Heat-sensitive recording medium

By providing a back coating containing ethylene-vinyl alcohol copolymer and ethylene-acrylic copolymer on the back of the thermal recording body, the water droplet problem caused by moisture vaporization in high-energy printing is solved, and excellent water vapor barrier properties are achieved and printing stability.

CN118973827APending Publication Date: 2024-11-15NIPPON PAPER IND CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202380031543.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-27
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the case of high-energy printing such as medical use, the moisture in the thermal recording body will vaporize, causing water droplets to appear on the back, causing device failure, affecting printing quality and equipment stability.

Method used

A thermal recording layer is provided on the support of the thermal recording body, and a back coating is set on the opposite side. The back coating contains ethylene-vinyl alcohol copolymer and ethylene-acrylic copolymer to achieve water vapor barrier properties .

Benefits of technology

It effectively prevents the production of water vapor on the back, ensures the stability of equipment and printing quality during long-term printing, avoids water droplets adhesion, and significantly improves the barrier properties of water vapor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005064858190000211
    Figure BDA0005064858190000211
Patent Text Reader

Abstract

[Problem] To provide a heat-sensitive recording material having water vapor barrier properties with respect to moisture in the heat-sensitive recording material. [Solution] A heat-sensitive recording material in which a heat-sensitive recording layer that contains a colorless or light-colored electron-donating leuco dye and an electron-accepting developer and a back coat layer that contains an ethylene-vinyl alcohol copolymer and an ethylene-acrylic copolymer are provided on a support body, the back coat layer being on the surface opposite the heat-sensitive recording layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a thermosensitive recording medium having water vapor barrier properties on the back side. Background Art

[0002] Generally, a thermosensitive recording medium is formed by applying a coating liquid containing a colorless or light-colored electron-donating leuco dye (hereinafter also referred to as "leuco dye") and an electron-accepting developer (hereinafter also referred to as "developer") on a support such as paper, synthetic paper, film, or plastic to form a thermosensitive recording layer, and developing color through an instantaneous chemical reaction caused by heating with a thermal head, thermal stamp, thermal pen, laser, etc., thereby obtaining a recorded image. Thermosensitive recording medium is widely used as a recording medium such as a fax, a terminal printer for a computer, an automatic ticket machine, a measuring recorder, and receipts for supermarkets and / or convenience stores.

[0003] In order to obtain good water resistance, a thermal recording material having a back coating layer containing an adhesive such as polyvinyl alcohol is known (Patent Document 1, etc.) In addition, paper substrates containing ethylene copolymerized polyvinyl alcohol and ethylene / acrylic acid copolymers are known to have water vapor barrier properties (Patent Documents 2 to 4, etc.).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 2003-175671

[0007] Patent Document 2: Japanese Patent Application Laid-Open No. 2013-169988

[0008] Patent Document 3: Japanese Patent Application Laid-Open No. 2014-173201

[0009] Patent Document 4: Japanese Patent Application Laid-Open No. 2020-190063 Summary of the invention

[0010] Problems to be solved by the invention

[0011] Since medical and other uses require high-sensitivity printers to print at high energy, the thermal head will become hot. If high-temperature printing is continued for a long time, the moisture in the thermal recording medium will vaporize and water droplets will be generated on the back side that has never been in contact with the thermal head, which may cause device failure.

[0012] Therefore, the present invention provides a thermosensitive recording material having water vapor barrier properties against water in the thermosensitive recording material.

[0013] Means for solving problems

[0014] After intensive research, the present inventors found that the above-mentioned problem can be solved by providing a thermosensitive recording layer on the support of the thermosensitive recording body, providing a back coating layer on the side opposite to the thermosensitive recording layer, and making the back coating layer contain ethylene-vinyl alcohol copolymer and ethylene-acrylic acid copolymer, thereby completing the present invention.

[0015] That is, the present invention is a thermosensitive recording medium, which is provided on a support with: a thermosensitive recording layer containing a colorless or light-colored electron-donating leuco dye and an electron-accepting developer, and a back coating layer on the side opposite to the thermosensitive recording layer, wherein the back coating layer contains an ethylene-vinyl alcohol copolymer and an ethylene-acrylic acid copolymer.

[0016] Effects of the Invention

[0017] According to the present invention, it is possible to obtain a thermosensitive recording medium having excellent water vapor barrier properties on the back side (ie, the side of the support opposite to the thermosensitive recording layer) and in which water vapor is not generated on the back side even during long-term printing. DETAILED DESCRIPTION

[0018] The thermosensitive recording medium of the present invention has a thermosensitive recording layer containing a leuco dye and a developer on a support, and has a back coating layer on the side of the support opposite to the thermosensitive recording layer.

[0019] The back coating layer of the present invention contains an ethylene-vinyl alcohol copolymer and an ethylene-acrylic acid copolymer.

[0020] The ethylene-vinyl alcohol copolymer used in the present invention is a polymer having ethylene units and vinyl alcohol units. The ethylene-vinyl alcohol copolymer is generally obtained by polymerizing ethylene and vinyl ester and saponifying the obtained ethylene-vinyl ester copolymer.

[0021] From the viewpoint of using a water-based coating, the ethylene content is preferably 3 to 20 mol%. In addition, in order to impart barrier properties, the saponification degree is preferably 80 to 100 mol%. When the saponification degree is less than 80 mol%, sufficient barrier properties and moisture resistance cannot be obtained.

[0022] The ethylene-acrylic acid copolymer used in the present invention is a copolymer obtained by emulsion polymerization of ethylene and acrylic acid monomers. As the acrylic acid monomer, acrylic acid and methacrylic acid are preferred, and acrylic acid is more preferred.

[0023] The ethylene-acrylic acid copolymer is preferably any one or more of the following: ethylene-acrylic acid copolymer, ethylene-methacrylic acid copolymer, ethylene-methyl acrylate copolymer, ethylene-methyl methacrylate copolymer, ethylene-ethyl acrylate copolymer, ethylene-ethyl methacrylate copolymer, ethylene-butyl acrylate copolymer, and ethylene-butyl methacrylate copolymer. In the copolymer, a small amount of monomers containing other compounds copolymerizable with ethylene and acrylic acid monomers may be copolymerized.

[0024] Among them, ethylene-acrylic acid copolymer and ethylene-methacrylic acid copolymer are more preferred, and ethylene-acrylic acid copolymer is even more preferred.

[0025] Specific examples of ethylene-acrylic acid-based copolymers include aqueous dispersions of ethylene-acrylic acid copolymer ammonium salts available as ZAIKTHENE (registered trademark) AC (copolymerization ratio of acrylic acid: 20%, manufactured by Sumitomo Seika Chemicals Co., Ltd.).

[0026] In addition, the back coat layer of the present invention may contain a water-soluble polymer, a water-dispersible resin, a pigment, etc. to the extent that there is no problem in the water vapor barrier property.

[0027] Examples of the water-soluble polymer include: polyvinyl alcohols other than ethylene-vinyl alcohol copolymers such as completely saponified polyvinyl alcohol and partially saponified polyvinyl alcohol; proteins such as casein, soy protein, and synthetic protein; starches such as oxidized starch, cationic starch, urea phosphate starch, and hydroxyethyl etherified starch; cellulose derivatives such as carboxymethyl cellulose, hydroxymethyl cellulose, and hydroxyethyl cellulose; polyvinyl pyrrolidone, sodium alginate, and the like.

[0028] Examples of the water-dispersible resin include natural rubber, diene rubber, non-diene rubber, and thermoplastic elastomer.

[0029] As the pigment, any pigment that can be used for a heat-sensitive recording layer can be used as appropriate, and aluminum hydroxide, silica, kaolin, and calcined kaolin are preferred, and aluminum hydroxide is more preferred.

[0030] The back coat layer may further contain, as required, lubricants, crosslinking agents, ultraviolet absorbers, dispersants, defoaming agents, fluorescent dyes, etc. that can be used in the thermosensitive recording layer, within a range not impairing the expected effects on the above-mentioned subjects.

[0031] The content (solid content) of the ethylene-vinyl alcohol copolymer in the back coat layer is preferably 10 to 80% by weight, more preferably 10 to 50% by weight.

[0032] The content (solid content) of the ethylene-acrylic acid-based copolymer in the back coat layer is preferably 10 to 80% by weight, more preferably 50 to 80% by weight.

[0033] However, the total content (solid content) of the ethylene-vinyl alcohol copolymer and the ethylene-acrylic acid copolymer in the back coat layer is preferably 50 to 100 wt %, more preferably 50 to 90 wt %, and even more preferably 70 to 90 wt %.

[0034] The content ratio (solid content) of the ethylene-acrylic acid-based copolymer to the ethylene-vinyl alcohol copolymer is preferably 2.5 to 40 parts, more preferably 10 to 40 parts, based on 10 parts by mass of the ethylene-vinyl alcohol copolymer.

[0035] The content (solid content) of the pigment in the back coat layer is preferably 50 to 10% by weight, more preferably 30 to 10% by weight.

[0036] The coating amount of the back coating layer is determined according to the required performance and recording adaptability. Although there is no special restriction on this, the usual coating amount is: 0.1 to 5 g / m 2 Among them, if it is 2.5~4.5g / m 2 A value of about 0.1% or less is preferred because it has excellent water vapor barrier properties and has good quality as a thermosensitive recording material.

[0037] The heat-sensitive recording layer of the present invention contains a leuco dye and a developer, and may also contain a sensitizer, a binder, a pigment, a cross-linking agent, an image stabilizer, and other components as desired.

[0038] As the leuco dye used in the present invention, all known products in the existing pressure-sensitive or heat-sensitive recording paper field can be used, although no particular restrictions are made to this, it is preferably triphenylmethane series compounds, fluorane series compounds, fluorene series, divinyl series compounds etc. The specific example of representative colorless or light-colored leuco dye (dye precursor) is shown below. In addition, these dye precursors can be used alone or in combination with more than 2 kinds.

[0039] <Triphenylmethane-based leuco dyes>

[0040] 3,3-Bis(p-dimethylaminophenyl)-6-dimethylaminophthalide [also known as crystal violet lactone]; 3,3-Bis(p-dimethylaminophenyl)phthalide [also known as malachite green lactone].

[0041] <Fluoran-based leuco dyes>

[0042] 3-Diethylamino-6-methylfluoran; 3-diethylamino-6-methyl-7-anilinofluoran; 3-diethylamino-6-methyl-7-(o-, p-dimethylanilino)fluoran; 3-diethylamino-6-methyl-7-chlorofluoran; 3-diethylamino-6-methyl-7-(m-trifluoromethylanilino)fluoran; 3-diethylamino-6-methyl-7-(o-chloroanilino)fluoran; 3-diethylamino-6-methyl-7-(p-chloroanilino)fluoran; 3-diethylamino-6-methyl-7-(o-fluoroanilino)fluoran; 3-diethylamino-6-methyl-7-(m-methylanilino)fluoran; 3-diethylamino-6-methyl-7-n-octylanilinofluoran; 3-diethylamino-6-methyl-7-n-octylaminofluoran 3-Diethylamino-6-methyl-7-benzylaminofluoran; 3-Diethylamino-6-methyl-7-dibenzylaminofluoran; 3-Diethylamino-6-chloro-7-methylfluoran; 3-Diethylamino-6-chloro-7-anilinofluoran; 3-Diethylamino-6-chloro-7-p-methylanilinofluoran; 3-Diethylamino-6-ethoxyethyl-7-anilinofluoran; 3-Diethylamino-7-methylfluoran; 3-Diethylamino-7-chlorofluoran; 3-Diethylamino-7-(m-trifluoromethylanilino)fluoran; 3-Diethylamino-7-(o-chloroanilino)fluoran; 3-Diethylamino-7-(p-chloroanilino)fluoran; 3-Diethylamino-7-(o-fluoroanilino)fluoran; 3-Diethylamino-benzo[ a〕fluoran; 3-diethylamino-benzo〔c〕fluoran; 3-dibutylamino-6-methyl-fluoran; 3-dibutylamino-6-methyl-7-anilinofluoran; 3-dibutylamino-6-methyl-7-(o-, p-dimethylanilino)fluoran; 3-dibutylamino-6-methyl-7-(o-chloroanilino)fluoran; 3-dibutylamino-6-methyl-7-(p-chloroanilino)fluoran; 3-dibutylamino-6-methyl-7-(o-fluoroanilino)fluoran; 3-dibutylamino-6-methyl-7-(m-trifluoromethylanilino)fluoran; 3-dibutylamino-6-methyl-chlorofluoran; 3-dibutylamino-6-ethoxyethyl-7-anilinofluoran; 3-dibutylamino-6-chloro-7-phenyl Amine fluoran; 3-dibutylamino-6-methyl-7-p-methylanilinofluoran; 3-dibutylamino-7-(o-chloroanilino)fluoran; 3-dibutylamino-7-(o-fluoroanilino)fluoran; 3-di-n-pentylamino-6-methyl-7-anilinofluoran; 3-di-n-pentylamino-6-methyl-7-(p-chloroanilino)fluoran; 3-di-n-pentylamino-7-(m-trifluoromethylanilino)fluoran; 3-di-n-pentylamino-6-chloro-7-anilinofluoran; 3-di-n-pentylamino-7-(p-chloroanilino)fluoran; 3-pyrrolidinyl-6-methyl-7-anilinofluoran; 3-piperidinyl-6-methyl-7-anilinofluoran; 3-(N-methyl-N-propylamino)-6-methyl-7-anilinofluoran;3-(N-methyl-N-cyclohexylamino)-6-methyl-7-anilinofluoran; 3-(N-ethyl-N-cyclohexylamino)-6-methyl-7-anilinofluoran; 3-(N-ethyl-N-hexylamino)-6-methyl-7-(p-chloroanilino)fluoran; 3-(N-ethyl-p-toluidinyl)-6-methyl-7-anilinofluoran; 3-(N-ethyl-N-isopentylamino)-6-methyl-7-anilinofluoran; 3-(N-ethyl-N-isopentylamino)-6-chloro-7-anilinofluoran; 3-(N-ethyl- N-tetrahydrofurfurylamino)-6-methyl-7-anilinofluoran; 3-(N-ethyl-N-isobutylamino)-6-methyl-7-anilinofluoran; 3-(N-ethyl-N-ethoxypropylamino)-6-methyl-7-anilinofluoran; 3-cyclohexylamino-6-chlorofluoran; 2-(4-oxahexyl)-3-dimethylamino-6-methyl-7-anilinofluoran; 2-(4-oxahexyl)-3-diethylamino-6-methyl-7-anilinofluoran; 2-(4-oxahexyl)-3-dipropylamino-6-methyl-7- Aniline fluoran; 2-methyl-6-p-(p-dimethylaminophenyl)aminoaniline fluoran; 2-methoxy-6-p-(p-dimethylaminophenyl)aminoaniline fluoran; 2-chloro-3-methyl-6-p-(p-phenylaminophenyl)aminoaniline fluoran; 2-chloro-6-p-(p-dimethylaminophenyl)aminoaniline fluoran; 2-nitro-6-p-(p-diethylaminophenyl)aminoaniline fluoran; 2-amino-6-p-(p-diethylaminophenyl)aminoaniline fluoran; 2-diethylamino-6-p-(p-diethylaminophenyl)aminoaniline fluoran ; 2-phenyl-6-methyl-6-p-(p-phenylaminophenyl)aminoanilinofluoran; 2-benzyl-6-p-(p-phenylaminophenyl)aminoanilinofluoran; 2-hydroxy-6-p-(p-phenylaminophenyl)aminoanilinofluoran; 3-methyl-6-p-(p-dimethylaminophenyl)aminoanilinofluoran; 3-diethylamino-6-p-(p-diethylaminophenyl)aminoanilinofluoran; 3-diethylamino-6-p-(p-dibutylaminophenyl)aminoanilinofluoran; 2,4-dimethyl-6-〔(4-dimethylamino)anilino〕-fluoran. ;

[0043] <Fluorene-based leuco dyes>

[0044] 3,6,6'-Tris(dimethylamino)spiro[fluorene-9,3'-phthalide]; 3,6,6'-Tris(diethylamino)spiro[fluorene-9,3'-phthalide].

[0045] <Divinyl Leuco Dye>

[0046] 3,3-Bis-〔2-(p-dimethylaminophenyl)-2-(p-methoxyphenyl)vinyl〕-4,5,6,7-tetrabromophthalide; 3,3-Bis-〔2-(p-dimethylaminophenyl)-2-(p-methoxyphenyl)vinyl〕-4,5,6,7-tetrachlorophthalide; 3,3-Bis-〔1,1-bis(4-pyrrolidinylphenyl)vinyl-2-yl〕-4,5,6,7-tetrabromophthalide; 3,3-Bis-〔1-(4-methoxyphenyl)-1-(4-pyrrolidinylphenyl)vinyl-2-yl〕-4,5,6,7-tetrachlorophthalide.

[0047] <Others>

[0048] 3-(4-diethylamino-2-ethoxyphenyl)-3-(1-ethyl-2-methylindol-3-yl)-4-azaphthalide; 3-(4-diethylamino-2-ethoxyphenyl)-3-(1-octyl-2-methylindol-3-yl)-4-azaphthalide; 3-(4-cyclohexylethylamino-2-methoxyphenyl)-3-(1-ethyl-2-methylindol-3-yl)-4-azaphthalide; 3,3-bis(1-ethyl-2-methylindol-3-yl)phthalide; 3,6-bis(diethylamino)fluoran-γ-(3'-nitro)aniline lactam; 3,6-bis( 1,1-bis-[2',2',2",2"-tetrakis-(p-dimethylaminophenyl)-vinyl]-2,2-dicyanoethane; 1,1-bis-[2',2',2",2"-tetrakis-(p-dimethylaminophenyl)-vinyl]-2-β-naphthoylethane; 1,1-bis-[2',2',2",2"-tetrakis-(p-dimethylaminophenyl)-vinyl]-2,2-diacetylethane; bis-[2,2,2',2'-tetrakis-(p-dimethylaminophenyl)-vinyl]-methylmalonic acid dimethyl ester.

[0049] As the developer that can be used in the thermosensitive recording medium of the present invention, there can be used any known substance in the field of existing pressure-sensitive or thermosensitive recording paper, and there is no particular limitation thereto. Examples thereof include activated clay, attapulgite, colloidal silica, inorganic acidic substances such as aluminum silicate, 4,4'-isopropylidene diphenol, 1,1-bis(4-hydroxyphenyl)cyclohexane, 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 4,4'-dihydroxydiphenyl sulfide, hydroquinone monobenzyl ether, 4-hydroxybenzoic acid benzyl ester, 4,4'-dihydroxydiphenyl sulfone, 2,4'-dihydroxydiphenyl sulfone, 4-hydroxy-4'-isopropoxydiphenyl sulfone, 4-hydroxy-4'-n-propoxydiphenyl sulfone, and the like. sulfone, di(3-allyl-4-hydroxyphenyl)sulfone, 4-hydroxy-4'-methyldiphenylsulfone, 4-hydroxyphenyl-4'-benzyloxyphenylsulfone, 3,4-dihydroxyphenyl-4'-methylphenylsulfone, 1-[4-(4-hydroxyphenylsulfonyl)phenoxy]-4-[4-(4-isopropoxyphenylsulfonyl)phenoxy]butane, the phenol polycondensation composition described in Japanese Unexamined Patent Publication No. 2003-154760, the aminobenzenesulfonamide derivative described in Japanese Unexamined Patent Publication No. 8-59603, di(4-hydroxyphenylthioethoxy)methane, 1,5-di(4-hydroxyphenylthio)-3-oxapentane, di(p-hydroxyphenyl)butyl acetate, di(p-hydroxyphenyl)acetate, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 1,4-bis[α-methyl-α-(4'-hydroxyphenyl)ethyl]benzene, 1,3-bis[α-methyl-α-(4'-hydroxyphenyl)ethyl]benzene, bis(4-hydroxy-3-methylphenyl)sulfide, 2,2'-thiobis(3-tert-octylphenol), 2,2'-thiobis(4-tert-octylphenol), N-[2-(3-phenylureido)phenyl]benzenesulfonamide, N,N'-bis-[3-(p-toluenesulfonyloxy)phenyl]urea, phenolic compounds such as the diphenylsulfone crosslinking compound described in WO97 / 16420, WO02 / 081229 or Japanese Patent Application Laid-Open No. 2002 Compounds described in Gazette No. 002-301873, thiourea compounds such as N,N'-di-m-chlorophenylthiourea, p-chlorobenzoic acid, stearyl gallate, di[4-(n-octyloxycarbonylamino)salicylic acid zinc] dihydrate, 4-[2-(p-methoxyphenoxy)ethoxy]salicylic acid, 4-[3-(p-tolylsulfonyl)propoxy]salicylic acid, 5-[p-(2-p-methoxyphenoxyethoxy)cumyl]salicylic acid, and salts of these aromatic carboxylic acids with polyvalent metal salts such as zinc, magnesium, aluminum, calcium, titanium, manganese, tin, and nickel, antipyrine complexes of zinc thiocyanate, and composite zinc salts of p-formylbenzoic acid and other aromatic carboxylic acids. These color developers can be used alone or in combination of two or more.1-[4-(4-hydroxyphenylsulfonyl)phenoxy]-4-[4-(4-isopropoxyphenylsulfonyl)phenoxy]butane can be obtained, for example, as a product name of TOMILA C214 manufactured by Mitsubishi Chemical Corporation, the phenol polycondensation composition described in Japanese Patent Application Publication No. 2003-154760 can be obtained, for example, as a product name of TOMILA C224 manufactured by Mitsubishi Chemical Corporation, and the diphenyl sulfone cross-linked compound described in International Publication No. WO97 / 16420 can be obtained as a product name of D-90 manufactured by Nippon Soda Co., Ltd. In addition, the compounds described in WO02 / 081229 and the like can be obtained as a product name of NKK-395 and D-100 manufactured by Nippon Soda Co., Ltd.

[0050] As the sensitizer that can be used in the thermosensitive recording medium of the present invention, a conventionally known sensitizer can be used. Examples of the sensitizer include fatty acid amides such as stearic acid amide and palmitic acid amide, ethylenebisamide, montanic acid wax, polyethylene wax, 1,2-di-(3-methylphenoxy)ethane, p-benzylbiphenyl, β-benzyloxynaphthalene, 4-biphenyl-p-tolyl ether, m-terphenyl, 1,2-diphenoxyethane, dibenzyl oxalate, di(p-chlorobenzyl)oxalate, di(p-methylbenzyl)oxalate, dibenzyl terephthalate, benzyl p-benzyloxybenzoate, carbonyl terephthalate, and the like. The sensitizer may be di-p-tolyl ester, phenyl-α-naphthyl carbonate, 1,4-diethoxynaphthalene, 1-hydroxy-2-phenyl naphthoate, o-xylene bis(phenyl ether), 4-(m-methylphenoxymethyl)biphenyl, 4,4'-ethylenedioxybisbenzoic acid dibenzyl ester, dibenzoyloxymethane, 1,2-bis(3-methylphenoxy)ethylene, di[2-(4-methoxy-phenoxy)ethyl]ether, methyl p-nitrobenzoate, phenyl p-toluenesulfonate, etc., but no particular limitation is made to this. These sensitizers may be used alone or in combination of two or more.

[0051] Examples of the binder that can be used in the present invention include fully saponified polyvinyl alcohol, partially saponified polyvinyl alcohol, carboxyl-modified polyvinyl alcohol, diacetone-modified polyvinyl alcohol, acetoacetyl-modified polyvinyl alcohol, amide-modified polyvinyl alcohol, sulfonic acid-modified polyvinyl alcohol, butyral-modified polyvinyl alcohol, olefin-modified polyvinyl alcohol, nitrile-modified polyvinyl alcohol, pyrrolidone-modified polyvinyl alcohol, silanol-modified polyvinyl alcohol, cation-modified polyvinyl alcohol, terminal alkyl-modified polyvinyl alcohol and the like polyvinyl alcohols, cellulose ethers such as hydroxyethyl cellulose, methyl cellulose, ethyl cellulose, carboxymethyl cellulose, acetyl cellulose and the like and derivatives thereof, starch, enzyme-modified starch, thermochemically modified starch, oxidized starch, esterified starch, etherified starch (e.g., hydroxyethylated starch, etc.), cationized starch and the like, polyacrylamide, cationic Polyacrylamides such as polyacrylamide, anionic polyacrylamide, and amphoteric polyacrylamide, urethane resins such as polyester polyurethane resins, polyether polyurethane resins, and polyurethane ionomer resins, acrylic resins containing (meth) acrylic acid and monomer components (excluding olefins) copolymerizable with (meth) acrylic acid, styrene-butadiene copolymers, styrene-butadiene-acrylonitrile copolymers, styrene-butadiene-acrylic copolymers, and other styrene-butadiene resins, polyvinyl acetate, vinyl chloride-vinyl acetate copolymers, ethylene-vinyl acetate copolymers and other polyolefin resins, polyvinyl chloride, polyvinylidene chloride, polyacrylates, gum arabic, polyvinyl butyral, polystyrene and copolymers thereof, silicone resins, petroleum resins, terpene resins, ketone resins, coumarone resins, etc. These may be used alone or in combination of two or more.

[0052] Examples of the pigment that can be used in the present invention include inorganic or organic fillers such as silicon dioxide, calcium carbonate, kaolin, calcined kaolin, diatomaceous earth, talc, titanium oxide, and aluminum hydroxide, etc. These can be used alone or in combination of two or more.

[0053] Examples of the crosslinking agent that can be used in the present invention include glyoxal, methylolmelamine, melamine formaldehyde resin, melamine urea resin, polyamine epichlorohydrin resin, polyamide epichlorohydrin resin, potassium persulfate, ammonium persulfate, sodium persulfate, ferric chloride, magnesium chloride, borax, boric acid, alum, and ammonium chloride.

[0054] Furthermore, in the present invention, as image stabilizers showing an oil resistance effect on recorded images, the following may be used, within the range not impairing the desired effect on the above-mentioned subject: 4,4'-butylene (6-tert-butyl-3-methylphenol), 2,2'-di-tert-butyl-5,5'-dimethyl-4,4'-sulfonyl diphenol, 1,1,3-tris(2-methyl-4-hydroxy-5-cyclohexylphenyl)butane, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 4-benzyloxy-4'-(2,3-epoxy-2-methylpropyloxy)diphenyl sulfone, etc.

[0055] In addition, benzophenone-based or triazole-based ultraviolet absorbers, lubricants, dispersants, defoaming agents, antioxidants, fluorescent dyes, and the like may be used.

[0056] The types and amounts of the electron donating leuco dye, electron accepting developer, and other various components used in the thermosensitive recording medium of the present invention are determined according to the required performance and recording suitability. Although not particularly limited, usually 0.5 to 10 parts by weight of the electron accepting developer and 0.5 to 10 parts by weight of the sensitizer are used per 1 part by weight of the electron donating leuco dye.

[0057] The types and amounts of binders, pigments, crosslinking agents, image stabilizers, and other components as other optional components are determined according to the required performance and recording adaptability. Although not particularly limited, generally, the binder is preferably about 5 to 50 parts by weight in terms of solid content relative to 100 parts by weight of the thermal recording layer (solid content), and the pigment is preferably about 0 to 50 parts by weight in terms of solid content relative to 100 parts by weight of the thermal recording layer (solid content). When a lubricant is used, the lubricant content is preferably about 5 to 10 parts by weight in terms of solid content relative to 100 parts by weight of the thermal recording layer (solid content).

[0058] In the thermosensitive recording medium of the present invention, a protective layer may be further provided on the thermosensitive recording layer. The protective layer is often composed mainly of a pigment and a resin, and the materials that can be used in the thermosensitive recording layer include the binders, pigments, crosslinking agents, etc. exemplified above.

[0059] As the binder, any of the binders that can be used in the above-mentioned thermosensitive recording layer can be used appropriately, but carboxyl-modified polyvinyl alcohol and non-core-shell acrylic resin are preferred. These binders can be used alone or in combination of two or more.

[0060] As the crosslinking agent, any crosslinking agent that can be used in the above-mentioned thermosensitive recording layer can be used as appropriate, and epichlorohydrin-based resins and polyamine / polyamide-based resins (except those contained in the epichlorohydrin-based resin) are preferred.

[0061] More preferably, the protective layer contains an epichlorohydrin-based resin and a polyamine / polyamide-based resin in addition to the carboxyl-modified polyvinyl alcohol, whereby the color development performance is further improved.

[0062] The carboxyl-modified polyvinyl alcohol can be obtained, for example, as the following substances: reaction products of polyvinyl alcohol and polycarboxylic acids such as fumaric acid, phthalic anhydride, mellitic anhydride, itaconic anhydride, or esters of their reaction products; and saponified copolymers of vinyl acetate and ethylenically unsaturated dicarboxylic acids such as maleic acid, fumaric acid, itaconic acid, crotonic acid, acrylic acid, and methacrylic acid. As a specific production method, for example, the method exemplified in Japanese Patent Publication No. 53-91995 can be cited. In addition, the saponification degree of the carboxyl-modified polyvinyl alcohol is preferably 72 to 100 mol%, and the degree of polymerization is 500 to 2400, and more preferably 1000 to 2000.

[0063] The glass transition temperature (Tg) of the non-core-shell acrylic resin is preferably 95° C. or lower, and more preferably higher than 50° C. The Tg is measured by differential scanning calorimetry (DSC).

[0064] The non-core-shell acrylic resin preferably contains (meth)acrylic acid and a monomer component copolymerizable with (meth)acrylic acid, and (meth)acrylic acid is 1 to 10 parts by weight in 100 parts by weight of the non-core-shell acrylic resin. (Meth)acrylic acid is alkali-soluble and has the property of converting the non-core-shell acrylic resin into a water-soluble resin by adding a neutralizing agent. By converting the non-core-shell acrylic resin into a water-soluble resin, especially when the protective layer contains a pigment, the binding property with the pigment is significantly improved, so that even when a large amount of pigment is contained, a protective layer with excellent strength can be formed. As components that can be copolymerized with (meth)acrylic acid, for example, alkyl acrylate resins such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and octyl (meth)acrylate, and modified alkyl acrylate resins such as the above-mentioned alkyl acrylate resins modified by epoxy resins, silicone resins, styrene or derivatives thereof, (meth)acrylonitrile, acrylic acid esters, and hydroxyalkyl acrylates can be exemplified. (meth)acrylonitrile is preferably added in an amount of 15 to 70 parts per 100 parts of non-core-shell acrylic resins. In addition, methyl methacrylate is preferably added in an amount of 20 to 80 parts per 100 parts of non-core-shell acrylic resins. When (meth)acrylonitrile and methyl methacrylate are contained, it is preferred that (meth)acrylonitrile accounts for 15 to 18 parts of 100 parts of the non-core-shell acrylic resin and methyl methacrylate accounts for 20 to 80 parts of 100 parts of the non-core-shell acrylic resin.

[0065] The epichlorohydrin resin is a resin characterized by containing epoxy groups in the molecule, for example, polyamide epichlorohydrin resin, polyamine epichlorohydrin resin, etc. can be cited, which can be used alone or in combination. In addition, as the amine present in the main chain of the epichlorohydrin resin, substances from primary amine to quaternary ammonium can be used, and no special restrictions are made to this. In addition, from the aspect of good water resistance, the cationization degree and molecular weight are preferably: cationization degree 5meq / g·Solid or less (measured value under pH7 conditions), molecular weight 500,000 or more. As specific examples of epichlorohydrin resins, Sumirez Resin 650 (30), Sumirez Resin 675A, Sumirez Resin 6615 (more than by Sumitomo Chemical Co., Ltd.), WS4002, WS4020, WS4024, WS4030, WS4046, WS4010, CP8970 (more than by Starlight PMC Co., Ltd.) and the like.

[0066] The polyamine / polyamide resin does not have an epoxy group in the molecule, and examples thereof include polyamide urea resin, polyalkylene polyamine resin, polyalkylene polyamide resin, polyamine polyurea resin, modified polyamine resin, modified polyamide resin, polyalkylene polyamine urea-formaldehyde resin, polyalkylene polyamine polyamide polyurea resin, etc., which can be used alone or in combination. Specific examples of the polyamine / polyamide resin include Sumirez Resin 302 (manufactured by Sumitomo Chemical Co., Ltd.: polyamine polyurea resin), Sumirez Resin 712 (manufactured by Sumitomo Chemical Co., Ltd.: polyamine polyurea resin), Sumirez Resin 703 (manufactured by Sumitomo Chemical Co., Ltd.: polyamine polyurea resin), Sumirez Resin 636 (manufactured by Sumitomo Chemical Co., Ltd.: polyamine polyurea resin), Sumirez Resin SPI-100 (manufactured by Sumitomo Chemical Co., Ltd.: modified polyamine resin), Sumirez Resin SPI-102A (manufactured by Sumitomo Chemical Co., Ltd.: modified polyamine resin), Sumirez Resin SPI-106N (manufactured by Sumitomo Chemical Co., Ltd.: modified polyamide resin), Sumirez Resin SPI-203 (50) (manufactured by Sumitomo Chemical Co., Ltd.), Sumirez Resin SPI-206 ... SPI-198 (manufactured by Sumitomo Chemical Co., Ltd.), primtive A-700, primtive A-600 (manufactured by Asahi Chemical Co., Ltd.), PA6500, PA6504, PA6634, PA6638, PA6640, PA6644, PA6646, PA6654, PA6702, PA6704 (manufactured by Starlight PMC Co., Ltd.: polyalkylene polyamine polyamide polyurea resin), CP8994 (manufactured by Starlight PMC Co., Ltd.: polyethyleneimine resin), etc. Although not particularly limited, it is preferred to use polyamine resins (polyalkylene polyamine resins, polyamine polyurea resins, modified polyamine resins, polyalkylene polyamine urea-formaldehyde resins, polyalkylene polyamine polyamide polyurea resins) from the perspective of good printing concentration.

[0067] In the protective layer, when epichlorohydrin-based resin and polyamine / polyamide-based resin are used together with carboxyl-modified polyvinyl alcohol, the content thereof is preferably 1 to 100 parts by weight, more preferably 5 to 50 parts by weight, and further preferably 10 to 40 parts by weight, respectively, relative to 100 parts by weight of carboxyl-modified polyvinyl alcohol.

[0068] As the pigment used in the protective layer, the pigments that can be used in the above-mentioned thermosensitive recording layer can be appropriately used, and kaolin, calcined kaolin, aluminum hydroxide, and silica are preferred. These pigments can be used alone or in combination of two or more.

[0069] The content (solid content) of the binder in the protective layer is preferably 20% by weight or more, more preferably about 20 to 80% by weight. When the protective layer contains a pigment, the content of the pigment and the binder is preferably: relative to 100 parts by weight of the pigment, the binder is about 30 to 300 parts by weight in terms of solid content.

[0070] The coating liquid for the protective layer may contain, as required, various auxiliary agents such as a crosslinking agent, a lubricant, a stabilizer, an ultraviolet absorber, a dispersant, a defoaming agent, an antioxidant, and a fluorescent dye, which can be used in the above-mentioned thermosensitive recording layer.

[0071] In addition, an undercoat layer may be provided between the support and the heat-sensitive recording layer. The undercoat layer mainly contains a binder and a pigment.

[0072] As the binder used in the undercoat layer, various binders used in the above-mentioned thermosensitive recording layer can be used. These binders can be used alone or in combination of two or more.

[0073] As the pigment used in the undercoat layer, various pigments used in the above-mentioned thermosensitive recording layer can be used. These pigments can be used alone or in combination of two or more.

[0074] The amount of the pigment in the primer layer is usually 50 to 95 parts by weight, preferably 70 to 90 parts by weight, based on 100 parts by weight of the total solid content of the primer layer.

[0075] The primer layer may contain various auxiliary agents such as a dispersant, a plasticizer, a pH adjuster, a defoamer, a water-retaining agent, a preservative, a coloring dye, and an ultraviolet light inhibitor as needed.

[0076] By applying the coating solution containing the composition coordinated by the above-mentioned coating layer purposes to any support such as paper, recycled paper, synthetic paper, film, plastic film, foamed plastic film, nonwoven fabric, etc., the target thermosensitive recording medium can be obtained. In addition, the composite sheet formed by these combinations can also be used as a support.

[0077] The electron donating leuco dye, electron accepting developer, electron acceptor, electron donor and materials added as needed are micronized to a particle size of less than several microns by a pulverizer such as a ball mill, an attritor, a sand mill or an appropriate emulsifying device, and various additives are added according to the purpose to prepare a coating liquid.

[0078] There is no particular restriction on the means of applying the above-mentioned coating layers, and the coating can be carried out according to the commonly known techniques. For example, it is possible to appropriately select and use: an off-machine coater or an on-machine coater equipped with various coaters such as an air knife coater, a rod blade coater, an exhaust blade coater, a bevel blade coater, a roller coater, a curtain coater, and a spray coater. The coating amount of the thermal recording layer is determined according to the required performance and recording adaptability, and is not particularly limited, but the general coating amount is 2 to 12 g / m in terms of solid content. 2 about.

[0079] Furthermore, each coating layer may be appropriately subjected to various well-known techniques in the field of thermosensitive recording materials after coating, such as smoothing treatment such as super calendering.

[0080] Example

[0081] Hereinafter, although the present invention is illustrated by examples, it is not intended to limit the present invention. It should be noted that in each example and comparative example, "part" represents "part by weight" and "%" represents "% by weight" unless otherwise specified.

[0082] [Preparation of each coating liquid]

[0083] The mixture having the following composition ratio was stirred and dispersed to prepare a coating liquid for an undercoat layer.

[0084] <Coating liquid for primer layer>

[0085] Calcined kaolin (Alfateccs HP, manufactured by Imerys) 50 parts

[0086] Plastic hollow particles (MH8109 manufactured by ZEON) 50 parts

[0087] Styrene / butadiene copolymer latex (ST5526, manufactured by ZEON Corporation, Japan, solid content 48%) 10 parts

[0088] 50 parts water

[0089] Next, the formulations having the following ratios were mixed to prepare back coat layer coating solutions 1 to 6.

[0090] <Back Coating Liquid 1>

[0091] Kaolin (manufactured by Imerys, trade name: Contour 1500) 20 parts

[0092] Ethylene-vinyl alcohol copolymer (manufactured by KURARAY CO., LTD., trade name: Exceval RS4104) 10 parts

[0093] Ethylene-acrylic acid copolymer (manufactured by Sumitomo Seika Chemicals Co., Ltd., trade name: ZAIKTHENE AC, melting point: 80-95°C) 40 parts

[0094] <Back Coating Liquid 2>

[0095] Kaolin (Imerys, trade name: Contour 1500) 20 parts

[0096] Ethylene-vinyl alcohol copolymer (RS4104) 10 parts

[0097] Ethylene-acrylic acid copolymer (ZAIKTHENE AC) 20 parts

[0098] Styrene-butadiene copolymer latex (ST5526) 20 parts

[0099] <Back coat coating liquid 3>

[0100] Kaolin (contour 1500) 20 parts

[0101] Ethylene-acrylic acid copolymer (ZAIKTHENE AC) 50 parts

[0102] <Back coating layer coating liquid 4>

[0103] Kaolin (contour 1500) 20 parts

[0104] Ethylene-vinyl alcohol copolymer (RS4104) 50 parts

[0105] <Back Coating Liquid 5>

[0106] Kaolin (contour 1500) 20 parts

[0107] 10 parts of fully saponified polyvinyl alcohol aqueous solution (PVA117)

[0108] Ethylene-acrylic acid copolymer (ZAIKTHENE AC) 40 parts

[0109] <Back Coating Liquid 6>

[0110] Kaolin (contour 1500) 20 parts

[0111] Ethylene-vinyl alcohol copolymer (RS4104) 10 parts

[0112] Styrene-butadiene copolymer latex (ST5526) 40 parts

[0113] The developer dispersion, leuco dye dispersion and sensitizer dispersion of the following proportions were wet-milled using a sand mill until the average particle size reached 0.5 μm.

[0114] Color developer dispersion (A1 solution)

[0115] N-[2-(3-phenylureido)phenyl]benzenesulfonamide

[0116] (Nippon Soda Co., Ltd., NKK1304, hereinafter referred to as "urea compound") 6.0 parts

[0117] 5.0 parts of a completely saponified polyvinyl alcohol aqueous solution (PVA117 manufactured by KURARAY, Inc., solid content 10%)

[0118] 1.5 parts water

[0119] Color developer dispersion (A2 solution)

[0120] 4-Benzyloxy-4'-hydroxydiphenyl sulfone (BPS-MA3 manufactured by Nikka Chemical Co., Ltd.) 6.0 parts

[0121] 5.0 parts of fully saponified polyvinyl alcohol aqueous solution (PVA117)

[0122] 1.5 parts water

[0123] Leuco dye dispersion (liquid B)

[0124] 3-Dibutylamino-6-methyl-7-anilinofluoran (ODB-2 manufactured by Yamamoto Chemicals Co., Ltd.) 6.0 parts

[0125] 5.0 parts of fully saponified polyvinyl alcohol aqueous solution (PVA117)

[0126] 1.5 parts water

[0127] Sensitizer dispersion (liquid C)

[0128] 1,2-Di-(3-methylphenoxy)ethane (manufactured by Sanko Co., Ltd., KS232) 6.0 parts

[0129] 5.0 parts of fully saponified polyvinyl alcohol aqueous solution (PVA117)

[0130] 1.5 parts water

[0131] Next, the respective dispersions were mixed at the following ratio to prepare a coating liquid for a thermosensitive recording layer.

[0132] <Thermosensitive recording layer coating liquid 1>

[0133] 18.0 parts of developer dispersion (A1 solution)

[0134] 18.0 parts of leuco dye dispersion (liquid B)

[0135] Sensitizer dispersion (liquid C) 36.0 parts

[0136] Silica dispersion (Mizusawa Chemical Co., Ltd., MIZUKASIL P-537, solid content 25%) 17.5 parts

[0137] 30.0 parts of fully saponified polyvinyl alcohol aqueous solution (PVA117)

[0138] <Thermosensitive recording layer coating liquid 2>

[0139] 18.0 parts of developer dispersion (A2 solution)

[0140] 18.0 parts of leuco dye dispersion (liquid B)

[0141] Sensitizer dispersion (liquid C) 36.0 parts

[0142] Silica dispersion (MIZUKASIL P-537) 17.5 parts

[0143] 30.0 parts of fully saponified polyvinyl alcohol aqueous solution (PVA117)

[0144] Next, a compound having the following ratio was mixed to prepare a protective layer coating liquid.

[0145] <Coating liquid for protective layer>

[0146] 9.0 parts of aluminum hydroxide dispersion (manufactured by Martinswerk, trade name: Martifin OL, solid content 50%)

[0147] 30.0 parts of carboxyl-modified polyvinyl alcohol aqueous solution (KURARAY Co., Ltd., trade name: KL318, degree of polymerization: about 1700, degree of saponification: 95-99 mol%, solid content 10%)

[0148] 4.0 parts of polyamide epichlorohydrin resin (manufactured by Seikyo PMC Co., Ltd., trade name: WS4030, solid content 25%)

[0149] Modified polyamine resin (manufactured by Sumitomo Chemical Co., Ltd., trade name: Sumirez Resin SPI-102A, solid content 45%) 2.2 parts

[0150] Zinc stearate (manufactured by Chukyo Oil & Fats Co., Ltd., trade name: HYDRIN Z-7-30, solid content 30%) 2.0 parts

[0151] 22.8 parts water

[0152] [Example 1]

[0153] On the support body (basic weight 60g / m 2 The coating amount is 6.0 g / m2 on one side of high-quality paper. 2 The primer coating liquid is applied by an exhaust blade method and then dried to obtain primer-coated paper.

[0154] The coating amount on the primer layer of the primer-coated paper was 3.0 g / m 2 The heat-sensitive recording layer coating liquid 1 is applied by a bar doctor blade method, dried, and processed by a super calender until the smoothness reaches 500 to 1000 seconds, thereby producing a heat-sensitive recording layer coated paper.

[0155] Next, on the heat-sensitive recording layer of the heat-sensitive recording layer coated paper, a coating amount of 3.0 g / m 2 The protective layer coating liquid is applied by a bar doctor blade method and then dried to produce protective layer coated paper.

[0156] Next, the protective layer was coated on the side of the paper opposite to the protective layer at a coating amount of 3.5 g / m 2 The back coating layer coating liquid 1 was applied by a bar blade method and then dried to produce a thermosensitive recording material.

[0157] [Example 2]

[0158] In addition to setting the coating amount of the back coating liquid to 2.0 g / m 2 A thermosensitive recording material was prepared in the same manner as in Example 1 except for the above.

[0159] [Example 3]

[0160] In addition to setting the coating amount of the back coating liquid to 2.5 g / m 2 A thermosensitive recording material was prepared in the same manner as in Example 1 except for the above.

[0161] [Example 4]

[0162] In addition to setting the coating amount of the back coating liquid to 4.5 g / m 2 A thermosensitive recording material was prepared in the same manner as in Example 1 except for the above.

[0163] [Example 5]

[0164] A thermosensitive recording material was prepared in the same manner as in Example 1 except that the back coat layer coating liquid was used in an amount of 30 parts of ethylene-vinyl alcohol copolymer and 20 parts of ethylene-acrylic acid copolymer.

[0165] [Example 6]

[0166] A thermosensitive recording material was prepared in the same manner as in Example 1 except that the coating liquid for the back coat layer was changed to 40 parts of ethylene-vinyl alcohol copolymer and 10 parts of ethylene-acrylic acid copolymer.

[0167] [Example 7]

[0168] A thermosensitive recording material was prepared in the same manner as in Example 1 except that the thermosensitive recording layer coating solution 2 was used instead of the thermosensitive recording layer coating solution 1.

[0169] [Example 8]

[0170] A thermosensitive recording material was prepared in the same manner as in Example 1 except that the back coat layer coating liquid 2 was used instead of the back coat layer coating liquid 1.

[0171] [Comparative Example 1]

[0172] A thermosensitive recording material was prepared in the same manner as in Example 1 except that the back coat layer coating liquid 3 was used instead of the back coat layer coating liquid 1.

[0173] [Comparative Example 2]

[0174] A thermosensitive recording material was prepared in the same manner as in Example 1 except that the back coat layer coating liquid 4 was used instead of the back coat layer coating liquid 1.

[0175] [Comparative Example 3]

[0176] A thermosensitive recording material was prepared in the same manner as in Example 1 except that the back coat layer coating liquid 5 was used instead of the back coat layer coating liquid 1.

[0177] [Comparative Example 4]

[0178] A thermosensitive recording material was prepared in the same manner as in Example 1 except that the back coat layer coating liquid 6 was used instead of the back coat layer coating liquid 1.

[0179] [Comparative Example 5]

[0180] A thermosensitive recording material was prepared in the same manner as in Example 1 except that the back coat layer coating liquid was not applied.

[0181] The produced thermosensitive recording material was evaluated as follows.

[0182] <Color rendering performance (printing density)>

[0183] The produced thermosensitive recording medium was printed with a checkered pattern at an applied energy of 0.35 mJ / dot and a printing speed of 50 mm / sec using TH-PMD (thermal recording paper printing tester, equipped with a thermal head manufactured by Kyocera Corporation) manufactured by Okura Electric Co., Ltd. The print density of the printed portion was measured with a Macbeth densitometer (RD-914, using an amber color filter) to evaluate the color development performance.

[0184] <Moisture-proof performance on the back>

[0185] The performance of the produced thermosensitive recording material was evaluated under the following two conditions.

[0186] (1) 23°C × 50% RH × 24 hours of storage → Printing at 23°C × 50% RH

[0187] (2) 35°C × 80% RH × 24 hours storage → printing at 23°C × 50% RH

[0188] That is, after printing a full-surface pattern on one roll (20 m) using UP-X898MD (thermal printer for medical use) manufactured by Sony under S mode conditions, visually observe whether water droplets are attached to the ink sac (damper) portion of the printer on the opposite side of the thermal head, and evaluate the moisture resistance based on the following criteria.

[0189] ○: No water droplets attached

[0190] △: Water droplets are attached but disappear immediately

[0191] ×: Water droplets are attached and do not disappear for several minutes

[0192] ××: Water droplets are attached and do not disappear for several hours

[0193] <Wrapping Adhesion>

[0194] The produced thermosensitive recording material was processed into a small roll (110 mm×20 m), left to stand for 24 hours under environmental conditions of 35° C.×80% RH, and then visually evaluated according to the following criteria.

[0195] ○: No blocking occurred, no peeling of the protective layer and back coating

[0196] ×: Blocking occurs, and the protective layer and / or back coating peels off

[0197] The results are shown in Table 1.

[0198]

Table 1

[0199]

[0200] As shown in Table 1, the thermosensitive recording material of the present invention has the effect of preventing water droplets from adhering to the back surface without adversely affecting the color development sensitivity and having excellent water vapor barrier properties.

Claims

1. A thermosensitive recording medium, comprising: a thermosensitive recording layer containing a colorless or light-colored electron-donating leuco dye and an electron-accepting developer, and a back coating layer on the side opposite to the thermosensitive recording layer, The back coating layer contains ethylene-vinyl alcohol copolymer and ethylene-acrylic acid copolymer.

2. The thermosensitive recording medium according to claim 1, wherein The content ratio of the ethylene-acrylic acid-based copolymer to the solid content of the ethylene-vinyl alcohol copolymer is 2.5 parts to 40 parts based on 10 parts by mass of the ethylene-vinyl alcohol copolymer.

3. The thermosensitive recording medium according to claim 1 or 2, wherein The total content of the ethylene-vinyl alcohol copolymer and the ethylene-acrylic acid copolymer in the back coat layer is 50% to 90% by weight as a solid content.

4. The thermosensitive recording material according to any one of claims 1 to 3, wherein The coating amount of the back coating is 2.5g / m 2 ~4.5g / m 2 .

Citation Information

Patent Citations

  • Heat-sensitive recording body

    CN101687424A

  • Recording material

    JP1997265149A

  • Thermosensitive recording body and thermosensitive recording body label

    JP2007245362A

  • Thermal transfer receiving sheet

    US20060194003A1

  • Heat-sensitive recording material

    US20060205593A1