VCSEL (Vertical Cavity Surface Emitting Laser) device with electron deceleration effect and preparation method thereof

By inserting low-doped Alx5Iny5Ga1-x5-y5N material into the N-type semiconductor layer of GaN-based VCSEL device, an electron potential well is formed, which solves the electron leakage problem and improves the energy utilization rate and photoelectric conversion efficiency of VCSEL devices.

CN118970628APending Publication Date: 2024-11-15Shandong Huaguang Optoelectronics Co. Ltd.
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410868747.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

GaN-based VCSEL devices have low energy utilization and photoelectric conversion efficiency due to low hole and electron recombination efficiency, and electrons are easily leaked from quantum wells, which seriously restricts the performance of the laser.

Method used

A layer of low-doped Alx5Iny5Ga1-x5-y5N material containing In components is inserted into the standard N-type semiconductor layer Alx4Iny4Ga1-x4-y4N, and potential well deceleration electrons are used.

Benefits of technology

Through the inserted electron reduction layer, the mobility of electrons is reduced, and the possibility that electrons are trapped by quantum wells is increased, thereby improving the performance and output power of the laser.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970628A_ABST
    Figure CN118970628A_ABST
Patent Text Reader

Abstract

The invention relates to a VCSEL device with an electron deceleration effect and a preparation method thereof, and belongs to the technical field of semiconductor lasers. The semiconductor device sequentially comprises a substrate, a buffer layer, a bottom nitride DBR, an electron deceleration layer, a multi-quantum well layer, a P-EBL, a P-type semiconductor material layer, a current limiting layer and a current expansion layer in the epitaxial growth direction. The electron deceleration layer is formed by overlapping three layers of materials, the middle layer is made of N-type semiconductor materials with small forbidden bandwidth, the two sides are made of N-type semiconductor materials with large forbidden bandwidth, and the material parameters of the two sides are the same. According to the electron deceleration layer, a layer of In component-containing material is inserted into an N-type semiconductor material, and a potential well formed by the two layers of materials has a certain deceleration effect on electrons, so that the probability that the electrons escape from a quantum well is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a VCSEL device with electron deceleration function and a preparation method thereof, belonging to the technical field of semiconductor lasers. Background Art

[0002] Laser is a far-reaching invention in the history of human science after computers and semiconductors in the last century. Laser has the advantages of high brightness, directional light emission, and high color purity. Maiman created the world's first ruby ​​laser in 1960. After years of development, laser technology has been combined with multiple disciplines to promote the development of multiple fields and is widely used in industry and life. According to the classification of luminescent materials, lasers can be divided into: solid lasers, gas lasers, liquid lasers and semiconductor lasers. VCSEL is a kind of semiconductor laser with the advantages of low threshold current, low power consumption, circular beam, easy coupling with optical fiber, and on-wafer testing. Therefore, it has a bright future in various applications such as display lighting, biosensors, high-density optical storage, visible light communication, and military detection. The ionic bond energy of GaN material is large, so its material properties are stable, which can greatly improve the reliability of device operation. In addition, by adjusting the band gap of nitride materials, the luminescence range of GaN-based light-emitting devices can cover the ultraviolet, blue, green and red light spectra, making it an important light-emitting material.

[0003] Today, a major problem facing the development of GaN-based VCSEL technology is that the low efficiency of hole-electron recombination results in low energy utilization and photoelectric conversion efficiency of laser devices. Related studies have shown that compared with holes, electrons have a smaller effective mass and a higher mobility, which makes it easy for electrons to leak from quantum wells. Secondly, the P-type semiconductor material required for the device is formed by Mg impurity doping, and its activation energy is higher than that of N-type Si doped impurities, so the efficiency of P-type doping is also relatively low, which in turn exacerbates the problem of low hole concentration. The lower hole injection efficiency will reduce the probability of electron and hole recombination, aggravate the problem of electron leakage, and seriously restrict the performance of the laser. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention provides a VCSEL device with electron deceleration effect and a preparation method thereof. x4 In y4 Ga 1-x4-y4 A layer of low-doped Al containing In components is inserted between N x5 In y5 Ga 1-x5-y5 N material, using Al x4 In y4 Ga 1-x4-y4 N and Al x5In y5 Ga 1-x5-y5 The potential well formed by N decelerates the electrons.

[0005] The technical solution of the present invention is as follows:

[0006] A VCSEL device with electron deceleration effect, which includes a substrate, a buffer layer, a bottom nitride DBR, an electron deceleration layer, a multi-quantum well layer, a P-EBL layer, a P-type semiconductor material layer, a current limiting layer, and a current expansion layer in sequence along the epitaxial growth direction, a top dielectric DBR layer and a P-type ohmic electrode are arranged above the current expansion layer, and an N-type ohmic electrode is arranged above the electron deceleration layer;

[0007] The electron deceleration layer is composed of three overlapping layers of materials. The material in the middle layer contains In components, while the upper and lower layers do not contain In components. The energy band width of the middle material is smaller than that of the upper and lower layers on both sides, and the material parameters of the upper and lower layers on both sides are the same.

[0008] Preferably, the electron deceleration layer comprises Al x4 In y4 Ga 1-x4-y4 N layer, Al x5 In y5 Ga 1-x5-y5 N layer, Al x4 In y4 Ga 1-x4-y4 N layers, where 0≤x4≤1, y4=0, 0≤1-x4-y4≤1, 0≤x5≤1, 0<y5≤1, 0≤1-x5-y5≤1, and the doping concentration is 1e13cm -3 ~1e26cm -3 ; y5>y4, control the size of In component to control the band width, the values ​​of x4 and x5 can be the same, just control y5 greater than y4; Al x5 In y5 Ga 1-x5-y5 The energy band width of the N layer is smaller than that of the Al x4 In y4 Ga 1-x4-y4 N layer, Al x5 In y5 Ga 1-x5-y5 The thickness of the N layer is controlled to be between 1 nm and 30 nm.

[0009] Further preferably, the inserted intermediate layer is low-doped and is located in the middle of the electron deceleration layer.

[0010] Preferably, the VCSEL device with electron deceleration effect includes one of the following solutions:

[0011] Ⅰ. The material of the substrate is sapphire, Si or SiC, and the substrate is divided into a polar substrate, a semi-polar substrate or a non-polar substrate according to the epitaxial growth direction;

[0012] II. The material of the buffer layer is Al x1 In y1 Ga 1-x1-y1 N; wherein 0≤x1≤1, 0≤y1≤1, 0≤1-x1-y1≤1, thickness is 10nm to 50nm, preferably 20nm;

[0013] III. The current spreading layer covers the current limiting layer, and the material selection includes ITO, Ni / Au, zinc oxide or graphene, and the thickness is 10 to 500 nm;

[0014] IV. The material of the top dielectric DBR layer is made of alternating high and low refractive index materials, with an alternating period of 10 to 30, and its thickness is one-fourth of the wavelength of the desired luminous wavelength in the medium, and the thickness is 500nm to 3000nm; preferably, it is preferably alternating for 15 periods;

[0015] V. The material of the P-type ohmic electrode is selected from Ni / Au, Cr / Au, Pt / Au or Ni / Al;

[0016] VI. The material of the N-type ohmic electrode is selected to be Al / Au, Cr / Au or Ti / Al / Ti / Au.

[0017] Preferably, the material of the bottom nitride DBR is Al x2 In y2 Ga 1-x2-y2 N / A x3 In y3 Ga 1-x3-y3 It is formed by alternating, and the alternating period ranges from 30 to 50, preferably 40 alternating periods, and the coefficients of each component are preferably 0≤x2≤1, 0≤y2≤1, 0≤1-x2-y2≤1, 0≤x3≤1, 0≤y3≤1, 0≤1-x3-y3≤1, and their thicknesses are one-fourth of the wavelength of the required luminous wavelength in the medium, and the thickness ranges from 500nm to 3000nm.

[0018] Preferably, the material of the multi-quantum well layer is Al x6 In y6 Ga 1-x6-y6 N / A x7 In y7 Ga 1-x7-y7N, preferably 5 periods, wherein 0≤x6≤1, 0≤y6≤1, 0≤1-x6-y6≤1, 0≤x7≤1, 0≤y7≤1, 0≤1-x7-y7≤1, x6≠x7, y6≠y7, the bandgap of the quantum barrier is higher than the bandgap of the quantum well, and the number of quantum wells is greater than or equal to 1; quantum well Al x6 In y6 Ga 1-x6-y6 N thickness is 1nm~10nm, non-doped; quantum barrier Al x7 In y7 Ga 1-x7-y7 N thickness is 4nm to 50nm, non-doped or P-type doped or N-type doped.

[0019] Furthermore, the material of the P-EBL layer is Al x8 In y8 Ga 1-x8-y8 N, wherein x8, y8 and 1-x8-y8 are all between 0 and 1, P-type doping, thickness is 10 to 50 nm, preferably 20 nm.

[0020] Furthermore, the material of the P-type semiconductor material layer is Al x9 In y9 Ga 1-x9-y9 N, wherein x9, y9 and 1-x9-y9 are all between 0 and 1, the thickness is 50 to 500 nm, and 250 nm is preferred.

[0021] Preferably, the outer side of the upper surface of the P-type semiconductor material layer is an annular insulating layer, which serves as a current limiting layer. Its material is undoped HfO2 or Ta2O5, with a thickness of 5 to 100 nm, preferably 15 nm, and a width of the ring of 0.2 to 10 μm, preferably 1 μm.

[0022] A method for preparing the above-mentioned VCSEL device with an electron deceleration layer comprises the following steps:

[0023] (1) First, in an MOCVD reactor, the substrate is baked at 1250-1350° C. to remove foreign matter on the substrate surface, and then a buffer layer, a bottom nitride DBR, an electron deceleration layer, a multi-quantum well layer, a P-EBL, and a P-type semiconductor material layer are grown respectively;

[0024] (2) Making steps by photolithography and etching processes, exposing 40% to 70% of the electron deceleration layer, and evaporating and photolithography to make an N-type ohmic electrode;

[0025] (3) photolithography a current confinement layer pattern on the P-type semiconductor material layer obtained in step (2), and depositing and growing a current confinement layer structure layer;

[0026] (4) evaporating a current spreading layer on the current limiting layer obtained in step (3), wherein the material of the current spreading layer is ITO, and patterning the current spreading layer by photolithography and wet etching, the patterned current spreading layer being located above the P-type semiconductor material layer and the current limiting layer;

[0027] (5) Atomic layer deposition of a top dielectric DBR layer is performed on the current spreading layer, and a P-type ohmic electrode is produced by evaporation and photolithography.

[0028] For any details not provided in the present invention, please refer to the prior art.

[0029] The present application inserts an N-InGaN layer between the N-type semiconductor material and the quantum well, uses the electron potential well formed between the N-type InGaN\N-type semiconductor material layers to decelerate the electrons, and at the same time reduces the doping concentration of the N-InGaN insertion layer, and uses the interface potential barrier formed at the doping interface to decelerate the electrons.

[0030] The beneficial effects of the present invention are:

[0031] The electron deceleration layer of the present invention is Al x4 In y4 Ga 1-x4-y4 N(L1) / Al x5 In y5 Ga 1-x5-y5 N(L2) / Al x4 In y4 Ga 1-x4-y4 N(L3), where the composition of each element x4, y4, x5, y5, 1-x4-y4 and 1-x8-y8 are between 0 and 1, and the doping concentration is 1e20cm -3 ~1e26cm -3 , and control the values ​​of x4, y4, x5, y5, 1-x4-y4 and 1-x5-y5 to make Al x5 In y5 Ga 1-x5-y5 The energy band width of the N(L2) layer is smaller than that of the Al x4 In y4 Ga 1-x4-y4 N(L1) and Al x4 In y4 Ga 1-x4-y4 N(L3) layer.

[0032] The structure of the present invention inserts a semiconductor material layer Al with a smaller energy band width into the N-type semiconductor material of the standard GaN-based VCSEL. x5 In y5 Ga 1-x5-y5N, an electron potential well is formed in the N-type semiconductor material of the VCSEL device. The formed electron potential well will reduce the mobility of electrons when they pass through, thereby increasing the possibility of being captured by the quantum well. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The drawings in the specification, which constitute a part of the present application, are used to provide further understanding of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute improper limitations on the present application.

[0034] Figure 1 Schematic diagram of the epitaxial structure of a VCSEL device without an electron deceleration layer;

[0035] Figure 2 A schematic diagram of the epitaxial structure of a VCSEL device with an electron deceleration layer according to the present invention;

[0036] Figure 3 for Figure 2 The schematic diagram of the epitaxial structure after the ICP etching is used to expose a part of the electron deceleration layer and the N-type ohmic electrode is evaporated;

[0037] Figure 4 For Figure 3 Schematic diagram of the product obtained after etching the current limiting layer pattern on the obtained P-type material layer and growing the current limiting layer and the ITO layer;

[0038] Figure 5 For Figure 4 Schematic diagram of a product obtained by evaporating a P-type ohmic electrode on the obtained product;

[0039] Figure 6 For Figure 5 Schematic diagram of the product obtained by growing a top dielectric DBR on the obtained product;

[0040] Figure 7 A power comparison diagram of the VCSEL device of the present invention and the existing standard VCSEL device;

[0041] Figure 8 A comparison diagram of electron concentration at the quantum well of the VCSEL device of the present invention and the existing standard VCSEL device;

[0042] Wherein: 101. substrate; 102. buffer layer; 103. bottom nitride DBR; 104. electron deceleration layer; 105. multi-quantum well layer; 106. P-EBL layer; 107. P-type semiconductor material layer; 108. current confinement layer; 109. current expansion layer; 110. top dielectric DBR layer; 111. P-type ohmic electrode; 112. N-type ohmic electrode; 113. Al x5 In y5 Ga 1-x5y5 N layers. DETAILED DESCRIPTION

[0043] The present invention will be further described below by way of embodiments in conjunction with the accompanying drawings, but is not limited thereto.

[0044] Embodiment 1:

[0045] A VCSEL device with electron deceleration effect, such as Figure 2-Figure 6 As shown, along the epitaxial growth direction, the substrate 101, the buffer layer 102, the bottom nitride DBR 103, the electron deceleration layer 104, the multi-quantum well layer 105, the P-EBL layer 106, the P-type semiconductor material layer 107, the current limiting layer 108, and the current expansion layer 109 are sequentially included; a top dielectric DBR layer 110 and a P-type ohmic electrode 111 are arranged above the current expansion layer 109; and an N-type ohmic electrode 112 is arranged above the electron deceleration layer 104.

[0046] The electron deceleration layer is formed by overlapping three layers of materials, wherein the material in the middle is an In-containing material, and the materials on both sides are In-free materials, and the material parameters of the two sides are the same.

[0047] The electron deceleration layer includes Al x4 In y4 Ga 1-x4-y4 N layer 106 (L1), Al x5 In y5 Ga 1-x5-y5 N layer 113 (L2), Al x4 In y4 Ga 1-x4-y4 N layer 106 (L3), where 0≤x4≤1, y4=0, 0≤1-x4-y4≤1, 0≤x5≤1, 0<y5≤1, 0≤1-x5-y5≤1, and doping concentration is 1e20cm -3 ~1e26cm -3 , control the size of In component to control the band width, control y5 to be greater than y4, Al x4 In y4 Ga 1-x4-y4 The energy band width of the N layer is larger than that of the Al x5 In y5 Ga 1-x5-y5 N layer, Al x4 In y4 Ga 1-x4-y4 The thickness of the N layer is controlled at 20nm.

[0048] The inserted intermediate layer is low-doped and is located in the middle of the electron deceleration layer.

[0049] The material of the substrate is sapphire, and the material of the buffer layer is Al x1 Iny1 Ga 1-x1-y1 N; wherein 0≤x1≤1, 0≤y1≤1, 0≤1-x1-y1≤1, and the thickness is 20nm; the material of the bottom nitride DBR is Al x2 In y2 Ga 1-x2-y2 N / A x3 In y3 Ga 1-x3-y3 It is formed by alternating for 40 cycles, and preferably, the coefficients of each component are 0≤x2≤1, 0≤y2≤1, 0≤1-x2-y2≤1, 0≤x3≤1, 0≤y3≤1, 0≤1-x3-y3≤1, and their thicknesses are one-fourth of the wavelength of the required luminous wavelength in the medium, and the thickness ranges from 500nm to 3000nm.

[0050] The multi-quantum well layer is made of 5-period Al x6 In y6 Ga 1-x6-y6 N / A x7 In y7 Ga 1-x7-y7 N, where 0≤x6≤1, 0≤y6≤1, 0≤1-x6-y6≤1, 0≤x7≤1, 0≤y7≤1, 0≤1-x7-y7≤1, x6≠x7, y6≠y7, the bandgap of the quantum barrier is higher than the bandgap of the quantum well, and the number of quantum wells is greater than or equal to 1; quantum well Al x6 In y6 Ga 1-x6-y6 N thickness is 3nm, non-doped; quantum barrier Al x7 In y7 Ga 1-x7-y7 N thickness is 4nm, undoped or P-type doped or N-type doped.

[0051] The material of P-EBL layer is Al x8 In y8 Ga 1-x8-y8 N, where x8, y8 and 1-x8-y8 are all between 0 and 1, P-type doping, and thickness is 20 nm.

[0052] The material of the P-type semiconductor material layer is Al x9 In y9 Ga 1-x9-y9 N, where x9, y9 and 1-x9-y9 are all between 0 and 1, and the thickness is 225 nm.

[0053] The outer side of the upper surface of the P-type semiconductor material layer is a ring-shaped insulating layer, which serves as a current limiting layer. The material of the insulating layer is non-doped HfO2, the thickness is 15nm, and the width of the ring is 1μm.

[0054] The current spreading layer covers the current limiting layer, and the material is ITO with a thickness of 20nm.

[0055] The material of the top dielectric DBR layer is made of alternating high and low refractive index materials, with an alternating period of 15. The thickness thereof is one quarter of the wavelength of the required light emitting wavelength in the medium, and the thickness is 500nm to 3000nm.

[0056] The material of the P-type ohmic electrode is Ni / Au; the material of the N-type ohmic electrode is Al / Au.

[0057] Example 2

[0058] A VCSEL device with electron deceleration effect, the structure of which is as described in Example 1, except that the substrate is SiC, the buffer layer thickness is 10nm, and the material of the bottom nitride DBR is Al x2 In y2 Ga 1-x2-y2 N / A x3 In y3 Ga 1-x3-y3 Alternating, the alternating period is 30, quantum well Al x6 In y6 Ga 1-x6-y6 N thickness is 1nm, quantum barrier Al x7 In y7 Ga 1-x7-y7 The thickness of N is 4nm. The thickness of P-EBL layer is 10nm. The thickness of P-type semiconductor material layer is 50nm. The current limiting layer is made of Ta2O5, with a thickness of 5nm and a ring width of 0.2μm. The current spreading layer is made of Ni / Au with a thickness of 10nm. The material of the top dielectric DBR layer is composed of alternating high and low refractive index materials with an alternating period of 10. The material of P-type ohmic electrode is Cr / Au; the material of N-type ohmic electrode is Ti / Al / Ti / Au.

[0059] Example 3

[0060] A VCSEL device with electron deceleration effect, the structure of which is as described in Example 1, except that the substrate is Si, the buffer layer thickness is 50nm, and the material of the bottom nitride DBR is Al x2 In y2 Ga 1-x2-y2 N / A x3 In y3 Ga 1-x3-y3 Alternating, the alternating period is 50, quantum well Al x6 In y6 Ga 1-x6-y6 N thickness is 10nm, quantum barrier Al x7 Iny7 Ga 1-x7-y7 N thickness is 50nm. P-EBL layer thickness is 50nm. P-type semiconductor material layer thickness is 500nm. Current limiting layer thickness is 100nm, and the width of the ring is 10μm. The current spreading layer material is zinc oxide, with a thickness of 500nm. The material of the top dielectric DBR layer is composed of alternating high and low refractive index materials, with an alternating period of 30. The material of the P-type ohmic electrode is Pt / Au; the material of the N-type ohmic electrode is Cr / Au.

[0061] Example 4

[0062] A VCSEL device with electron deceleration effect, the structure of which is as described in Example 1, except that the thickness of the current limiting layer is 40nm, the width of the ring is 2.5μm, the material of the current spreading layer is graphene, and the material of the P-type ohmic electrode is Ni / Al.

[0063] Example 5

[0064] A method for preparing a VCSEL device having an electron deceleration layer according to Example 1 comprises the following steps:

[0065] (1) First, in an MOCVD reactor, the substrate is baked at 1250-1350° C. to remove foreign matter on the substrate surface, and then a buffer layer, a bottom nitride DBR, an electron deceleration layer, a multi-quantum well layer, a P-EBL, and a P-type semiconductor material layer are grown respectively;

[0066] (2) Making steps by photolithography and etching processes, exposing 40% to 70% of the electron deceleration layer, and evaporating and photolithography to make an N-type ohmic electrode;

[0067] (3) photolithography a current confinement layer pattern on the P-type semiconductor material layer obtained in step (2), and depositing and growing a current confinement layer structure layer;

[0068] (4) evaporating a current spreading layer on the current limiting layer obtained in step (3), wherein the material of the current spreading layer is ITO, and patterning the current spreading layer by photolithography and wet etching, the patterned current spreading layer being located above the P-type semiconductor material layer and the current limiting layer;

[0069] (5) Atomic layer deposition of a top dielectric DBR layer is performed on the current spreading layer, and a P-type ohmic electrode is produced by evaporation and photolithography.

[0070] Comparative Example 1:

[0071] like Figure 1As shown in the figure, a standard VCSEL device epitaxial structure includes, along the epitaxial growth direction, a substrate, a buffer layer, a bottom nitride DBR, an N-type semiconductor material layer, a multi-quantum well layer, a P-type electron blocking layer, a P-type semiconductor material layer, a current limiting layer, a current spreading layer, a top dielectric DBR, a P-type ohmic electrode, and an N-type ohmic electrode.

[0072] Compared with the standard VCSEL device in comparative example 1, an insertion layer containing In components is added to the N-type semiconductor material layer of the present invention, and the electron potential well formed between the insertion layer and the adjacent material has a certain blocking effect on electrons, thereby reducing the probability of their escape from the quantum well.

[0073] Figure 7 The power comparison diagram of the VCSEL device of the present invention and the existing standard N-GaN electron injection layer VCSEL device, that is, the power comparison of Example 1 and Comparative Example 1, from Figure 7 It can be seen that the VCSEL device with an electron blocking layer of the present invention has a lower threshold and a higher output power at the same current. This is caused by the reduction of the mobility of electrons in the electron deceleration layer, which causes more electrons to be captured in the active region.

[0074] Figure 8 This is a comparison diagram of the electron concentration in the quantum well of the VCSEL device of the present invention and the existing standard N-GaN electron injection layer VCSEL device, that is, the comparison of the electron concentration in the quantum well of Example 1 and Comparative Example 1. It can be seen from the figure that the VCSEL device with the electron deceleration layer has a higher electron concentration in the quantum well.

[0075] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A VCSEL device with electron deceleration effect, characterized in that: The epitaxial growth direction includes a substrate, a buffer layer, a bottom nitride DBR, an electron deceleration layer, a multi-quantum well layer, a P-EBL layer, a P-type semiconductor material layer, a current limiting layer, and a current expansion layer. A top dielectric DBR layer and a P-type ohmic electrode are arranged above the current expansion layer, and an N-type ohmic electrode is arranged above the electron deceleration layer. The electron deceleration layer is composed of three overlapping layers of materials. The material in the middle layer contains In components, while the upper and lower layers do not contain In components. The energy band width of the middle material is smaller than that of the upper and lower layers on both sides, and the material parameters of the upper and lower layers on both sides are the same.

2. The VCSEL device with electron deceleration effect according to claim 1, characterized in that: The electron deceleration layer includes Al x4 In y4 Ga 1-x4-y4 N layer, Al x5 In y5 Ga 1-x5-y5 N layer, Al x4 In y4 Ga 1-x4-y4 N layers, where 0≤x4≤1, y4=0, 0≤1-x4-y4≤1, 0≤x5≤1, 0<y5≤1, 0≤1-x5-y5≤1, and the doping concentration is 1e13cm -3 ~1e26cm -3 ;Al x5 In y5 Ga 1-x5-y5 The energy band width of the N layer is smaller than that of the Al x4 In y4 Ga 1-x4-y4 N layer, Al x5 In y5 Ga 1-x5-y5 The thickness of the N layer is controlled to be between 1 nm and 30 nm.

3. The VCSEL device with electron deceleration effect according to claim 2, characterized in that: The inserted intermediate layer is low-doped and is located in the middle of the electron deceleration layer.

4. The VCSEL device with electron deceleration effect according to claim 1, characterized in that: The VCSEL device with electron deceleration effect includes one of the following solutions: Ⅰ. The material of the substrate is sapphire, Si or SiC, and the substrate is divided into a polar substrate, a semi-polar substrate or a non-polar substrate according to the epitaxial growth direction; II. The material of the buffer layer is Al x1 In y1 Ga 1-x1-y1 N; wherein 0≤x1≤1, 0≤y1≤1, 0≤1-x1-y1≤1, thickness is 10nm to 50nm, preferably 20nm; III. The current spreading layer covers the current limiting layer, and the material selection includes ITO, Ni / Au, zinc oxide or graphene, and the thickness is 10 to 500 nm; IV. The material of the top dielectric DBR layer is made of alternating high and low refractive index materials, with an alternating period of 10 to 30, and its thickness is one quarter of the wavelength of the desired luminous wavelength in the medium, and the thickness is 500nm to 3000nm; preferably, the alternating period is 15; V. The material of the P-type ohmic electrode is selected from Ni / Au, Cr / Au, Pt / Au or Ni / Al; VI. The material of the N-type ohmic electrode is selected to be Al / Au, Cr / Au or Ti / Al / Ti / Au.

5. The VCSEL device with electron deceleration effect according to claim 1, characterized in that: The material of the bottom nitride DBR is Al x2 In y2 Ga 1-x2-y2 N / A x3 In y3 Ga 1-x3-y3 It is formed by alternating, and the alternating period ranges from 30 to 50, preferably 40 alternating periods, and the coefficients of each component are preferably 0≤x2≤1, 0≤y2≤1, 0≤1-x2-y2≤1, 0≤x3≤1, 0≤y3≤1, 0≤1-x3-y3≤1, and their thicknesses are one-fourth of the wavelength of the required luminous wavelength in the medium, and the thickness ranges from 500nm to 3000nm.

6. The VCSEL device with electron deceleration effect according to claim 1, characterized in that: The multi-quantum well layer is made of Al x6 In y6 Ga 1-x6-y6 N / A x7 In y7 Ga 1-x7-y7 N, preferably 5 periods, wherein 0≤x6≤1, 0≤y6≤1, 0≤1-x6-y6≤1, 0≤x7≤1, 0≤y7≤1, 0≤1-x7-y7≤1, x6≠x7, y6≠y7, the bandgap of the quantum barrier is higher than the bandgap of the quantum well, and the number of quantum wells is greater than or equal to 1; quantum well Al x6 In y6 Ga 1-x6-y6 N thickness is 1nm~10nm, non-doped; quantum barrier Al x7 In y7 Ga 1-x7-y7 N thickness is 4nm to 50nm, non-doped or P-type doped or N-type doped.

7. The VCSEL device with electron deceleration effect according to claim 1, characterized in that: The material of the P-EBL layer is Al x8 In y8 Ga 1-x8-y8 N, wherein x8, y8 and 1-x8-y8 are all between 0 and 1, P-type doping, thickness is 10 to 50 nm, preferably 20 nm.

8. The VCSEL device with electron deceleration effect according to claim 1, characterized in that: The material of the P-type semiconductor material layer is Al x9 In y9 Ga 1-x9-y9 N, wherein x9, y9 and 1-x9-y9 are all between 0 and 1, the thickness is 50 to 500 nm, and 250 nm is preferred.

9. The VCSEL device with electron deceleration effect according to claim 1, characterized in that: The outer side of the upper surface of the P-type semiconductor material layer is an annular insulating layer, which serves as a current limiting layer. Its material is non-doped HfO2 or Ta2O5, with a thickness of 5 to 100 nm, preferably 15 nm, and a width of the ring of 0.2 to 10 μm, preferably 1 μm.

10. A method for preparing a VCSEL device having an electron deceleration layer according to any one of claims 1 to 9, characterized in that: The steps include: (1) First, in an MOCVD reactor, the substrate is baked at 1250-1350° C. to remove foreign matter on the substrate surface, and then a buffer layer, a bottom nitride DBR, an electron deceleration layer, a multi-quantum well layer, a P-EBL, and a P-type semiconductor material layer are grown respectively; (2) Making steps by photolithography and etching processes, exposing 40% to 70% of the electron deceleration layer, and evaporating and photolithography to make an N-type ohmic electrode; (3) photolithography a current confinement layer pattern on the P-type semiconductor material layer obtained in step (2), and depositing and growing a current confinement layer structure layer; (4) evaporating a current spreading layer on the current limiting layer obtained in step (3), wherein the material of the current spreading layer is ITO, and patterning the current spreading layer by photolithography and wet etching, the patterned current spreading layer being located above the P-type semiconductor material layer and the current limiting layer; (5) Atomic layer deposition of a top dielectric DBR layer is performed on the current spreading layer, and a P-type ohmic electrode is produced by evaporation and photolithography.