Coating slurry, diaphragm and lithium ion battery thereof

By using coating slurry of bio-based particles, inorganic ceramic particles and metal organic framework particles on the lithium battery separator, the problems of insufficient high temperature resistance and electrolyte emollience of the lithium battery separator are solved, and higher high temperature resistance is achieved and electrolyte infiltration rate extend the service life and safety of lithium-ion batteries.

CN118970374AInactive Publication Date: 2024-11-15ANHUI LIKE NEW MATERIAL TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411015724.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing lithium battery separators have insufficient high temperature resistance and electrolyte wetting properties, which cannot meet the performance requirements of lithium battery.

Method used

Using a coating slurry, including bio-based particles, inorganic ceramic particles and metal organic framework particles, the coating is formed by mixing and stirring it with water to improve the high temperature resistance of the membrane and the electrolyte infiltration rate, and through the metal organic framework The particles provide open metal sites to alleviate the decomposition of the electrolyte and enhance the electrode reaction kinetics.

Benefits of technology

It significantly improves the high temperature resistance of the diaphragm and the infiltration rate of the electrolyte, improves the liquid retention volume, and extends the service life and safety of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970374A_ABST
    Figure CN118970374A_ABST
Patent Text Reader

Abstract

The invention discloses coating slurry, a diaphragm and a lithium ion battery thereof. The coating slurry comprises the following components in parts by mass: 1.0-3.0 parts of bio-based particles; 18-35 parts by mass of inorganic ceramic particles; 1-8 parts by mass of metal organic framework particles; and 50-70 parts by mass of water. The preparation method of the metal organic framework particles comprises the following steps: dissolving metal ions and a carboxyl-containing compound in a solvent for reaction to form a mixed solution, and then filtering, washing and drying to obtain the metal organic framework particles. When the coating slurry is applied to a diaphragm, the high temperature resistance of a diaphragm product can be improved, the infiltration rate of electrolyte is increased, and the liquid retention amount is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and in particular to a coating slurry, a diaphragm and a lithium ion battery thereof. Background Art

[0002] With the gradual consumption of global energy, available non-renewable energy will become less and less, and the use of non-renewable energy will bring challenges to the environment, such as global warming, haze, etc. Therefore, many countries are vigorously developing sustainable energy.

[0003] Lithium batteries have attracted much attention in sustainable energy due to their advantages such as sustainable use, environmental friendliness, safety and convenience. Lithium batteries are generally composed of positive electrodes, negative electrodes, separators and electrolytes, among which the separator plays a vital role in lithium batteries. The separator mainly separates the positive and negative electrodes to prevent short circuits, while allowing ions to pass through, so that the battery can complete the charging and discharging process.

[0004] At present, most commercial diaphragms are polyolefin diaphragms, and common polyolefin diaphragm materials include polyethylene (PE) and polypropylene (PP). In order to further improve the performance of the diaphragm, polyolefin or polypropylene diaphragms are usually used as base films for slurry coating, that is, the slurry is coated on the base film to form a coated diaphragm. Inorganic ceramic particles are usually used in the slurry, and there is also a solution of mixing aramid and ceramic particles. However, the diaphragm formed by this slurry coating has very limited improvement in wettability and high temperature resistance, and cannot meet the current requirements for lithium battery performance.

[0005] Therefore, the performance of existing separators needs to be improved. Summary of the invention

[0006] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, one object of the present invention is to provide a coating slurry, a diaphragm and a lithium-ion battery thereof, wherein the coating slurry is applied to the diaphragm to improve the high temperature resistance of the diaphragm product, increase the infiltration rate of the electrolyte, and increase the liquid retention.

[0007] In one aspect of the present invention, the present invention provides a coating slurry. According to an embodiment of the present invention, the coating slurry comprises:

[0008] 1.0 to 3.0 parts by mass of bio-based particles;

[0009] 18 to 35 parts by mass of inorganic ceramic particles;

[0010] 1 to 8 parts by weight of metal organic framework particles;

[0011] 50 to 70 parts by weight of water.

[0012] The preparation method of the metal organic framework particles comprises: dissolving metal ions and carboxyl-containing compounds in a solvent to react to form a mixed solution, and then filtering, washing and drying to obtain the mixed solution.

[0013] According to the coating slurry of the embodiment of the present invention, the coating slurry is obtained by mixing bio-based particles, inorganic ceramic particles and metal organic framework particles with water and stirring. The bio-based particle material reinforces the interior of the subsequent diaphragm coating without increasing the coating thickness, thereby improving the high temperature resistance of the diaphragm product; the addition of metal organic framework particles can provide open metal sites to spontaneously adsorb anions, while alleviating the decomposition of the electrolyte, enhancing the electrode reaction kinetics, and reducing the interface resistance between the electrolyte and the electrode. In addition, the metal organic framework particle material has a low density and is porous, which can further significantly increase the electrolyte infiltration rate and improve the liquid retention capacity.

[0014] In addition, the coating slurry according to the above embodiment of the present invention may also have the following additional technical features:

[0015] In some embodiments of the present invention, the metal ions are one or more of copper, iron, zinc, aluminum, cobalt, iron, nickel and magnesium.

[0016] In some embodiments of the present invention, the carboxyl-containing compound is one or more of terephthalic acid, trimesic acid, 2-hydroxyterephthalic acid and 2-aminoterephthalic acid.

[0017] In some embodiments of the present invention, the solvent includes one or more of N-methylpyrrolidone, 1,5-dimethyl-2-pyrrolidone, dimethyl sulfoxide and N,N-dimethylformamide.

[0018] In some embodiments of the present invention, the mass ratio of the metal ion to the carboxyl-containing compound is 1:(0.5-3.5), and the ratio of the carboxyl-containing compound to the solvent is (1-20) mg:1 mL.

[0019] In some embodiments of the present invention, the reaction temperature is 90-220° C., and the reaction time is 10-100 h.

[0020] In some embodiments of the present invention, the bio-based particles are one or more of furan-based polyamide, furan-based polyimide and furan polyester, with a particle size of 0.01 to 0.1 μm and a thermal decomposition temperature of >400°C.

[0021] In some embodiments of the present invention, the inorganic ceramic particles are one or more of alumina, boehmite, silicon dioxide, magnesium oxide, lithium aluminum titanium phosphate, lithium lanthanum zirconium oxide, and lithium lanthanum titanium oxide, with a particle size of 0.1 to 1 μm and a specific surface area of ​​4 to 10 m 2 / g.

[0022] In some embodiments of the present invention, the coating slurry further comprises: 0.1 to 0.5 parts by mass of a dispersant; 5 to 10 parts by mass of a binder; and 0.1 to 0.5 parts by mass of a wetting agent. Thus, the performance of the coating slurry can be further enhanced, which is beneficial to the improvement of the performance of the diaphragm.

[0023] In some embodiments of the present invention, the dispersant is one or more of polyester ammonium salts, quaternary ammonium salts, polyurethanes, polyesters and silanols.

[0024] In some embodiments of the present invention, the binder is one or more of polyimides, polyamides, polyacrylates and polyacrylic acids, and has a glass transition temperature of >180°C.

[0025] In some embodiments of the present invention, the wetting agent is one or more of polyethers, fatty alcohols and fatty acid esters.

[0026] In the second aspect of the present invention, the present invention provides a diaphragm. According to an embodiment of the present invention, the diaphragm includes: a base film; a coating, the coating is provided on the base film, and the coating is formed by coating the coating slurry on at least one side of the base film. As a result, the high temperature resistance and wettability of the diaphragm to the electrolyte are improved.

[0027] In some embodiments of the present invention, the coating process is gravure roller coating or extrusion, and the thickness of the coating is ≤3 μm.

[0028] In the third aspect of the present invention, the present invention provides a lithium-ion battery. According to an embodiment of the present invention, the lithium-ion battery comprises: a positive electrode; a negative electrode; and a battery separator, wherein the battery separator adopts the above-mentioned separator. Thus, the safety and service life of the lithium-ion battery are improved.

[0029] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0031] Figure 1 is a SEM image of the diaphragm prepared in Example 2 of the present invention at a scale of 100 μm;

[0032] Figure 2 This is a SEM image of the diaphragm prepared in Example 2 of the present invention at a scale of 1 μm;

[0033] Figure 3It is a thermal shrinkage state diagram of the diaphragms prepared in Example 2, Comparative Example 1 and Comparative Example 2 of the present invention after being baked at 120° C., 130° C., 150° C. and 160° C. for 1 hour. DETAILED DESCRIPTION

[0034] The embodiments of the present invention are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain the present invention, and cannot be interpreted as limiting the present invention. In addition, if not explicitly stated, all reagents used in the following embodiments are commercially available, or can be synthesized according to this article or known methods, and the reaction conditions not listed are also easily available to those skilled in the art.

[0035] Example 1

[0036] 1.1 g of furan-based polyamide particles with a particle size of 0.05 μm and 19 g of particles with a particle size of 0.5 μm and a specific surface area of ​​6 m 2 / g boehmite, 1.5g Cu@MOF particles and 51g water were mixed and stirred evenly to obtain a diaphragm coating slurry. The diaphragm coating slurry was then coated on one side of a 9μm PE base film using a gravure roller coating process, and the coating thickness was 3μm, and finally a lithium battery diaphragm was obtained.

[0037] Preparation process of Cu@MOF: 1g of copper nitrate and 0.6g of terephthalic acid were dissolved in 100mL of N,N-dimethylformamide, and the reaction was carried out for 90h at a reaction temperature of 200°C to obtain a mixed solution. The mixed solution was then filtered, washed with ethanol, and vacuum dried for 10h to finally obtain solid Cu@MOF particles, which were ground and set aside for use.

[0038] Example 2

[0039] 1.5 g of furan-based polyamide particles with a particle size of 0.09 μm, 0.15 g of polyester ammonium salt and 60 g of deionized water were mixed, and the high-speed disperser had a rotation speed of 1000 rpm and a revolution speed of 25 rpm, and stirred for 30 minutes to form a primary mixture. Then 25 g of 0.1 μm particle size and a specific surface area of ​​7 m 2 / g of alumina ceramic particles, and 5g of Ni@MOF particles with a particle size of 0.6μm. Set the high-speed disperser's self-rotation speed to 2000rpm, the revolution speed to 30rpm, and high-speed stirring for 60min to obtain a ceramic dispersion. Then use a sand mill to fully mix the slurry, the sand mill speed is 650rpm, and after sanding 3 times, a first slurry is formed; then 0.3g of polyether wetting agent and 8g of polyacrylic acid binder are added to the first slurry, and the high-speed dispersant's self-rotation speed is set to 400rpm, the revolution speed is 25rpm, and stirring is carried out for 30min to obtain a diaphragm coating slurry, and then the diaphragm coating slurry is coated on one side of the 9μm PE base film using a gravure roller coating process. The coating thickness is 4μm, and finally a lithium battery diaphragm is obtained. The SEM image of the diaphragm under a 100μm scale is shown in Figure 1 , SEM image of the diaphragm at 1 μm scale is shown in Figure 2 .

[0040] Preparation process of Ni@MOF: 1g of aluminum nitrate and 3g of trimesic acid were dissolved in 200mL of N,N-dimethylformamide, and the reaction temperature was 100°C for 15h to obtain a mixed solution, which was then filtered and washed with ethanol and then vacuum dried for 10h to finally obtain solid Ni@MOF particles, which were ground and set aside for use.

[0041] Example 3

[0042] 2.9 g of furan-based polyimide particles with a particle size of 0.02 μm and 34 g of particles with a particle size of 0.1 μm and a specific surface area of ​​5 m 2 / g of alumina ceramic particles, 7.8g of Cu@MOF, 0.5g of polyurethane dispersant, 9.8g of polyamide binder, 0.5g of fatty alcohol wetting agent and 69g of water were mixed. The preparation process of Cu@MOF was the same as that in Example 1. After uniform mixing, a diaphragm coating slurry was obtained, and then the diaphragm coating slurry was coated on one side of a 9μm PE base film by gravure roller coating. The coating thickness was 4μm, and finally a lithium battery diaphragm was obtained.

[0043] Example 4

[0044] 2.9 g of furan-based polyimide particles with a particle size of 0.02 μm and 30 g of particles with a particle size of 0.9 μm and a specific surface area of ​​9 m 2 / g of alumina ceramic particles, 7g of Ni@MOF, 0.5g of silanol dispersant, 9g of polyacrylate binder, 0.5g of fatty alcohol wetting agent and 60g of water were mixed. The preparation process of Ni@MOF was the same as that in Example 2. After uniform mixing, a diaphragm coating slurry was obtained, and then the diaphragm coating slurry was coated on one side of a 9μm PE base film by gravure roller coating. The coating thickness was 4μm, and finally a lithium battery diaphragm was obtained.

[0045] Comparative Example 1

[0046] 9μm thick PE base film.

[0047] Comparative Example 2

[0048] Without adding furan-based polyamide particles and metal organic framework particles, the remaining process was the same as in Example 2, and finally a lithium battery separator was prepared.

[0049] Comparative Example 3

[0050] Without adding metal organic framework particles, the rest of the process was the same as in Example 2, and finally a lithium battery separator was prepared.

[0051] Comparative Example 4

[0052] Without adding furan-based polyamide particles, the remaining process was the same as in Example 2, and finally a lithium battery separator was prepared.

[0053] The diaphragms prepared in Examples 1-4 and Comparative Examples 1-4 were subjected to a heat shrinkage test and a wettability test. The heat shrinkage test results are shown in Table 1, and the wettability test results are shown in Table 2.

[0054] Table 1 Thermal shrinkage of the diaphragms obtained in Examples 1-4 and Comparative Examples 1-4

[0055]

[0056] From the data in Table 1, it can be seen that after the diaphragms prepared in Examples 1-4 were baked at 120°C, 130°C, 150°C, and 160°C for 1 hour, the MD / TD thermal shrinkage rates were relatively low, and there was an obvious advantage in thermal shrinkage at high temperatures of 120-160°C. Figure 3 The diaphragm prepared in Example 2 still exhibits a good morphology at 160°C, while the diaphragms prepared in Comparative Examples 1 and 2 have already experienced obvious thermal shrinkage at 150°C and 160°C.

[0057] Table 2 Wetting of the diaphragms obtained in Examples 1-4 and Comparative Examples 1-4 by the electrolyte

[0058]

[0059] From the data in Table 2, it can be seen that the membranes prepared in Examples 1-4 have large liquid absorption rate, liquid retention rate and wetted area, indicating that the wettability of the membranes prepared in this technical solution is significantly better.

[0060] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0061] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A coating slurry, characterized in that: include: 1 to 3 parts by weight of bio-based particles; 18 to 35 parts by mass of inorganic ceramic particles; 1 to 8 parts by weight of metal organic framework particles; 50-70 parts by weight of water; The method for preparing the metal organic framework particles comprises: dissolving metal ions and carboxyl-containing compounds in a solvent to react to form a mixed solution, and then filtering, washing and drying the solution to obtain the mixed solution.

2. The coating slurry according to claim 1, characterized in that: The metal ions are one or more of copper, iron, zinc, aluminum, cobalt, iron, nickel and magnesium; The carboxyl-containing compound is one or more of terephthalic acid, trimesic acid, 2-hydroxyterephthalic acid and 2-aminoterephthalic acid; The solvent includes one or more of N-methylpyrrolidone, 1,5-dimethyl-2-pyrrolidone, dimethyl sulfoxide and N,N-dimethylformamide.

3. The coating slurry according to claim 1 or 2, characterized in that: The mass ratio of the metal ion to the carboxyl-containing compound is 1:(0.5-3.5), and the ratio of the carboxyl-containing compound to the solvent is (1-20) mg:1 mL; The reaction temperature is 90-220° C., and the reaction time is 10-100 hours.

4. The coating slurry according to claim 1, characterized in that: The bio-based particles are one or more of furan-based polyamide, furan-based polyimide and furan polyester, with a particle size of 0.01 to 0.1 μm and a thermal decomposition temperature of more than 400° C.

5. The coating slurry according to claim 1, characterized in that: The inorganic ceramic particles are one or more of alumina, boehmite, silicon dioxide, magnesium oxide, lithium aluminum titanium phosphate, lithium lanthanum zirconium oxide, and lithium lanthanum titanium oxide, with a particle size of 0.1 to 1 μm and a specific surface area of ​​4 to 10 m 2 / g.

6. The coating slurry according to claim 1, characterized in that: Also includes: 0.1 to 0.5 parts by mass of a dispersant; 5 to 10 parts by weight of a binder; 0.1 to 0.5 parts by mass of a wetting agent.

7. The coating slurry according to claim 6, characterized in that: The dispersant is one or more of polyester ammonium salts, quaternary ammonium salts, polyurethanes, polyesters and silanols; The binder is one or more of polyimide, polyamide, polyacrylate and polyacrylic acid, and has a glass transition temperature of >180°C; The wetting agent is one or more of polyethers, fatty alcohols and fatty acid esters.

8. A diaphragm, characterized in that: include: Basement membrane; A coating layer is provided on the base film and is formed by coating the coating slurry according to any one of claims 1 to 7 on at least one side of the base film.

9. The diaphragm according to claim 8, characterized in that The coating process is gravure roller coating or extrusion coating, and the thickness of the coating is ≤3 μm.

10. A lithium ion battery, characterized in that: include: positive electrode; negative electrode; A battery separator, wherein the battery separator adopts the separator according to claim 8 or 9.

Citation Information

Patent Citations

  • Metal-organic framework composite diaphragm, battery comprising same and manufacturing method of metal-organic framework composite diaphragm

    CN115810867A

  • Preparation and application of water-based coating slurry for improving diaphragm rupture temperature

    CN116387751A

  • Lithium battery slurry coated diaphragm and preparation method and coating slurry thereof

    CN116487820A

  • Preparation method for coating bio-based furan polyamide film on lithium ion battery diaphragm

    CN117438738A

  • Isolating membrane for lithium battery and manufacturing method thereof

    CN117954780A

Cited By

  • Lithium ion battery diaphragm based on composite coating as well as preparation method and application of lithium ion battery diaphragm

    CN120511435A