Display panel, manufacturing method thereof and display device
By providing nano-level grooves and stress absorbers formed by laser ablation on the surface of the first inorganic layer of the OLED display panel, the crack expansion problem during drop is solved, the compression resistance and drop performance of the display screen are improved, and the black spots are prevented. Appear.
Patent Information
- Application Number
- CN202310545086.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-15
AI Technical Summary
The OLED display panel is prone to black spots when it falls. The reason is that the packaging structure of bare crystal Die and metal wires is easily damaged under the action of external forces, resulting in fractures of the organic layer and cracks spreading, affecting the display performance.
Stress relief parts such as grooves and stress absorbers are provided on the surface of the first inorganic layer of the display panel away from the light emitting layer, forming nano-level grooves by laser ablation to absorb and relieve stress of the cracks and prevent further expansion of the cracks.
It effectively improves the compressive resistance of OLED displays in drop scenarios, prevents cracks from affecting the performance of organic layers and other film layers, improves the phenomenon of dark spots on the screen, and improves the drop performance of electronic devices.
Smart Images

Figure CN118973339A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of display technology, and in particular to a display panel and a manufacturing method thereof, and a display device. Background Art
[0002] In recent years, organic light-emitting diodes (OLEDs) have become a very popular display product due to their advantages such as self-luminescence, wide viewing angle, short response time, high luminous efficiency, wide color gamut, and low operating voltage. More and more electronic devices are equipped with OLED display panels.
[0003] The screen of the electronic device also integrates touch-related functional components. In the touch-related functional components, metal wires are usually used to transmit signals between the bare die and other circuit components. Since the diameter of the metal wire is very small and it is very easy to break, the metal wire is usually encapsulated by the dispensing process in the relevant technology. There is only a small gap between the dispensing encapsulation part and the panel layer panel of the OLED display panel.
[0004] However, when an electronic device falls, the glue-dispensing packaging part can easily impact the panel under the action of external force, causing damage to the panel and black spots on the screen. Summary of the invention
[0005] In view of this, the present application provides a display panel and a manufacturing method thereof, and a display device, wherein the display panel can improve the phenomenon of black spots appearing on the screen when the electronic device falls, so that the screen of the electronic device performs better in the falling scenario.
[0006] This application specifically adopts the following technical solutions:
[0007] A first aspect of an embodiment of the present application provides a display panel, the display panel comprising:
[0008] substrate;
[0009] A light-emitting layer, wherein the light-emitting layer is disposed on one side of the substrate;
[0010] a first inorganic layer, the first inorganic layer covering a surface of the light-emitting layer away from the substrate;
[0011] Wherein, a surface of the first inorganic layer away from the light-emitting layer has at least one stress relief portion.
[0012] Optionally, the stress relief portion comprises a groove, and an opening end of the groove is located on a surface of the first inorganic layer away from the light-emitting layer.
[0013] Optionally, the groove is a laser ablation groove, and the diameter of the laser ablation groove ranges from 10 to 100 nm.
[0014] Optionally, the light-emitting layer includes a pixel defining layer, and at least one light-emitting device defined by the pixel defining layer;
[0015] An orthographic projection of the groove on the substrate is located outside an orthographic projection of the light emitting device on the substrate.
[0016] Optionally, the stress relief portion further comprises a stress absorber;
[0017] The stress absorber is filled in the groove to absorb energy released from the stress concentration position on the first inorganic layer.
[0018] Optionally, the display panel further includes an organic layer, wherein the organic layer covers a surface of the first inorganic layer away from the light-emitting layer and is connected to the at least one stress relief portion.
[0019] Optionally, the display panel further includes a driving layer located between the substrate and the light-emitting layer, and a functional film layer located on a side of the organic layer away from the substrate.
[0020] Optionally, the driving layer includes a buffer layer, a polysilicon layer, a gate insulating layer, a gate metal layer, an interlayer dielectric layer, a source-drain metal layer, a planarization layer and an anode layer which are sequentially stacked in a direction away from the substrate;
[0021] and / or,
[0022] The functional film layer comprises a second inorganic layer, a touch layer, a pressure-sensitive adhesive layer, a polarizer layer, an optical adhesive layer and a glass cover plate which are sequentially stacked in a direction away from the substrate.
[0023] A second aspect of an embodiment of the present application provides a method for manufacturing a display panel, the method comprising:
[0024] forming a light-emitting layer on a substrate;
[0025] forming a first inorganic layer on a side of the light-emitting layer away from the substrate;
[0026] Wherein, a surface of the first inorganic layer away from the light-emitting layer has at least one stress relief portion.
[0027] Optionally, the stress relief portion comprises a groove, and an opening end of the groove is located on a surface of the first inorganic layer away from the light-emitting layer.
[0028] Optionally, the groove is a laser ablation groove, and the method further comprises:
[0029] The first inorganic layer is irradiated with laser to form a laser ablation groove on a surface of the first inorganic layer away from the organic light-emitting layer, wherein the diameter of the laser ablation groove is in the range of 10-100 nm.
[0030] Optionally, the laser is a femtosecond laser; and / or,
[0031] The central wavelength of the laser is 700-900nm; and / or,
[0032] The energy density of the laser is 0.03-0.08 J / cm 2 and / or,
[0033] The laser irradiation time is 10-60ps; and / or,
[0034] The laser bombards the surface of the first inorganic layer away from the organic light-emitting layer for 20-60 times.
[0035] Optionally, an orthographic projection of the groove on the substrate is outside an orthographic projection of the light-emitting layer on the substrate.
[0036] Optionally, the stress relief portion further includes a stress absorber, and the method further includes:
[0037] A stress absorber is formed on a side of the first inorganic layer away from the substrate. The stress absorber is filled in the groove and is used to absorb energy released from a stress concentration site on the first inorganic layer.
[0038] Optionally, the method further comprises:
[0039] An organic layer is formed on a side of the first inorganic layer away from the substrate, the organic layer covers a surface of the first inorganic layer away from the light-emitting layer and is connected to the at least one stress relief portion.
[0040] Optionally, before forming the light-emitting layer, the method further comprises:
[0041] forming a driving layer on the substrate;
[0042] The step of forming a light-emitting layer on a substrate comprises:
[0043] forming the light emitting layer on a side of the driving layer away from the substrate;
[0044] After forming the organic layer, the method further includes:
[0045] A functional film layer is formed on a side of the organic layer away from the substrate.
[0046] Optionally, forming a driving layer on one side of the substrate includes:
[0047] A buffer layer, a polysilicon layer, a gate insulating layer, a gate metal layer, an interlayer dielectric layer, a source-drain metal layer, a planarization layer and an anode layer are sequentially formed on the substrate;
[0048] and / or,
[0049] The forming of a functional film layer on a side of the organic layer away from the substrate comprises:
[0050] A second inorganic layer, a touch layer, a pressure-sensitive adhesive layer, a polarizer layer, an optical adhesive layer and a glass cover are sequentially formed on a side of the organic layer away from the substrate.
[0051] A third aspect of the embodiments of the present application provides a display device, which includes the display panel described in the first aspect.
[0052] In the display panel provided in the embodiment of the present application, at least one stress relief portion is provided on the surface of the first inorganic layer away from the light-emitting layer. When a crack is generated at the junction of the first inorganic layer and the light-emitting layer, the crack extending into the first inorganic layer will pass through the stress relief portion, and then the stress relief portion can eliminate the stress of the first inorganic layer, thereby preventing the crack from continuing to expand and preventing it from affecting the performance of other film layers including the organic layer. Therefore, the display panel provided in the embodiment of the present application improves the performance of electronic devices equipped with OLED display screens in falling scenarios and effectively improves the phenomenon of black spots on the screen. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0054] Figure 1 is a schematic diagram of crack expansion generated in a display panel when the whole device falls in the related art;
[0055] Figure 2 is a structural schematic diagram of a display panel provided in an embodiment of the present application;
[0056] Figure 3 It is a schematic diagram of the working principle of a stress relief portion provided in an embodiment of the present application;
[0057] Figure 4 It is a schematic diagram of the working principle of another stress relief portion provided in an embodiment of the present application;
[0058] Figure 5 is a schematic diagram of the structure of another display panel provided in an embodiment of the present application;
[0059] Figure 6 is a structural schematic diagram of another display panel provided in an embodiment of the present application;
[0060] Figure 7 It is a flow chart of a method for manufacturing a display panel provided in an embodiment of the present application.
[0061] Reference numerals:
[0062] 000, crack;
[0063] 100, substrate;
[0064] 200, light-emitting layer; 210, pixel defining layer; 220, light-emitting device;
[0065] 300, first inorganic layer; 300a, surface; 310, stress relief portion; 311, groove; 312, stress absorber;
[0066] 400, organic layer;
[0067] 500, driving layer; 510, buffer layer; 520, polysilicon layer; 530, gate insulating layer; 540, gate metal layer; 550, interlayer dielectric layer; 560, source and drain metal layer; 570, planarization layer; 580, anode layer;
[0068] 600, functional film layer; 610, second inorganic layer; 620, touch layer; 630, pressure-sensitive adhesive layer; 640, polarizer layer; 650, optical adhesive layer; 660, glass cover plate. DETAILED DESCRIPTION
[0069] In order to make the technical solutions and advantages of the present application more clear, the implementation methods of the present application will be further described in detail below with reference to the accompanying drawings.
[0070] In the related art, when an electronic device equipped with an OLED display screen falls, black spots are likely to appear on the screen. The inventors have found through testing that this is mostly caused by the collision or compression of the gold wire packaging structure of the bare die and the panel under the action of strong external force during the fall, resulting in fractures and cracks in the organic layer of the panel. The inventors further analyzed and found that if Figure 1 As shown, the crack 000 starts at the interface between the light emitting layer EL, the pixel defining layer PDL and the inorganic layer CVD, and propagates toward the inside of the inorganic layer CVD, thereby splitting the organic layer IJP.
[0071] Based on the above conclusions, an embodiment of the present application provides a display panel, which may be an OLED display panel. The display panel can prevent cracks from extending to the organic layer, thereby improving the performance of an electronic device equipped with an OLED display screen in a drop scenario and effectively improving the phenomenon of black spots on the screen.
[0072] like Figure 2 As shown, an embodiment of the present application provides a display panel, the display panel comprising:
[0073] Substrate 100;
[0074] A light emitting layer 200, wherein the light emitting layer 200 is disposed on one side of the substrate 100;
[0075] A first inorganic layer 300, the first inorganic layer 300 covers a surface of the light emitting layer 200 away from the substrate 100;
[0076] The surface 300 a of the first inorganic layer 300 away from the light emitting layer 200 has at least one stress relief portion 310 .
[0077] In the display panel provided in the embodiment of the present application, at least one stress relief portion 310 is provided on the surface 300a of the first inorganic layer 300 away from the light-emitting layer 200. When a crack 000 is generated at the junction of the first inorganic layer 300 and the light-emitting layer 200, the crack 000 extending into the first inorganic layer 300 will pass through the stress relief portion 310, and then the stress relief portion 310 can eliminate the stress of the first inorganic layer 300 here, thereby preventing the expansion of the crack 000 and preventing it from affecting the performance of other film layers including the organic layer 400. Therefore, the display panel provided in the embodiment of the present application improves the performance of electronic devices equipped with OLED display screens in falling scenarios and effectively improves the phenomenon of black spots on the screen.
[0078] In some implementations of the embodiments of the present application, Figure 2 As shown, the stress relief portion 310 is a groove 311 , and an opening end of the groove 311 is located on a surface 300 a of the first inorganic layer 300 away from the light emitting layer 200 .
[0079] like Figure 3 As shown, at least one groove 311 is formed on the surface 300a of the first inorganic layer 300 away from the light-emitting layer 200, and a compressive stress layer (ie, nanometer-level thickness) can be formed on the outer side of the groove wall of each groove 311. Figure 3When the crack 000 initiated from the edge of the light-emitting layer 200 and caused by the collision caused by the whole device falling expands to the outer edge of the groove 311, the compressive stress layer will absorb the energy of the expansion of the crack 000. At the same time, the groove 311 will alleviate the stress concentration at the tip of the crack 000, so that the stress of the first inorganic layer 300 that forms the crack 000 is released at the groove 311, thereby avoiding the further expansion of the crack 000.
[0080] Optionally, the groove 311 may be formed on the surface 300 a of the first inorganic layer 300 away from the light emitting layer 200 by etching, ablation or the like.
[0081] In some embodiments of the present application, the groove 311 is a laser ablated groove, and the diameter of the laser ablated groove is in the range of 10-100 nm.
[0082] The laser ablation groove refers to a groove 311 formed by laser irradiation. When the laser irradiates the surface 300a of the first inorganic layer 300 away from the light-emitting layer 200, the laser pulse bombards the surface 300a multiple times, causing the surface material forming the surface 300a of the first inorganic layer 300 to melt and vaporize instantly, thereby forming a groove 311 with a certain depth.
[0083] In the embodiment of the present application, when the diameter of the laser ablation groove formed on the surface 300a is in the range of 10-100nm, the laser irradiation of the surface 300a is stopped. The whole machine drop test shows that the laser ablation groove within this diameter range can withstand a certain pressure and has little effect on the display performance of the panel.
[0084] In some embodiments of the present application, the orthographic projection of the groove 311 on the substrate 100 is located outside the orthographic projection of the light emitting device 220 of the light emitting layer 200 on the substrate 100 .
[0085] like Figure 2 As shown, the light-emitting layer 200 includes a pixel defining layer 210 and at least one light-emitting device 220 defined by the pixel defining layer 210. When there are multiple light-emitting devices 220, the multiple light-emitting devices 220 are used to form multiple sub-pixels, and at least two of the multiple sub-pixels have different colors from each other.
[0086] The plurality of light emitting devices 220 are separated by the pixel defining layer 210. Exemplarily, the pixel defining layer 210 is provided with a plurality of pixel openings, each of which is used to define a layout space for a light emitting device 220, and the plurality of light emitting devices 220 are located in the plurality of pixel openings in a one-to-one correspondence.
[0087] When using laser to irradiate the first inorganic layer 300, it is necessary to avoid the position corresponding to the light emitting device 220 to prevent the formed groove 311 from affecting the light emitting device 220 and causing a large color deviation of the viewing angle. Figure 2 As shown, the orthographic projection of the groove 311 on the substrate 100 is located outside the orthographic projection of the light emitting device 220 on the substrate 100 .
[0088] In some embodiments of the present application, Figure 2 As shown, the light emitting layer 200 further includes a spacer, which is located on the side of the pixel defining layer 210 away from the substrate 100. The spacer and the pixel defining layer 210 are made of the same light-transmitting material and are made by a single patterning process. Exemplarily, the spacer and the pixel defining layer 210 are made of transparent polyimide or silicone material.
[0089] In another implementation of the embodiment of the present application, Figure 4 As shown, the stress relief portion 310 includes a groove 311 and a stress absorption member 312; the groove 311 is opened on the first inorganic layer 300, and the open end of the groove 311 is located on the surface 300a of the first inorganic layer 300 away from the light-emitting layer 200; the stress absorption member 312 is filled in the groove 311 to absorb the energy released by the stress concentration part on the first inorganic layer 300.
[0090] The stress absorber 312 is filled in the groove 311 and connected to the inner wall of the groove 311. When the crack 000 generated at the edge of the light-emitting layer 200 caused by the collision caused by the whole device falling extends to the groove 311, it will further extend to the stress absorber 312. However, the stress absorber 312 will absorb the energy of the crack 000 extension and alleviate the stress concentration at the tip of the crack 000, thereby preventing the crack 000 from continuing to expand.
[0091] The stress absorber 312 can absorb energy through a special structure or material. For example, the stress absorber 312 can be a multi-cavity, multi-porous structure. For another example, the stress absorber 312 can be an elastic member with sufficient elastic margin in the groove 311. When the stress is transmitted to the stress absorber 312, the stress absorber 312 can be deformed to consume the energy.
[0092] In some embodiments of the present application, Figure 5 As shown, the display panel further includes an organic layer 400 , which covers a surface 300 a of the first inorganic layer 300 away from the light-emitting layer 200 and is connected to at least one stress relief portion 310 .
[0093] The encapsulation layer includes multiple inorganic layers and multiple organic layers 400 , and the multiple inorganic layers and the multiple organic layers 400 are alternately stacked. Figure 6, a simple three-layer packaging structure is shown, including a first inorganic layer 300, an organic layer 400, and a second inorganic layer 610, wherein the first inorganic layer 300 and the second are formed by a chemical vapor deposition process, and the organic layer 400 is formed by an inkjet printing process.
[0094] In an embodiment of the present application, the stress relief portion 310 is located between the first inorganic layer 300 and the organic layer 400 of the encapsulation layer, and is connected to the organic layer 400, so that when the crack 000 generated at the edge of the self-luminous layer 200 expands toward the inside of the first inorganic layer 300, on the expansion path of the crack 000, the stress relief portion 310 is located before the organic layer 400, so the crack 000 will be eliminated from the stress relief portion 310 and will not extend to the organic layer 400, thereby protecting the organic layer 400 and further ensuring the display performance of the display panel.
[0095] In the embodiment of the present application, the display panel further includes a driving layer 500 located between the substrate 100 and the light-emitting layer 200 , and a functional film layer 600 located on a side of the organic layer 400 away from the substrate 100 .
[0096] like Figure 5 As shown, the driving layer 500 includes a buffer layer 510, a polysilicon layer 520, a gate insulating layer 530, a gate metal layer 540, an interlayer dielectric layer 550, a source-drain metal layer 560, a planarization layer 570 and an anode layer 580 which are sequentially stacked in a direction away from the substrate 100.
[0097] In some embodiments of the present application, the gate insulation layer 530 includes a first gate insulation layer GI1 and a second gate insulation layer GI2, the gate metal layer 540 includes a first gate layer G1 and a second gate layer G2, the source-drain metal layer 560 includes a first source-drain layer SD1 and a second source-drain layer SD2, and the planarization layer 570 includes a first planarization layer PLN1 and a second planarization layer PLN2.
[0098] The substrate 100 may be made of polyimide material, which has temperature resistance, excellent chemical stability and mechanical properties.
[0099] The buffer layer 510 is generally made of organic materials and is used to prevent water vapor from penetrating, thereby extending the service life of the OLED display panel and improving the flatness of the panel surface.
[0100] The first gate insulating layer GI1 covers the side of the polysilicon layer 520 away from the substrate 100 and can be made of polyimide to have high bending strength and tensile strength, so that when the display panel is bent, it can bend accordingly with the display panel and ensure its insulation.
[0101] The first gate layer G1 is located on a side of the first gate insulating layer GI1 away from the substrate 100 and is used to create or eliminate a channel between the source and the drain, thereby allowing or preventing electrons from flowing through.
[0102] The second gate insulating layer GI2 covers the side of the first gate layer G1 away from the substrate 100 and can be made of polyimide to have high bending strength and tensile strength, so that when the display panel is bent, it can cooperate with the display panel to make corresponding bends and ensure its insulation.
[0103] The second gate layer G2 is located on a side of the second gate insulating layer GI2 away from the substrate 100 and is used to create or eliminate a channel between the source and the drain, thereby allowing or preventing electrons from flowing through.
[0104] The interlayer dielectric layer 550 is located on the side of the second gate layer G2 away from the substrate 100 and is generally made of a low-k material to reduce time delay and increase speed. For example, silicon oxide material may be selected.
[0105] The first source-drain electrode layer SD1 is located on a side of the interlayer dielectric layer 550 away from the substrate 100 , and is used to penetrate through via holes provided in the interlayer dielectric layer 550 and the gate insulating layer 530 and overlap with the active layer.
[0106] The first planar layer PLN1 is located on a side of the first source / drain layer SD1 away from the substrate 100 , and is used to meet the planarity requirement of the substrate plane.
[0107] The second source-drain layer SD2 is located on a side of the first planar layer PLN1 away from the substrate 100 , and is used to penetrate through via holes formed in the first planar layer PLN1 , the interlayer dielectric layer 550 and the gate insulating layer 530 , and overlap with the active layer.
[0108] The second planar layer PLN2 is located on a side of the second source / drain layer SD2 away from the substrate 100 , and is used to meet the planarity requirement of the substrate plane.
[0109] The anode layer 580 is located on the side of the second planar layer PLN2 away from the substrate 100. In the embodiment of the present application, the display panel further includes a cathode layer (not shown in the figure), which is located on the side of the light emitting layer 200 away from the substrate 100 and on the side of the first inorganic layer 300 close to the substrate 100.
[0110] like Figure 6 As shown, the functional film layer 600 includes a second inorganic layer 610 , a touch layer 620 , a pressure-sensitive adhesive layer 630 , a polarizer layer 640 , an optical adhesive layer 650 and a glass cover plate 660 which are sequentially stacked in a direction away from the substrate 100 .
[0111] Among them, Figure 6As shown, the touch layer 620 includes a plurality of touch sensors, and the plurality of touch sensors include a plurality of touch sensors Tx extending along a first direction and a plurality of touch sensors Rx extending along a second direction, wherein the first direction is perpendicular to the second direction. Figure 6 As shown, the touch sensor includes a portion located in the first touch layer M1 and a portion located in the second touch layer M2, wherein the first touch layer M1 and the second touch layer M2 are located in different layers. An interlayer insulating layer IL is provided between the first touch layer M1 and the second touch layer M2, and the interlayer insulating layer IL is made of inorganic insulating material.
[0112] In summary, in the display panel provided in the embodiment of the present application, the surface 300a of the first inorganic layer 300 away from the light-emitting layer 200 is provided with at least one stress relief portion 310. When a crack 000 is generated at the junction of the first inorganic layer 300 and the light-emitting layer 200, the crack 000 extending into the first inorganic layer 300 will pass through the stress relief portion 310, and then the stress relief portion 310 can eliminate the stress of the first inorganic layer 300, thereby preventing the crack 000 from continuing to expand and preventing it from affecting the performance of other film layers including the organic layer 400. Therefore, the display panel provided in the embodiment of the present application improves the performance of electronic devices equipped with OLED display screens in falling scenarios and effectively improves the phenomenon of black spots on the screen.
[0113] The present application also provides a method for manufacturing a display panel, which is used to manufacture the display panel described in any of the above embodiments. Figure 7 As shown, the manufacturing method includes:
[0114] S710, forming a light-emitting layer on a substrate;
[0115] S720, forming a first inorganic layer on a side of the light-emitting layer away from the substrate, wherein a surface of the first inorganic layer away from the light-emitting layer has at least one stress relief portion.
[0116] The display panel manufactured by the manufacturing method provided in the embodiment of the present application has at least one stress relief portion disposed on the surface of the first inorganic layer away from the light-emitting layer. When a crack is generated at the junction of the first inorganic layer and the light-emitting layer, the crack extending into the first inorganic layer will pass through the stress relief portion, and the stress relief portion can eliminate the stress of the first inorganic layer here, thereby preventing the expansion of the crack and avoiding it from affecting the performance of other film layers including the organic layer. Therefore, the display panel provided in the embodiment of the present application improves the performance of electronic devices equipped with OLED display screens in falling scenarios and effectively improves the phenomenon of black spots on the screen.
[0117] In some implementations of the embodiments of the present application, the stress relief portion is a groove, and an open end of the groove is located on a surface of the first inorganic layer away from the light-emitting layer.
[0118] A compressive stress layer with a thickness of nanometers can be formed on the outer side of the groove wall of each groove. Figure 3 When the crack initiated from the edge of the light-emitting layer and caused by the collision caused by the whole device falling expands to the outer edge of the groove, the compressive stress layer absorbs the energy of the crack expansion. At the same time, the groove alleviates the stress concentration at the tip of the crack, so that the stress of the first inorganic layer that forms the crack is released at the groove, thereby avoiding further expansion of the crack.
[0119] In some embodiments, the groove is a laser ablation groove, and the manufacturing method further includes: irradiating the first inorganic layer with a laser to form a laser ablation groove on a surface of the first inorganic layer away from the organic light-emitting layer, wherein the diameter of the laser ablation groove ranges from 10 to 100 nm.
[0120] The whole machine drop test shows that the laser ablation grooves within this diameter range can withstand a certain amount of pressure and have little effect on the display performance of the panel.
[0121] In some embodiments of the present application, the laser used to irradiate the first inorganic layer satisfies at least one of the following conditions:
[0122] The laser is a femtosecond laser;
[0123] The central wavelength of the laser is 700-900nm;
[0124] The energy density of the laser is 0.03-0.08J / cm 2 ;
[0125] The laser irradiation time is 10-60ps; and,
[0126] The laser bombards the surface of the first inorganic layer away from the organic light-emitting layer for 20-60 times.
[0127] Optionally, the central wavelength of the laser may be, for example, 700 nm, 750 nm, 800 nm, 850 nm or 900 nm.
[0128] Optionally, the energy density of the laser can be, for example, 0.03, 0.04, 0.05, 0.069, 0.07 or 0.08 J / cm 2 .
[0129] Optionally, the irradiation time of the laser may be, for example, 10, 20, 30, 40, 50 or 60 ps.
[0130] Optionally, the number of times that the laser strikes the surface of the first inorganic layer away from the organic light-emitting layer may be, for example, 20, 30, 40, 50 or 60 times.
[0131] In some embodiments of the present application, an orthographic projection of the groove on the substrate is located outside an orthographic projection of the light-emitting device of the light-emitting layer on the substrate.
[0132] In some embodiments of the present application, after forming the first inorganic layer, a femtosecond laser is used to irradiate the first inorganic layer, and the central wavelength of the laser is 800 nm and the energy density is 0.06 J / cm 2 The irradiation time is 10-60ps, and the bombardment times are 20-60 times, thereby forming a laser ablation groove with a diameter of 10-100nm on the surface of the first inorganic layer away from the organic light-emitting layer. The position of the laser irradiation should avoid the light-emitting device of the light-emitting layer to prevent the laser ablation groove from affecting the light-emitting device and causing a large visual angle deviation.
[0133] After laser irradiation, the display panel continues to undergo TFE (Thin Film Encapsulation) encapsulation and DOT (direct on-cell touch, the touch screen is directly embedded in the display screen) routing according to conventional methods in the art.
[0134] In some embodiments of the present application, the stress relief portion also includes a stress absorber, and the manufacturing method also includes: forming a stress absorber on a side of the first inorganic layer away from the substrate, the stress absorber is filled in the groove, and the stress absorber is used to absorb the energy released by the stress concentration part on the first inorganic layer.
[0135] The stress absorber is filled in the groove and connected to the inner wall of the groove. When the crack caused by the collision caused by the whole device falling and generated at the edge of the light-emitting layer extends to the groove, it will further extend to the stress absorber. However, the stress absorber will absorb the energy of the crack extension and alleviate the stress concentration at the crack tip, thereby preventing the crack from continuing to expand.
[0136] The stress absorber can absorb energy through a special structure or material. For example, the stress absorber can be a multi-cavity, multi-porous structure. For another example, the stress absorber can be an elastic member with sufficient elastic margin in the groove. When the stress is transmitted to the stress absorber, the stress absorber can be deformed to consume the energy.
[0137] In some embodiments of the present application, the manufacturing method further includes: forming an organic layer on a side of the first inorganic layer away from the substrate, wherein the organic layer covers a surface of the first inorganic layer away from the light-emitting layer and is connected to the at least one stress relief portion.
[0138] In some embodiments of the present application, before forming the light-emitting layer, the manufacturing method further includes: forming a driving layer on the substrate.
[0139] Illustratively, before forming the light emitting layer, a buffer layer, a polysilicon layer, a gate insulating layer, a gate metal layer, an interlayer dielectric layer, a source-drain metal layer, a planarization layer and an anode layer are sequentially formed on the substrate.
[0140] In some embodiments of the present application, forming the light-emitting layer on the substrate includes: forming the light-emitting layer on a side of the driving layer away from the substrate.
[0141] In some embodiments of the present application, after forming the organic layer, the manufacturing method further includes: forming a functional film layer on a side of the organic layer away from the substrate.
[0142] Illustratively, after the organic layer is formed, a second inorganic layer, a touch layer, a pressure-sensitive adhesive layer, a polarizer layer, an optical adhesive layer and a glass cover are sequentially formed on a side of the organic layer away from the substrate.
[0143] The display panel manufactured by the manufacturing method provided in the embodiment of the present application has at least one stress relief portion disposed on the surface of the first inorganic layer away from the light-emitting layer. When a crack is generated at the junction of the first inorganic layer and the light-emitting layer, the crack extending into the first inorganic layer will pass through the stress relief portion, and the stress relief portion can eliminate the stress of the first inorganic layer here, thereby preventing the expansion of the crack and avoiding it from affecting the performance of other film layers including the organic layer. Therefore, the display panel provided in the embodiment of the present application improves the performance of electronic devices equipped with OLED display screens in falling scenarios and effectively improves the phenomenon of black spots on the screen.
[0144] An embodiment of the present application further provides a display device, which may be, for example, an OLED display device. The display device includes the display panel described in any of the above embodiments.
[0145] Therefore, in the display device provided in the embodiment of the present application, at least one stress relief portion is provided on the surface of the first inorganic layer of the display panel away from the light-emitting layer. When a crack is generated at the junction of the first inorganic layer and the light-emitting layer, the crack extending into the first inorganic layer will pass through the stress relief portion, and then the stress relief portion can eliminate the stress of the first inorganic layer here, thereby preventing the expansion of the crack and avoiding it from affecting the performance of other film layers including the organic layer. Therefore, the display panel provided in the embodiment of the present application improves the performance of electronic devices equipped with OLED display screens in falling scenarios and effectively improves the phenomenon of black spots on the screen.
[0146] Example 1
[0147] The whole-machine drop test was performed on an electronic device equipped with a display panel in the related art and three electronic devices equipped with a display panel provided in the embodiment of the present application, and the number of test samples for each device was 5. Among them, in the display panel provided in the embodiment of the present application, the stress relief portion was a laser-etched groove, and the test pressures were 60N, 80N, 100N, and 120N, respectively, and the test results shown in Table 1 below were obtained.
[0148] Table 1. Results of drop tests on four electronic devices
[0149]
[0150] Among them, test sample 1: an electronic device equipped with a display panel in the related art;
[0151] Test sample 2: an electronic device equipped with a display panel provided in an embodiment of the present application, wherein the average diameter of the laser-etched grooves in the display panel is 23 nm;
[0152] Test sample 3: an electronic device equipped with a display panel provided in an embodiment of the present application, wherein the average diameter of the laser-etched grooves in the display panel is 62 nm;
[0153] Test sample 4: an electronic device equipped with the display panel provided by an embodiment of the present application, wherein the average diameter of the laser-etched grooves in the display panel is 87 nm.
[0154] See Table 1 above:
[0155] When the test pressure of the whole device drop test is 60N, the number of electronic devices with black spots on the screen in these four test samples is 0, that is, test samples 1-4 all pass the test;
[0156] When the test pressure of the whole device drop test is 80N, the number of electronic devices with black spots on the screen in test sample 1 is 5, and the number of electronic devices with black spots on the screen in test samples 2-4 is 0, that is, all electronic devices in test sample 1 fail the test, and all electronic devices in test samples 2-4 pass the test;
[0157] When the test pressure of the whole device drop test is 100N, the number of electronic devices with black spots on the screen in test sample 2 is 3, and the number of electronic devices with black spots on the screen in test samples 3-4 is 0, that is, 3 electronic devices in test sample 2 failed the test, and all electronic devices in test samples 3-4 passed the test;
[0158] When the test pressure of the whole machine drop test is 120N, the number of electronic devices with black spots on the screen in test sample 2 is 2, the number of electronic devices with black spots on the screen in test sample 3 is 1, and the number of electronic devices with black spots on the screen in test sample 4 is 3, that is, 2 electronic devices in test sample 2 failed the test, 1 electronic device in test sample 3 failed the test, and 3 electronic devices in test sample 4 failed the test.
[0159] From the above analysis, we can know that in the whole machine drop test, the compression resistance from high to low are test sample 3, test sample 4, test sample 2 and test sample 1. Therefore, when the average diameter of the laser etched groove is 62nm, its ability to absorb crack expansion energy is relatively the strongest, so the display panel achieves the best compression and drop resistance.
[0160] In the present application, it should be understood that the terms "first", "second", "third", etc. are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features.
[0161] The above description is only for the purpose of facilitating those skilled in the art to understand the technical solution of the present application and is not intended to limit the present application. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A display panel, It is characterized in that The display panel comprises: A substrate (100); A light-emitting layer (200), wherein the light-emitting layer (200) is disposed on one side of the substrate (100); A first inorganic layer (300), the first inorganic layer (300) covering a surface of the light-emitting layer (200) away from the substrate (100); The surface (300a) of the first inorganic layer (300) away from the light-emitting layer (200) has at least one stress relief portion (310).
2. The display panel according to claim 1, It is characterized in that The stress relief portion (310) comprises a groove (311), and an opening end of the groove (311) is located on a surface (300a) of the first inorganic layer (300) away from the light-emitting layer (200).
3. The display panel according to claim 2, It is characterized in that The groove (311) is a laser ablation groove, and the diameter of the laser ablation groove ranges from 10 to 100 nm.
4. The display panel according to claim 2 or 3, It is characterized in that The light-emitting layer (200) comprises a pixel defining layer (210) and at least one light-emitting device (220) defined by the pixel defining layer (210); An orthographic projection of the groove (311) on the substrate (100) is located outside an orthographic projection of the light-emitting device (220) on the substrate (100).
5. The display panel according to claim 2, It is characterized in that The stress relief portion (310) further includes a stress absorbing member (312); The stress absorber (312) is filled in the groove (311) and is used to absorb energy released from a stress concentration location on the first inorganic layer (300).
6. The display panel according to claim 1, It is characterized in that The display panel further comprises an organic layer (400), wherein the organic layer (400) covers a surface (300a) of the first inorganic layer (300) away from the light-emitting layer (200) and is connected to the at least one stress relief portion (310).
7. The display panel according to claim 6, It is characterized in that The display panel further comprises a driving layer (500) located between the substrate (100) and the light-emitting layer (200), and a functional film layer (600) located on a side of the organic layer (400) away from the substrate (100).
8. The display panel according to claim 7, It is characterized in that The driving layer (500) comprises a buffer layer (510), a polysilicon layer (520), a gate insulating layer (530), a gate metal layer (540), an interlayer dielectric layer (550), a source-drain metal layer (560), a planar layer (570), and an anode layer (580) which are sequentially stacked in a direction away from the substrate (100); and / or, The functional film layer (600) comprises a second inorganic layer (610), a touch layer (620), a pressure-sensitive adhesive layer (630), a polarizer layer (640), an optical adhesive layer (650), and a glass cover plate (660) which are sequentially stacked in a direction away from the substrate (100).
9. A method for manufacturing a display panel, It is characterized in that The method comprises: forming a light-emitting layer (200) on a substrate (100); forming a first inorganic layer (300) on a side of the light-emitting layer (200) away from the substrate (100); The surface (300a) of the first inorganic layer (300) away from the light-emitting layer (200) has at least one stress relief portion (310).
10. The method according to claim 9, It is characterized in that The stress relief portion (310) comprises a groove (311), and an opening end of the groove (311) is located on a surface (300a) of the first inorganic layer (300) away from the light-emitting layer (200).
11. The method according to claim 10, It is characterized in that The groove (311) is a laser ablation groove, and the method further comprises: The first inorganic layer (300) is irradiated with laser to form a laser ablation groove on a surface (300a) of the first inorganic layer (300) away from the organic light-emitting layer (200), wherein the diameter of the laser ablation groove is in the range of 10-100 nm.
12. The method according to claim 11, It is characterized in that The laser is a femtosecond laser; and / or, The central wavelength of the laser is 700-900nm; and / or, The energy density of the laser is 0.03-0.08 J / cm 2 and / or, The laser irradiation time is 10-60ps; and / or, The laser bombards the surface (300a) of the first inorganic layer (300) away from the organic light-emitting layer (200) for a number of times ranging from 20 to 60 times.
13. The method according to any one of claims 10 to 12, It is characterized in that The orthographic projection of the groove (311) on the substrate (100) is located outside the orthographic projection of the light-emitting layer (200) on the substrate (100).
14. The method according to claim 10, It is characterized in that The stress relief portion (310) further comprises a stress absorber (312), and the method further comprises: A stress absorber (312) is formed on a side of the first inorganic layer (300) away from the substrate (100), and the stress absorber (312) is filled in the groove (311). The stress absorber (312) is used to absorb energy released by a stress concentration portion on the first inorganic layer (300).
15. The method according to claim 9, It is characterized in that The method further comprises: An organic layer (400) is formed on a side of the first inorganic layer (300) away from the substrate (100), and the organic layer (400) covers a surface (300a) of the first inorganic layer (300) away from the light-emitting layer (200) and is connected to the at least one stress relief portion (310).
16. The method according to claim 15, It is characterized in that Before forming the light-emitting layer (200), the method further comprises: forming a driving layer (500) on the substrate (100); The step of forming a light-emitting layer (200) on a substrate (100) comprises: forming the light-emitting layer (200) on a side of the driving layer (500) away from the substrate (100); After forming the organic layer (400), the method further comprises: A functional film layer (600) is formed on a side of the organic layer (400) away from the substrate (100).
17. The method according to claim 16, It is characterized in that The step of forming a driving layer (500) on one side of the substrate (100) comprises: A buffer layer (510), a polysilicon layer (520), a gate insulating layer (530), a gate metal layer (540), an interlayer dielectric layer (550), a source-drain metal layer (560), a planarization layer (570), and an anode layer (580) are sequentially formed on the substrate (100); and / or, The forming of a functional film layer (600) on a side of the organic layer (400) away from the substrate (100) comprises: A second inorganic layer (610), a touch layer (620), a pressure-sensitive adhesive layer (630), a polarizer layer (640), an optical adhesive layer (650) and a glass cover plate (660) are sequentially formed on a side of the organic layer (400) away from the substrate (100).
18. A display device, It is characterized in that The display device comprises the display panel according to any one of claims 1 to 8.