore-forming agent can participate in pore making and increase the porosity of the polystyrene microspheres; the polystyrene microspheres are prepared by suspension polymerization, and the styrene monomer is suspended in the polymerization medium in the form of small droplets after stirring and dispersing. Since the small droplets are surrounded by the polymerization medium, the polymerization heat can be directly and effectively removed; the small droplets first undergo bulk polymerization, and when the conversion rate reaches a certain level, the liquid surface becomes sticky and easily sticks into blocks; when the dispersant is added, the droplets can be stabilized. When the conversion rate is further increased, the small droplets gradually harden and the risk of bonding is reduced; in the later stage of the reaction, as the concentration of the reactants decreases, the second pore-forming agent dispersed in the water participates in pore making, thereby obtaining porous polystyrene microspheres.

[0033] Preferably, the mixing comprises: pre-mixing and dispersing the solvent and the second pore-forming agent, and then adding the styrene monomer, the dispersant and the initiator thereto and mixing them.

[0034] Preferably, the premixing and dispersing temperature is 80-85°C, for example, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, etc.; the rotation speed is 200-300rpm, for example, 200rpm, 220rpm, 240rpm, 260rpm, 280rpm, 300rpm, etc.; the premixing and dispersing is performed until the second pore-forming agent is fully dissolved.

[0035] Preferably, the reaction is carried out in the presence of a protective atmosphere; the protective atmosphere includes but is not limited to nitrogen; the reaction temperature is 80-90°C, for example, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 88°C, 90°C, etc.; the reaction time is 8-10h, for example, 8h, 9h, 10h, etc.

[0036] Preferably, the method of removing the second pore forming agent comprises extraction.

[0037] In the present invention, the extraction method comprises placing the polystyrene microspheres obtained by the reaction into a solvent capable of dissolving the second pore-forming agent (including but not limited to dichloromethane), removing the second pore-forming agent, and then drying at 50-60° C. to obtain porous polystyrene microspheres.

[0038] Preferably, the D50 particle size of the porous polystyrene microspheres is 0.8-1.2 μm, for example, it can be 0.8 μm, 0.82 μm, 0.84 μm, 0.85 μm, 0.86 μm, 0.88 μm, 0.9 μm, 0.92 μm, 0.94 μm, 0.95 μm, 0.96 μm, 0.98 μm, 1 μm, 1.02 μm, 1.04 μm, 1.06 μm, 1.08 μm, 1.1 μm, 1.12 μm, 1.14 μm, 1.16 μm, 1.18 μm, 1.2 μm, etc.

[0039] In the present invention, by controlling the D50 particle size of the porous polystyrene microspheres within a specific range, the porosity of the cellulose membrane can be regulated, thereby obtaining a cellulose membrane with high wettability and air permeability; if the D50 particle size of the porous polystyrene microspheres is too small, the porosity of the cellulose membrane is reduced, and a small particle size will result in an excessively large specific surface area. As time goes by, the porous polystyrene microspheres are prone to agglomeration, and the viscosity of the dispersion will rise sharply, affecting the fluidity of the dispersion, and the microspheres cannot be evenly dispersed in the cellulose dispersion, affecting the air permeability, wettability or heat resistance of the cellulose membrane; if the D50 particle size is too large, the improvement of the porosity is not obvious, and the microspheres cannot be completely removed in the later stage, resulting in the porous polystyrene microspheres remaining in the cellulose membrane, resulting in abnormal phenomena such as black spots on the surface of the cellulose membrane and uneven membrane surface, affecting the membrane-related properties.

[0040] In the present invention, other conditions are the same, the thickness of the cellulose membrane is 5-10 μm, when the D50 particle size of the porous polystyrene microspheres is in the range of 0.8-1.2 μm, the corresponding cellulose membrane has a porosity of 42-48%, a pore size of 42-45 nm, and an air permeability of 165-195 s / 100 cc.

[0041] Preferably, the porosity of the porous polystyrene microspheres is 45-75%, for example, it can be 45%, 46%, 48%, 50%, 52%, 54%, 56%, 58%, 60%, 62%, 64%, 66%, 68%, 70%, 72%, 74%, 75%, etc.

[0042] Preferably, the pore size of the porous polystyrene microspheres is 9-20 nm, for example, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm, etc.

[0043] Preferably, the specific surface area of ​​the porous polystyrene microspheres is 85-170 m 2 / g, for example, 85m 2 / g, 90m 2 / g, 95m 2 / g、100m 2 / g、105m 2 / g, 110m 2 / g, 115m 2 / g, 120m 2 / g, 125m 2 / g, 130m 2 / g, 135m 2 / g, 140m 2 / g, 145m 2 / g, 150m 2 / g, 155m2 / g, 160m 2 / g, 165m 2 / g, 170m 2 / g, etc.

[0044] Preferably, the rotation speed of the mixing and dispersing in step (1) is 1500-2000rpm, for example, it can be 1500rpm, 1600rpm, 1700rpm, 1800rpm, 1900rpm, 2000rpm, etc.; the time is 2-4h, for example, it can be 2h, 2.5h, 3h, 3.5h, 4h, etc.

[0045] Preferably, step (2) further includes a step of degassing the dispersion before molding.

[0046] In the present invention, the degassing method includes degassing by vacuuming.

[0047] Preferably, the molding method in step (2) includes casting molding.

[0048] Preferably, the molding temperature in step (2) is 45-55°C, for example, 45°C, 46°C, 48°C, 50°C, 52°C, 54°C, 55°C, etc.

[0049] In the present invention, the casting molding comprises casting the dispersion obtained in step (1) into a glass model with a fixed thickness for molding; the thickness of the glass model is 5 to 10 μm.

[0050] Preferably, the first organic solvent comprises an alcohol solvent.

[0051] Preferably, the alcohol solvent includes at least one of methanol, ethanol, 1-propanol, isopropanol, 2,2,2-trifluoroethanol, 2-butanol and isobutanol.

[0052] Preferably, the mass concentration of the first organic solvent is ≥98%.

[0053] Preferably, the method of treating with the first organic solvent comprises: soaking cellulose and / or the first membrane material in the first organic solvent, and drying to obtain a treated material.

[0054] Since water and the hydroxyl groups in cellulose will form hydrogen bonds, when cellulose is dried, as the water molecules are gradually evaporated, the cellulose chains will be closer together, the pore structure of cellulose will become smaller, and a dense network structure will be formed; and by selecting a first organic solvent with a low boiling point and low polarity for treatment, the capillary effect between the fibers can be reduced, the distance between the cellulose chains can be relatively increased, and the pore structure of the fibers can be relatively increased, thereby improving the air permeability and wettability of the cellulose membrane.

[0055] Preferably, the immersion time in the first organic solvent is 12-20 h, for example, it can be 12 h, 13 h, 14 h, 15 h, 16 h, 17 h, 18 h, 19 h, 20 h, etc.

[0056] Preferably, the drying temperature after the first organic solvent treatment is 60-75°C, for example, 60°C, 62°C, 64°C, 66°C, 68°C, 70°C, 72°C, 74°C, 75°C, etc.; the drying time is 1-3h, for example, 1h, 1.5h, 2h, 2.5h, 3h, etc.

[0057] Preferably, the second organic solvent in step (3) comprises at least one of toluene, tetrahydrofuran, acetone, butanone, ethyl acetate, N,N-dimethylformamide, chloroform, benzene or xylene.

[0058] In the present invention, the second organic solvent can dissolve the porous polystyrene microspheres, thereby forming a large number of pore structures in the cellulose membrane, improving the porosity of the cellulose membrane, and further improving the air permeability and wettability of the cellulose membrane.

[0059] Preferably, the mixing method in step (3) comprises: immersing the first film material in the second organic solvent.

[0060] In the present invention, if the first film material is treated with a first organic solvent, the first film material is treated with the first organic solvent and then mixed with the second organic solvent.

[0061] Preferably, the immersion time in the second organic solvent is 5-7 hours, for example, 5 hours, 5.5 hours, 6 hours, 6.5 hours, 7 hours, etc.; and the temperature is room temperature.

[0062] Preferably, step (3) further includes a drying step after the mixing.

[0063] In the present invention, the drying temperature is 100-110° C. and the drying time is 1-2 hours.

[0064] As a preferred technical solution of the present invention, the preparation method comprises the following steps:

[0065] (1) mixing and dispersing the cellulose material and the first pore-forming agent at 1500-2000 rpm for 2-4 hours to obtain a dispersion; based on solid mass, the mass ratio of the cellulose to the first pore-forming agent is 1:(0.5-1.6);

[0066] (2) casting the dispersion obtained in step (1) at 45-55° C. to obtain a first film material; soaking the first film material in a first organic solvent for 12-20 hours, and drying at 60-75° C. for 1-3 hours to obtain a treated first film material;

[0067] (3) Soaking the treated first membrane material obtained in step (2) in a second organic solvent at room temperature for 5-7 hours and drying to obtain the cellulose membrane.

[0068] In the present invention, the solid-liquid ratio when the first film material is immersed in the first organic solvent in step (2) and the solid-liquid ratio when the treated first film material obtained in step (2) is immersed in the second organic solvent in step (3) are each independently 1:(5-8), wherein the specific value in (5-8) can be, for example, 5, 5.5, 6, 6.5, 7, 7.5, 8, etc.

[0069] In the present invention, it is preferred to use a first organic solvent to treat the first membrane material, which can not only reduce the capillary effect between cellulose and increase the pore structure; it can also accelerate the evaporation of carried water through the low boiling point, dehydrate the polystyrene-cellulose dispersion into a gel state, further reduce the capillary effect, increase the pore size, and shorten the process flow and reduce costs.

[0070] In a second aspect, the present invention provides a cellulose film, wherein the cellulose film is prepared according to the preparation method described in the first aspect.

[0071] Preferably, the porosity of the cellulose membrane is 40-50%, for example, 40%, 40.5%, 41%, 41.5%, 42%, 42.5%, 43%, 43.5%, 44%, 44.5%, 45%, 45.5%, 46%, 46.5%, 47%, 47.5%, 48%, 49%, 50% and the like.

[0072] In the present invention, the thickness of the cellulose film is 5-10 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, etc.

[0073] In a third aspect, the present invention provides a membrane, comprising a cellulose membrane prepared according to the preparation method of the first aspect or a cellulose membrane according to the second aspect.

[0074] In a fourth aspect, the present invention provides a lithium ion battery, wherein the lithium ion battery comprises the cellulose membrane prepared according to the preparation method of the first aspect or the separator according to the third aspect.

[0075] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0076] Compared with the prior art, the present invention has the following beneficial effects:

[0077] The preparation method provided by the present invention selects porous polystyrene microspheres as pore-forming agents, and controls the mass ratio of the first pore-forming agent to cellulose within a specific range, thereby improving the air permeability and wettability of the cellulose membrane while ensuring the mechanical properties and heat resistance of the cellulose membrane; it is more conducive to the infiltration of electrolytes and the transmission of lithium ions, and is lightweight. BRIEF DESCRIPTION OF THE DRAWINGS

[0078] Figure 1 A transmission electron micrograph of the porous polystyrene microspheres provided in Preparation Example 1 of the present invention;

[0079] Figure 2 The infrared spectrum of the porous polystyrene microspheres provided in Preparation Example 1 of the present invention;

[0080] Figure 3 This is a scanning electron microscope image of the cellulose film obtained in Example 1 of the present invention;

[0081] Figure 4 In the preparation methods provided in Example 1, Example 14 and Comparative Example 1 of the present invention, a weight change curve of the first film material is shown as the immersion time in toluene increases. DETAILED DESCRIPTION

[0082] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0083] Preparation Example 1

[0084] This preparation example provides a porous polystyrene microsphere, and the preparation method of the porous polystyrene microsphere comprises the following steps:

[0085] At a temperature of 85°C and a rotation speed of 200 r / min, deionized water and polyethylene glycol (PEG) are mixed and stirred until PEG is fully dissolved; nitrogen is introduced, styrene (ST) and divinylbenzene (DVB) are added thereto, the dispersion speed is adjusted to 400 r / min, benzoyl peroxide (BPO) and polyvinyl alcohol (PVA) are added thereto, and after reacting at 85°C for 9 hours, white PS microspheres are obtained after cooling and rotary evaporation; the PS microspheres are placed in a dichloromethane solvent, residual PEG is removed by extraction, and the porous PS microspheres are obtained after drying in an oven at 60°C; wherein the mass of PEG (M PEG ) and the total quality of ST and DVB (M ST+DVB ) ratio is 2:1; the mass ratio of ST to DVB is 50:1; the mass of BPO is 1.5% of the mass of ST; the mass of PVA (M PVA ) accounts for 0.65% of the total mass of the system.

[0086] The morphology of the porous PS microspheres obtained in Preparation Example 1 was characterized by transmission electron microscopy. Figure 1 shown by Figure 1 It can be seen that the porous PS microspheres have a pore structure and present a certain core-shell structure.

[0087] The structure of the porous PS microspheres obtained in Preparation Example 1 was characterized by Fourier transform infrared spectroscopy. Figure 2 shown by Figure 2 It can be seen that 2922cm -1 、1492cm -1 and 1452cm -1 The absorption peak at 668 cm is the characteristic absorption peak of the benzene ring skeleton vibration. -1 The peak at represents the characteristic CH plane vibration of the benzene ring, and there is no characteristic absorption peak of vinyl C=C, which means that the polymerization reaction is successful and a copolymer of styrene and divinylbenzene is obtained.

[0088] Preparation Examples 2 to 10, Comparative Preparation Example 1

[0089] Preparation Examples 2 to 9 respectively provide a porous PS microsphere, which differs from Preparation Example 1 only in that the contents of PEG and PVA are different (see Table 1 for details), and other raw materials, amounts and preparation methods are the same as those in Preparation Example 1.

[0090] Preparation Example 10 provides a porous PS microsphere, which is different from Preparation Example 1 only in that the dispersant is polymethyl acrylate, and the other raw materials, amounts and preparation methods are the same as those in Preparation Example 1.

[0091] Comparative Preparation Example 1 provides a PS microsphere, in which PEG and PVA are not added to the preparation raw materials, and other raw materials, amounts and preparation methods are the same as those in Preparation Example 1.

[0092] The formulations of Preparation Examples 1 to 10 and Comparative Preparation Example 1, as well as the obtained PS microspheres' D50 particle size, porosity, pore size and specific surface area are shown in Table 1; wherein, " / " in Table 1 indicates that no test is required or cannot be obtained.

[0093] D50 particle size of PS microspheres (test method): The dispersion was tested using a TOPSIZER laser particle size analyzer, and the corresponding refractive index was selected to obtain the cumulative particle size distribution of the dispersion. The particle size at which 50% of the total particle size was accumulated from the particle side was recorded as D50.

[0094] Porosity test method: Use the water saturation method to test, place the PS microsphere sample to be tested in a vacuum container, then apply a certain vacuum pressure to evacuate the gas in the container, then connect the vacuum container to a water tank, inject the water in the water tank into the container, apply a certain water pressure to the sample, and then measure the water level change to calculate the porosity.

[0095] Pore ​​size test method: The mercury intrusion method is used to test, in which mercury is forced into the pores of the material by applying external pressure, and the pore size of the pore structure of the PS microsphere sample is directly obtained by measuring the amount of mercury entering.

[0096] Specific surface area test method: refer to GB / T 19587-2004.

[0097] Table 1

[0098]

[0099] Example 1

[0100] This embodiment provides a method for preparing a cellulose film, which specifically comprises the following steps:

[0101] (1) 50 g of porous PS microspheres (Preparation Example 1, M PEG :M ST+DVB =2:1) ​​was mixed with 833 mL of cellulose nanocrystal dispersion (CNC dispersion, solvent is water, solid content is 4%, CNC diameter is 8-10 nm, length is 50-100 nm), and dispersed at a speed of 1500 rpm for 3 h to obtain a uniformly dispersed dispersion (labeled as CNC&PS);

[0102] (2) After vacuum degassing, the CNC&PS dispersion obtained in step (1) is uniformly cast into a glass model with a fixed thickness (7 μm) at a casting temperature of 50° C. to obtain a first film material; according to a solid-liquid ratio of 1:6, the first film material is immersed in an ethanol solution (mass concentration of 99 wt%) for 12 h (dehydration) to obtain a CNC&PS gel; and the obtained gel is then baked in an oven at 65° C. for 2 h to obtain a CNC&PS film;

[0103] (3) The baked CNC&PS membrane was placed in a toluene solution (mass concentration 50 wt%) at a solid-liquid ratio of 1:8, and after being left for 6 hours, it was baked in an oven at 105° C. for 1.5 hours to obtain the cellulose membrane.

[0104] The morphology of the cellulose film prepared by the method provided in Example 1 was characterized by scanning electron microscopy. Figure 3 As shown; it can be clearly seen from the figure that the surface of the cellulose membrane has a microporous structure, indicating that the porosity of the cellulose membrane is significantly improved.

[0105] Example 2

[0106] This embodiment provides a method for preparing a cellulose film, which specifically comprises the following steps:

[0107] (1) 50 g of porous PS microspheres (Preparation Example 1) were mixed with 833 mL of cellulose nanocrystal dispersion (CNC dispersion, solvent: water, solid content: 4%, CNC diameter: 8-10 nm, length: 50-100 nm), and dispersed at a speed of 2000 rpm for 4 h to obtain a uniformly dispersed dispersion (labeled as CNC&PS);

[0108] (2) After vacuum degassing, the CNC&PS dispersion obtained in step (1) is uniformly cast into a glass model with a fixed thickness (7 μm) at a casting temperature of 55° C. to obtain a first film material; according to a solid-liquid ratio of 1:6, the first film material is immersed in an ethanol solution (mass concentration of 99 wt%) for 18 h (dehydration) to obtain a CNC&PS gel; and the obtained gel is then baked in an oven at 75° C. for 3 h to obtain a CNC&PS film;

[0109] (3) The baked CNC&PS membrane was placed in an acetone solution (mass concentration 99.5 wt%) at a solid-liquid ratio of 1:8, and after being placed for 7 hours, it was baked in an oven at 105° C. for 2 hours to obtain the cellulose membrane.

[0110] Embodiments 3 to 11

[0111] Examples 3 to 11 respectively provide a method for preparing a cellulose membrane, which differs from Example 1 only in that the porous PS microspheres are provided by Preparation Examples 2 to 10 respectively, and the other components, amounts and process parameters are the same as those in Example 1.

[0112] Example 12

[0113] This embodiment provides a method for preparing a cellulose membrane, which differs from Embodiment 1 only in that the content of porous PS microspheres is adjusted so that the mass ratio of CNC to porous PS microspheres is 1:0.5 (based on solid mass), and other components, amounts and process parameters are the same as those in Embodiment 1.

[0114] Embodiment 13

[0115] This embodiment provides a method for preparing a cellulose membrane, which differs from Embodiment 1 only in that the content of porous PS microspheres is adjusted so that the mass ratio of CNC to porous PS microspheres is 1:1 (based on solid mass), and other components, amounts and process parameters are the same as those in Embodiment 1.

[0116] Embodiment 14

[0117] This embodiment provides a method for preparing a cellulose film, which differs from Embodiment 1 only in that, in step (2), no ethanol solution is used for soaking treatment, and the first film material is directly baked in an oven at 65° C. for 2 h. The other steps are the same as those in Embodiment 1.

[0118] Embodiment 15

[0119] This embodiment provides a method for preparing a cellulose film, which differs from Embodiment 1 only in that the ethanol solution is replaced with propylene glycol methyl ether of equal mass, and the other steps are the same as those in Embodiment 1.

[0120] Comparative Example 1

[0121] This comparative example provides a method for preparing a cellulose membrane, which differs from Example 1 only in that, in the preparation method, porous PS microspheres are not added and ethanol solution is not used for soaking treatment, and other steps are the same as those in Example 1.

[0122] Comparative Example 2

[0123] This comparative example provides a method for preparing a cellulose membrane, which differs from Example 1 only in that the porous PS microspheres are replaced with the PS microspheres provided in Comparative Preparation Example 1 of equal mass, and the other steps are the same as those in Example 1.

[0124] Comparative Example 3

[0125] This comparative example provides a method for preparing a cellulose membrane, which differs from Example 1 only in that the content of porous PS microspheres is adjusted so that the mass ratio of CNC to porous PS microspheres is 1:5 (based on solid mass), and other components, amounts and process parameters are the same as those in Example 1.

[0126] Comparative Example 4

[0127] This comparative example provides a method for preparing a cellulose membrane, which differs from Example 1 only in that the content of porous PS microspheres is adjusted so that the mass ratio of CNC to porous PS microspheres is 1:0.3 (based on solid mass), and other components, amounts and process parameters are the same as those in Example 1.

[0128] Performance Testing

[0129] (1) Observe the weight change of the first film material in toluene

[0130] Taking Example 1, Example 14 and Comparative Example 1 as examples, the weight of the membrane material was weighed at different times during the toluene immersion process. The results are as follows: Figure 4 shown by Figure 4It can be seen that the weight of the pure cellulose film (Comparative Example 1) in toluene does not change, which indirectly proves that cellulose has good stability in toluene solution; in Example 1 and Example 14, the weight of the first film material drops sharply in the early stage, and then reaches a state of equilibrium until the PS balls are completely dissolved and stabilized. However, the time to reach the equilibrium point is 22 minutes (Example 1) and 30 minutes (Example 14), respectively. The first film material obtained by the preparation method provided by the present invention reaches the equilibrium time point in a shorter time, indicating that the permeability and porosity of the two films are also different; according to the porosity and permeability performance, the arrangement is from large to small: Example 1> Example 14> Comparative Example 1.

[0131] (2) Breathability

[0132] The air permeability index reflects the smoothness of lithium ion transmission in the channel of the lithium battery. If the air permeability value is too large, it will cause difficulty in lithium ion transmission and easily lead to battery short circuit.

[0133] In the present invention, the standard method for testing the air permeability value of cellulose membrane is: GB / T36363-2018.

[0134] (3) Standard method for testing the porosity of cellulose membranes: GB / T36363-2018.

[0135] (4) Thermal stability

[0136] Thermal stability is an important indicator for evaluating the performance of diaphragms. Taking polyolefin diaphragms as an example, when the temperature rises to the melting temperature of polyolefin diaphragms, diaphragms with high thermal stability can maintain dimensional integrity at high temperatures and block direct contact between the positive and negative electrodes.

[0137] In the present invention, the standard method for testing the thermal stability of cellulose membrane is GB / T12027-2004.

[0138] The cellulose film was heat treated at 180°C for 60 min, and the transverse (TD) and longitudinal (MD) dimensions of the cellulose film before and after the treatment were measured, and the thermal shrinkage was calculated; wherein, thermal shrinkage = (dimension before treatment - dimension after treatment) / dimension before treatment × 100%.

[0139] (5) Wetting performance

[0140] The electrolyte wettability of the separator is a key performance of lithium-ion separators and an important indicator that directly reflects the lithium-ion transmission performance and electrolyte penetration. The electrolyte absorption rate shows the difference between the wettability through the contact angle characteristics. The specific test method refers to GB / T30447-2018.

[0141] The polyolefin separator was used as the control group.

[0142] Control group: polyethylene diaphragm (SW807C, Shenzhen Xingyuan Material Technology Co., Ltd.), thickness of 7 μm.

[0143] The specific test results are shown in Table 2:

[0144] Table 2

[0145]

[0146]

[0147] It can be seen from Table 2 that the cellulose membrane surface obtained by the specific preparation method of the present invention has polar groups, large pore size and high porosity; therefore, the membrane has a small air permeability value, good air permeability, and is more conducive to the transmission of lithium ions; it has good heat resistance and low thermal shrinkage when treated at 180°C; and it has a low contact angle and good wettability to the electrolyte.

[0148] It can be seen from Comparative Example 1 that the air permeability of the obtained cellulose membrane exceeds the standard when porous PS microspheres are not added and ethanol solution is not used for treatment in the preparation method. The reason is that during the CNC drying process, the strong hydrogen bonding and capillary action around the cellulose surface cause the distance between the cellulose fibers to be shortened, resulting in the almost closed porosity of the diaphragm, which hinders the transmission of lithium ions to a certain extent; and the contact angle of the cellulose membrane increases, and the wettability is slightly poor.

[0149] It can be seen from Comparative Example 2 that the first pore-forming agent is not porous polystyrene microspheres, but polystyrene microspheres are used instead, and the air permeability, thermal stability and wettability of the cellulose membrane are all deteriorated.

[0150] It can be seen from Comparative Examples 3 and 4 that the mass ratio of the first pore-forming agent to cellulose is not within the range specified in the present invention, the thermal stability of the cellulose membrane deteriorates, and the air permeability is slightly reduced.

[0151] It can be seen from Example 14 that when the preparation method does not use ethanol solution for treatment, the air permeability and contact angle of the obtained cellulose membrane are slightly higher, and the air permeability and wettability of the cellulose membrane are slightly worse.

[0152] It can be seen from the control group that, compared with the polyolefin separator, the cellulose membrane obtained by the present invention has better air permeability, heat resistance and electrolyte wettability.

[0153] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a cellulose film, characterized in that: The preparation method comprises the following steps: (1) mixing and dispersing cellulose and a first pore-forming agent to obtain a dispersion; (2) forming the dispersion obtained in step (1) to obtain a first film material; (3) mixing the first membrane material obtained in step (2) with a second organic solvent to obtain the cellulose membrane; Wherein, the first pore-forming agent comprises porous polystyrene microspheres; Calculated on a solid basis, the mass ratio of the cellulose to the first pore-forming agent is 1:(0.5-1.6); The first pore former is soluble in the second organic solvent.

2. The preparation method according to claim 1, characterized in that: The cellulose in step (1) comprises nanocellulose; Preferably, the cellulose comprises at least one of cellulose nanocrystals, nanofiber filaments or bacterial cellulose; Preferably, the cellulose and / or the first film material is treated with a first organic solvent, the polarity of the first organic solvent is less than that of water, and the boiling point of the first organic solvent is less than 100°C.

3. The preparation method according to claim 1 or 2, characterized in that: The raw materials for preparing the porous polystyrene microspheres include styrene monomers, a second pore-forming agent, a dispersant, an initiator and a solvent; Preferably, the mass ratio of the second pore-forming agent to the styrene monomer is (1-3):1, more preferably (1-2):1; Preferably, the second pore-forming agent comprises polyethylene glycol; Preferably, the mass percentage of the dispersant in the preparation raw material is 0.5-0.8%; Preferably, the dispersant includes any one of polyvinyl alcohol, sodium dodecylbenzene sulfonate, glycerol, and polymethyl acrylate, or a mixture of at least two thereof; Preferably, the styrene monomer comprises styrene and / or divinylbenzene; Preferably, the styrene monomers include styrene and divinylbenzene, and the mass ratio of styrene to divinylbenzene is (40-60):1; Preferably, the amount of the initiator is 1-5% of the mass of styrene.

4. The preparation method according to claim 3, characterized in that: The preparation method of the porous polystyrene microspheres comprises: The styrene monomer, the second pore-forming agent, the dispersant, the initiator and the solvent are mixed, reacted, and the second pore-forming agent is removed to obtain the porous polystyrene microspheres; Preferably, the mixing comprises: pre-mixing and dispersing the solvent and the second pore-forming agent, and then adding the styrene monomer, the dispersant and the initiator thereto and mixing them; Preferably, the premixing and dispersing temperature is 80-85°C and the rotation speed is 200-300rpm; Preferably, the reaction is carried out in the presence of a protective atmosphere, the reaction temperature is 80-90° C., and the reaction time is 8-10 h; Preferably, the method of removing the second pore forming agent comprises extraction.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The D50 particle size of the porous polystyrene microspheres is 0.8-1.2 μm; Preferably, the porosity of the porous polystyrene microspheres is 45-75%; Preferably, the pore size of the porous polystyrene microspheres is 9-20 nm; Preferably, the specific surface area of ​​the porous polystyrene microspheres is 85-170 m 2 / g.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The mixing and dispersing in step (1) is carried out at a speed of 1500-2000 rpm for 2-4 hours; Preferably, step (2) further comprises a step of degassing the dispersion before molding; Preferably, the molding method in step (2) includes casting molding; Preferably, the molding temperature in step (2) is 45-55°C; Preferably, the first organic solvent comprises an alcohol solvent; Preferably, the alcohol solvent includes at least one of methanol, ethanol, 1-propanol, isopropanol, 2,2,2-trifluoroethanol, 2-butanol, and isobutanol; Preferably, the mass concentration of the first organic solvent is ≥98%; Preferably, the method of treating with the first organic solvent comprises: soaking cellulose and / or the first membrane material in the first organic solvent, and drying to obtain a treated material; Preferably, the immersion time in the first organic solvent is 12-20 hours; Preferably, the drying temperature after the first organic solvent treatment is 60-75° C. and the drying time is 1-3 h; Preferably, the second organic solvent in step (3) comprises at least one of toluene, tetrahydrofuran, acetone, butanone, ethyl acetate, N,N-dimethylformamide, chloroform, benzene or xylene; Preferably, the mixing method in step (3) comprises: immersing the first film material in the second organic solvent; Preferably, the immersion time in the second organic solvent is 5-7 hours, and the temperature is room temperature; Preferably, step (3) further includes a drying step after the mixing.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: (1) mixing and dispersing cellulose and a first pore-forming agent at 1500-2000 rpm for 2-4 hours to obtain a dispersion; based on solid mass, the mass ratio of the cellulose to the first pore-forming agent is 1:(0.5-1.6); (2) casting the dispersion obtained in step (1) at 45-55° C. to obtain a first film material; soaking the first film material in a first organic solvent for 12-20 hours, and drying at 60-75° C. for 1-3 hours to obtain a treated first film material; (3) Soaking the treated first membrane material obtained in step (2) in a second organic solvent at room temperature for 5-7 hours and drying to obtain the cellulose membrane.

8. A cellulose film, characterized in that The cellulose film is prepared by the preparation method according to any one of claims 1 to 7; Preferably, the porosity of the cellulose membrane is 40-50%.

9. A diaphragm, characterized in that: The separator comprises a cellulose film prepared by the preparation method according to any one of claims 1 to 7 or a cellulose film according to claim 8.

10. A lithium ion battery, characterized in that: The lithium-ion battery comprises a cellulose film prepared by the preparation method according to any one of claims 1 to 7 or a separator according to claim 9.

Citation Information

Patent Citations

  • Blocking support frame and preparation method thereof

    CN108543117A

  • Nano cellulose diaphragm as well as preparation method and application thereof

    CN117080677A

  • Composite modified cellulose nylon diaphragm as well as preparation method and application thereof

    CN117096547A