Anisotropic light-diffusing adhesive layer and display device having anisotropic light-diffusing adhesive layer

By using an anisotropic light diffusion adhesive layer composed of acrylic copolymer and needle filler in a liquid crystal display device, the content of carboxylic monomer and the orientation of needle filler are controlled, and the optical characteristics and moisture and heat resistance in the prior art are solved. The problem of insufficient results has improved the field of view and humidity resistance.

CN118974191APending Publication Date: 2024-11-15TOMOEGAWA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380031375.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing anisotropic light diffusion adhesive layer is difficult to take into account high optical characteristics and humidity resistance in liquid crystal display devices, especially in diversified applications and humidity and heat environments.

Method used

The anisotropic light diffusion adhesive layer consisting of an acrylic copolymer and a needle-shaped filler oriented in one direction is controlled to control the content of carboxylic monomers below 1%, the needle-shaped filler content is 1-50 parts by mass, and the orientation degree is The haze value difference was 2% or less, and the humidity resistance test was passed at 85°C and 85% relative humidity for 168 hours.

Benefits of technology

Excellent performance in optical characteristics and field angle characteristics are achieved, and good humidity resistance is maintained in humid and heat environments, which extends the service life of the light diffusion adhesive layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974191A_ABST
    Figure CN118974191A_ABST
Patent Text Reader

Abstract

Provided is an anisotropic light-diffusing adhesive layer having excellent wet heat resistance. An anisotropic light-diffusing adhesive layer according to one embodiment of the present invention comprises: an adhesive comprising an acrylic copolymer; and a needle-like filler which is oriented and dispersed in one direction. Among all the monomers constituting the acrylic copolymer, the ratio of the monomer having a carboxyl group is 1% or less, the content of the needle-like filler is 1-50 parts by mass when the total solid content of the anisotropic light-diffusing adhesive layer is 100 parts by mass, and the orientation degree of the anisotropic light-diffusing adhesive layer is 10 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an anisotropic light-diffusing adhesive layer and a display device having the anisotropic light-diffusing adhesive layer. Background Art

[0002] In recent years, as a light diffuser used in a liquid crystal display device, an anisotropic light diffuser that diffuses transmitted light in a predetermined direction rather than isotropically has been proposed.

[0003] For example, Patent Document 1 discloses an anisotropic light-diffusing adhesive laminate, which includes at least one adhesive layer in which needle-shaped fillers are dispersed in an adhesive in an approximately uniform orientation, and the adhesive layer is two or more layers. According to such an anisotropic light-diffusing adhesive laminate, when linear light is vertically incident on the anisotropic light-diffusing adhesive laminate, the projection image of the transmitted light becomes an elliptical shape extending in a direction orthogonal to the long axis direction of the needle-shaped fillers.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2004-258105 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] The above-mentioned anisotropic light-diffusing adhesive laminate is a useful technology because it can achieve both anisotropic light-diffusing function and adhesive function.

[0009] However, as the applications of liquid crystal display devices have become more diverse, an anisotropic light diffusing element having further improved optical properties and moisture and heat resistance has been required.

[0010] Therefore, an object of the present invention is to provide an anisotropic light-diffusing pressure-sensitive adhesive layer having excellent viewing angle characteristics and moisture-heat resistance among optical characteristics.

[0011] Means used to solve problems

[0012] The inventors of the present invention have conducted intensive studies and have found that the above-mentioned problems can be solved by making the anisotropic light-diffusing pressure-sensitive adhesive layer have a predetermined composition, thereby completing the present invention.

[0013] One embodiment of the present invention is an anisotropic light-diffusing adhesive layer, characterized by comprising:

[0014] An adhesive composed of an acrylic copolymer, and

[0015] Needle-shaped fillers oriented and dispersed in one direction;

[0016] Among all the monomer components constituting the acrylic copolymer, the ratio of the monomer having a carboxyl group is 1% or less,

[0017] The content of the needle-shaped filler is 1 to 50 parts by mass, based on 100 parts by mass of the total solid content of the anisotropic light-diffusing adhesive layer.

[0018] The anisotropic light-diffusing adhesive layer has an orientation degree of 10 or more.

[0019] The anisotropic light-diffusing adhesive layer may have a difference in haze value before and after 168 hours in a moisture and heat resistance test in an atmosphere of 85° C. and 85% relative humidity (haze value before 168 hours minus haze value after 168 hours) of 2% or less.

[0020] The needle-shaped filler may include one or more components selected from carbonates, sulfates, and nitrates.

[0021] The needle-shaped filler may have a short diameter of 0.1 μm to 10 μm, a long diameter of 2 μm to 1000 μm, and an aspect ratio of 10 to 100.

[0022] The weight average molecular weight of the acrylic copolymer may be 200,000 to 1.8 million.

[0023] The anisotropic light-diffusing adhesive layer may have a thickness of 5 μm to 100 μm.

[0024] Another aspect of the present invention is a liquid crystal display device, characterized in that:

[0025] With upper polarizer,

[0026] The anisotropic light-diffusing adhesive layer according to any one of claims 1 to 6 is laminated on the visible side of the upper polarizing plate so that the angle difference between the orientation axis of the needle-shaped filler and the absorption axis of the upper polarizing plate is within ±5°.

[0027] Effects of the Invention

[0028] According to the present invention, it is possible to provide an anisotropic light-diffusing pressure-sensitive adhesive layer having excellent viewing angle characteristics and moisture-heat resistance among optical characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a graph showing the measurement results of the contrast ratios at the front and at 60° for Examples and Comparative Examples. DETAILED DESCRIPTION

[0030] Hereinafter, the anisotropic light-diffusing adhesive layer of the present invention will be described in detail, but the present invention is not limited thereto.

[0031] Furthermore, the present invention may be not only an anisotropic light-diffusing adhesive layer but also an adhesive coating for obtaining the anisotropic light-diffusing adhesive layer, a display device using the anisotropic light-diffusing adhesive layer, and a method for producing the same.

[0032] Furthermore, the present invention may be a laminate including an anisotropic light-diffusing pressure-sensitive adhesive layer and other predetermined layers (base material or other pressure-sensitive adhesive layers).

[0033] In the following description, "(meth)acrylic acid" means including both "acrylic acid" and "methacrylic acid".

[0034] <<<<Components of anisotropic light-diffusing adhesive layer>>>>

[0035] The anisotropic light-diffusing adhesive layer contains an acrylic copolymer and a needle-shaped filler. In addition, the anisotropic light-diffusing adhesive layer may contain other components such as known additives.

[0036] According to another way of expression, the anisotropic light-diffusing adhesive layer contains an adhesive composed of an acrylic copolymer (which may contain a known additive) and a needle-shaped filler (the needle-shaped filler is dispersed in the adhesive).

[0037] <<<Acrylic acid copolymer>>>

[0038] In the acrylic copolymer, the content of the monomer component having a carboxyl group (carboxyl group-containing monomer) is preferably small.

[0039] Carboxyl group-containing monomers are often used as monomer components of acrylic copolymers for the purpose of using carboxyl groups as reaction points, etc. However, when an anisotropic light-diffusing adhesive layer containing needle-shaped fillers is formed using an acrylic copolymer obtained by using carboxyl group-containing monomers as a main component, when the anisotropic light-diffusing adhesive layer is placed in a hot and humid environment, the carboxyl groups of the acrylic copolymer react (hydrolyze) with other components containing needle-shaped fillers, etc., and the diffusion property is deteriorated, making it difficult to obtain the target optical properties.

[0040] In other words, the inventors of the present invention have found that an anisotropic light-diffusing adhesive layer comprising an acrylic copolymer having a very low content of or no carboxyl-containing monomer in the monomer components and a needle-shaped filler can suppress a decrease in diffusibility.

[0041] From the above viewpoint, in the acrylic copolymer, the ratio (weight ratio) of the carboxyl group-containing monomer in all the components of the monomer is 1% or less, preferably 0.5% or less, more preferably 0.1% or less, and further preferably 0% (in all the components of the monomer, except for the inevitable components, the carboxyl group-containing monomer is not included). By constituting in this way, the carboxyl group contained in the acrylic copolymer can be reduced, and the above effect can be further improved.

[0042] <<Monomers not containing a carboxyl group>>

[0043] The monomer not containing a carboxyl group is not particularly limited and may be selected from among the materials used for the optical pressure-sensitive adhesive layer so that the performance (optical properties, strength, heat resistance, chemical resistance, viscosity) of the acrylic copolymer falls within a desired range.

[0044] Examples of the monomer not containing a carboxyl group include (meth)acrylic acid alkyl ester monomers, hydroxyl group-containing (meth)acrylic acid monomers, alicyclic structure-containing (meth)acrylic acid monomers, and (meth)acrylamide monomers.

[0045] Examples of the alkyl (meth)acrylate monomer include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isononyl (meth)acrylate, lauryl (meth)acrylate, and isostearyl (meth)acrylate.

[0046] Examples of the hydroxyl group-containing (meth)acrylic monomer include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl 2-(meth)acrylate, and 2-hydroxy-3-phenoxypropyl (meth)acrylate.

[0047] Examples of the alicyclic structure-containing (meth)acrylic monomer include isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, and dicyclopentanyl (meth)acrylate.

[0048] Examples of the (meth)acrylamide-based monomers include (meth)acrylamide, diethyl (meth)acrylamide, dimethyl (meth)acrylamide, and isopropyl (meth)acrylamide.

[0049] The monomer not containing a carboxyl group can be used alone or in combination of two or more.

[0050] <<Crosslinking agent>>

[0051] The acrylic copolymer can be crosslinked by a crosslinking agent. The crosslinking agent is not particularly limited as long as it does not impair the effect of the invention, and for example, an isocyanate crosslinking agent, an aziridine crosslinking agent, an epoxy crosslinking agent, a metal chelate crosslinking agent, etc. can be used. These can be used alone or in combination.

[0052] <<Physical properties / characteristics>>

[0053] <Weight average molecular weight>

[0054] The weight average molecular weight of the acrylic copolymer is preferably 200,000 to 1,800,000, more preferably 200,000 to 1,000,000, further preferably 300,000 to 900,000, and particularly preferably 400,000 to 800,000.

[0055] The weight average molecular weight can be measured using a known measurement method, for example, by a method in accordance with JIS K7252-1:2008 “Plastics - Method for determination of average molecular weight and molecular weight distribution of polymers by size exclusion chromatography”.

[0056] <Glass transition temperature>

[0057] The glass transition temperature (Tg) of the acrylic copolymer is preferably -50° C. to -0° C., more preferably -40° C. to -10° C. By limiting the Tg of the acrylic copolymer to such a range, the adhesive can have a higher hardness and the adhesiveness can be improved.

[0058] Tg can be measured using a known measurement method, and can be measured by, for example, a method in accordance with JIS K7121-1987 "Methods for measuring transition temperatures of plastics".

[0059] <<<Needle-shaped filler>>>

[0060] <<Material>>

[0061] The needle-shaped filler is not particularly limited as long as it is a needle-shaped (including fibrous) filler with a high aspect ratio. However, when the anisotropic light-diffusing adhesive layer is used in a liquid crystal display device, etc., the needle-shaped filler is preferably colorless or white to prevent coloration of transmitted light.

[0062] Preferably, the needle-shaped filler contains one or more components selected from carbonates, sulfates and nitrates. More specifically, the needle-shaped filler preferably contains one or more needle-shaped or fibrous substances such as basic magnesium sulfate, calcium sulfate, barium sulfate, and calcium carbonate. In order to exert the characteristics of the present invention, it is more preferable to contain calcium carbonate.

[0063] <<Shape>>

[0064] The minor diameter of the needle-shaped filler is preferably 0.1 μm to 10 μm, more preferably 0.3 μm to 5 μm, and even more preferably 0.5 μm to 1 μm.

[0065] The major diameter of the needle-shaped filler is preferably 2 μm to 1000 μm, more preferably 10 μm to 150 μm.

[0066] By limiting the short diameter and long diameter of the needle-shaped filler to such a range, the diffusion of light achieved by the needle-shaped filler in the anisotropic light-diffusing adhesive layer becomes optimal, for example, the viewing angle widening effect of the anisotropic light-diffusing adhesive layer can be improved. For example, when the needle-shaped filler as a whole is 100% by mass, preferably 90% by mass or more or 95% by mass or more of the needle-shaped filler has such a short diameter and / or long diameter.

[0067] In addition, the major axis of the needle-shaped filler indicates the length of the needle-shaped filler in the axial direction, and the minor axis of the needle-shaped filler indicates the diameter of the needle-shaped filler in a cross section perpendicular to the axial direction.

[0068] The aspect ratio (longer diameter / shorter diameter) of the needle-shaped filler is preferably 10-100, more preferably 15-80, further preferably 20-60, and particularly preferably 30-60.

[0069] By limiting the aspect ratio of the needle-shaped filler to such a range, the diffusion of light achieved by the needle-shaped filler in the anisotropic light-diffusing adhesive layer becomes optimal, for example, the viewing angle enlargement effect of the anisotropic light-diffusing adhesive layer can be improved. For example, when the needle-shaped filler as a whole is 100% by mass, preferably 90% by mass or more or 95% by mass or more of the needle-shaped filler has such an aspect ratio.

[0070] The refractive index of the needle-shaped filler in the major axis direction is preferably 1.48 to 1.58.

[0071] The refractive index of the needle-shaped filler in the minor axis direction is preferably 1.60 to 1.70.

[0072] By limiting the refractive index of the needle-shaped filler in the short axis direction or the long axis direction to such a range, light diffusion by the needle-shaped filler in the anisotropic light-diffusing adhesive layer becomes optimal, and for example, the viewing angle widening effect of the anisotropic light-diffusing adhesive layer can be enhanced.

[0073] <<Content>>

[0074] When the total solid content of the anisotropic light-diffusing adhesive layer is 100 parts by mass, the content of the needle-shaped filler is 1 to 50 parts by mass, preferably 2 to 25 parts by mass, and more preferably 5 to 15 parts by mass. By limiting the content of the needle-shaped filler to such a range, the diffusion of light achieved by the needle-shaped filler in the anisotropic light-diffusing adhesive layer becomes optimal, for example, the viewing angle enlargement effect of the anisotropic light-diffusing adhesive layer can be improved.

[0075] <<<Other ingredients>>>

[0076] The anisotropic light diffusion adhesive layer can contain other ingredients. As other ingredients, they are not particularly limited as long as they do not damage the effect of the invention. As other ingredients, for example, various general additives in the field of adhesive compositions such as coupling agents, leveling agents, crosslinking aids, plasticizers, softeners, fillers, antistatic agents, anti-aging agents, ultraviolet absorbers, antioxidants, light stabilizers, surfactants, etc. can be cited. For such various additives, conventionally known additives can be used.

[0077] <<<<Structure / physical properties of anisotropic light-diffusing adhesive layer>>>>

[0078] <<<Orientation degree of anisotropic light diffusing adhesive>>>

[0079] The needle-shaped filler is oriented and dispersed in one direction in the anisotropic light-diffusing adhesive layer. In addition, the needle-shaped filler being oriented in one direction includes not only a state in which the needle-shaped filler is completely oriented in one direction, but also a state in which the needle-shaped filler as a whole tends to be oriented in one direction (as a result, the anisotropic light-diffusing adhesive layer is in a state of a predetermined orientation degree).

[0080] The degree of orientation of the anisotropic light-diffusing adhesive can be measured by the following method.

[0081] A laminate 1 is produced by laminating a TAC film (triacetyl cellulose film) on an anisotropic light-diffusing adhesive layer. The TAC film is, for example, FUJITAC TG60UL manufactured by FUJIFILM Corporation.

[0082] The haze value of the laminate 1 was measured using a haze meter (NDH7000, manufactured by Nippon Denshoku Industries) in accordance with JIS K7136.

[0083] Next, laminate 1 was stacked between two polarizing plates with absorption axes differing by 90° (crossed Nicols arrangement) so that the absorption axis of one polarizing plate was parallel to the orientation axis of the needle-shaped filler in the anisotropic light-diffusing adhesive layer in laminate 1 to obtain laminate 2 .

[0084] Next, the total light transmittance of the laminate 2 was measured using a haze meter used for haze value measurement in accordance with JIS K7361. At this time, light from a light source was irradiated from one polarizing plate side, and the total light transmittance of the other polarizing plate side (a polarizing plate whose absorption axis is not parallel to the orientation axis of the needle-shaped filler in the anisotropic light-diffusing adhesive layer) was measured.

[0085] From the obtained total light transmittance, [Haze value of laminate 1] / [total light transmittance of laminate 2] was calculated, and this value was defined as the degree of orientation of the anisotropic light-diffusing adhesive.

[0086] At this time, if the orientation degree is larger, the anisotropic light diffusion adhesive layer has a smaller influence on the transmission axes of the two polarizing plates being formed into a 90° relationship (cross Nicol), that is, the needle-shaped filler has good orientation. Since the orientation degree is preferably large, it is preferably 10 or more, more preferably 15 or more, and further preferably 18 or more.

[0087] By limiting the degree of orientation to such a range, diffusion of light by the needle-shaped filler in the anisotropic light-diffusing adhesive layer becomes optimal, and the viewing angle widening effect of the anisotropic light-diffusing adhesive layer can be enhanced.

[0088] The degree of orientation of the anisotropic light-diffusing adhesive can be adjusted by the viscosity of the coating material, the coating thickness of the coating material, the coating speed, the types of the resin and the needle-shaped filler of the adhesive, and the like.

[0089] <<<Thickness>>>

[0090] The thickness of the anisotropic light-diffusing adhesive layer is preferably 5 μm to 100 μm, more preferably 5 μm to 30 μm. By limiting the thickness of the anisotropic light-diffusing adhesive layer to such a range, the diffusion of light achieved by the needle-shaped fillers in the anisotropic light-diffusing adhesive layer becomes optimal, and the viewing angle expansion effect of the anisotropic light-diffusing adhesive layer can be improved.

[0091] <<<Difference in haze value before and after the moisture and heat resistance test>>>

[0092] For the anisotropic light-diffusing adhesive layer, the difference in haze value before and after 168 hours in a moisture-heat resistance test at 85°C and a relative humidity of 85% (haze value before 168 hours - haze value after 168 hours) is preferably 2% or less. By limiting the difference in haze value to such a range, an anisotropic light-diffusing adhesive layer having excellent moisture-heat resistance can be obtained.

[0093] Among them, a laminate 3 in which an anisotropic light-diffusing adhesive layer is sandwiched between a glass plate and a PET film (manufactured by Toyobo Co., Ltd., Cosmoshine SRF (registered trademark), thickness 80 μm) is used as a test sample. According to JIS K7136, the diffuse transmittance (%) and the total light transmittance (%) are measured, and the haze value is the value calculated by the following formula.

[0094] Haze value (%) = (diffuse transmittance / total light transmittance) × 100

[0095] The haze value of the laminate 3 before the moisture and heat resistance test is preferably 10 to 80. By limiting the haze value range to such a range, the viewing angle widening effect of the anisotropic light-diffusing adhesive layer can be enhanced.

[0096] <<<<Method for producing anisotropic light-diffusing adhesive layer>>>>

[0097] An example of a method for producing an anisotropic light-diffusing adhesive layer is described below.

[0098] First, a solution containing the components constituting the above-mentioned anisotropic light-diffusing adhesive layer and a solvent (volatile solvent) as an optional component is stirred to prepare a coating material.

[0099] Next, after applying the coating to a substrate such as a release film or various optical elements, the solvent is dried and removed to form a composition, and the release film or various optical elements are laminated on the composition. In addition, in order to harden or stabilize the composition as needed, the composition is cured for about 1 day to 2 weeks in a temperature environment of about room temperature to about 60°C, thereby producing an anisotropic light-diffusing adhesive layer.

[0100] When applying a coating containing needle-shaped fillers, the long diameter of the needle-shaped fillers is oriented in a manner substantially along the coating direction by applying a shear force to the coating containing needle-shaped fillers, so that an anisotropic light-diffusing adhesive layer in which the needle-shaped fillers are oriented and dispersed in the same direction (approximately the same direction) can be manufactured. In addition, the degree of orientation of the needle-shaped fillers can be adjusted by the size of the needle-shaped fillers, the viscosity of the coating containing needle-shaped fillers, the coating method, the coating speed, etc. In addition, the film thickness of the anisotropic light-diffusing adhesive layer formed can be adjusted by the coating thickness of the coating, the amount of solvent in the coating, etc.

[0101] <<<<Application of anisotropic light-diffusing adhesive layer>>>>

[0102] The anisotropic light-diffusing pressure-sensitive adhesive layer can be suitably used for bonding the surface of the polarizing plate (upper polarizing plate) on the viewing side of a display device to an optical functional layer such as a hard coat layer.

[0103] When the display device is a liquid crystal display device, by using an anisotropic light-diffusing adhesive layer, a display device can be obtained in which the absorption axis of the upper polarizing plate (the polarizing plate on the visible side) of the liquid crystal display device is stacked in parallel with the orientation direction of the needle-shaped filler of the anisotropic light-diffusing adhesive layer.

[0104] More specifically, by using an anisotropic light-diffusing adhesive layer, a display device can be obtained that is stacked on the visible side of the upper polarizing plate of a liquid crystal display device in such a way that the angle difference between the orientation axis of the needle-shaped filler in the anisotropic light-diffusing adhesive layer and the absorption axis of the upper polarizing plate of the liquid crystal display device is within ±5°.

[0105] By adopting such a structure, a display device having an excellent viewing angle widening effect can be obtained.

[0106] The method for applying an anisotropic light-diffusing adhesive layer to a component to be bonded may be a method of directly forming the anisotropic light-diffusing adhesive layer on the component, or a method of forming the anisotropic light-diffusing adhesive layer in a sheet form on a peeling substrate (such as a film, etc.), and after attaching the anisotropic light-diffusing adhesive layer on the peeling substrate to the component, peeling off the peeling substrate.

[0107] Example

[0108] Hereinafter, the present invention will be described in more detail with reference to Examples and the like, but the scope of the present invention is not limited to these Examples and the like.

[0109] <<Manufacturing of anisotropic light diffusion film>>

[0110] <Example 1>

[0111] As a needle-shaped filler, calcium carbonate whiskers (long diameter: 10 μm to 30 μm, short diameter: 0.5 μm to 1.0 μm, refractive index in the long diameter direction: 1.49) were dispersed in ethyl acetate at a concentration of 20 wt % to prepare a dispersion.

[0112] Next, 91.7 parts by weight of a binder component 1 composed of an acrylic copolymer (solid content concentration: 35%, ratio of carboxyl-containing monomers in all monomer components: 0.0%, solvent: ethyl acetate, monomer components: EA, HEA, 2EHA) with a solid content, 7.8 parts by weight of a dispersion of calcium carbonate whiskers with a concentration of 20 wt% and 0.5 parts by weight of a hexamethylene diisocyanate curing agent as a curing agent were added to ethyl acetate and mixed while being diluted to produce a coating 1 with a viscosity of 3300 mPa·s.

[0113] Next, the coating 1 was applied to a 38 μm thick release PET film 1 with a target film thickness of 16 μm using an applicator, and then dried at 80° C. for 2 minutes to produce a composition 1. A 38 μm thick release PET film 2 that was easier to peel off than the applied release PET film was laminated on the produced composition 1, and then cured at room temperature for 1 week to obtain an anisotropic light-diffusing adhesive layer 1 with a double-sided film of Example 1. The film thickness of the anisotropic light-diffusing adhesive layer 1 was 17 μm.

[0114] <Example 2>

[0115] A coating 2 was prepared in the same manner as in Example 1 except that the coating viscosity was 2000 mPa·s, and a composition 2 was prepared from the coating 2. The anisotropic light-diffusing adhesive layer 2 with double-sided films of Example 2 was obtained using the composition 2. The thickness of the anisotropic light-diffusing adhesive layer 2 was 17 μm.

[0116] <Example 3>

[0117] Coating 3 was prepared in the same manner as in Example 1 except that the coating viscosity was 1500 mPa·s, and composition 3 was prepared from coating 3. Anisotropic light-diffusing adhesive layer 3 with double-sided films of Example 3 was obtained using composition 3. The thickness of anisotropic light-diffusing adhesive layer 3 was 17 μm.

[0118] <Example 4>

[0119] A binder component 2 composed of an acrylic copolymer with a solid content of 76.6 parts by weight (solid content concentration: 40%, ratio of carboxyl-containing monomers in all monomer components: 0.7%, solvent: ethyl acetate, monomer components: BA, HEA, AA), a dispersion of calcium carbonate whiskers with a solid content of 23.0 parts by weight and a concentration of 20wt%, and 0.4 parts by weight of a hexamethylene diisocyanate-based curing agent as a curing agent were added to ethyl acetate and mixed while being diluted to produce a coating 4 with a viscosity of 3000mPa·s.

[0120] Composition 4 was prepared from coating material 4 in the same manner as in Example 1 except that coating material 1 was replaced by coating material 4. Anisotropic light-diffusing adhesive layer 4 with double-sided films of Example 4 was obtained using composition 4. The thickness of anisotropic light-diffusing adhesive layer 4 was 15 μm.

[0121] <Comparative Example 1>

[0122] A binder component 3 composed of an acrylic copolymer with a solid content of 93.9 parts by weight (solid content concentration: 25%, ratio of carboxyl-containing monomers in all monomer components: 3.0%, solvent: ethyl acetate, monomer components: BA, MA, AA), a dispersion of calcium carbonate whiskers with a solid content of 6.0 parts by weight and a concentration of 20wt%, and 0.1 parts by weight of an epoxy curing agent as a curing agent are added to ethyl acetate and mixed while being diluted to produce a coating 5 with a viscosity of 2500mPa·s.

[0123] Composition 5 was prepared from coating material 5 in the same manner as in Example 1 except that coating material 1 was replaced by coating material 5, and an anisotropic light-diffusing adhesive layer 5 with double-sided films of Comparative Example 1 was obtained using composition 5. The thickness of anisotropic light-diffusing adhesive layer 5 was 16 μm.

[0124] <Comparative Example 2>

[0125] A coating material 6 was prepared in the same manner as in Example 1 except that the coating material viscosity was 700 mPa·s, and a composition 6 was prepared from the coating material 6. The anisotropic light-diffusing adhesive layer 6 with double-sided films of Comparative Example 2 was obtained using the composition 6. The thickness of the anisotropic light-diffusing adhesive layer 6 was 18 μm.

[0126] <<Evaluation>>

[0127] The following evaluations were performed on the anisotropic diffusion adhesive layers with double-sided films of Examples 1 to 4 and Comparative Examples 1 and 2 obtained above.

[0128] <Orientation evaluation by measuring the degree of orientation>

[0129] After peeling off the double-sided films of the anisotropic light-diffusing adhesive layers of the embodiments and comparative examples, TAC films (manufactured by Fujifilm Corporation, FUJITAC TG60UL) were laminated on both sides of the anisotropic light-diffusing adhesive layer to manufacture a laminate with double-sided TAC (hereinafter referred to as laminate 1), and the haze value of the manufactured laminate 1 was measured according to JIS K7136 using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., NDH7000).

[0130] Next, the stack 1 is stacked between two polarizing plates whose absorption axes differ by 90° (orthogonal Nicol configuration) in such a way that the absorption axis of one polarizing plate is parallel to the orientation axis of the needle-shaped filler in the anisotropic light-diffusing adhesive layer in the manufactured stack 1, thereby manufacturing a stack with double-sided polarizing plates TAC (hereinafter referred to as stack 2).

[0131] The total light transmittance of the manufactured laminate 2 was measured in accordance with JIS K7361 using a haze meter that measured the haze value. In addition, this measurement was performed in the following manner, that is, with respect to irradiation with light from a light source, irradiation was performed from the side of a polarizing plate having an absorption axis parallel to the orientation direction of the needle-shaped filler in the laminate 2, and the total light transmittance of the other polarizing plate side (a polarizing plate whose absorption axis is not parallel to the orientation direction of the needle-shaped filler) in the laminate 2 was measured.

[0132] From the obtained total light transmittance and haze value, [haze value of laminate 1] / [total light transmittance of laminate 2] was calculated, and this value was defined as the degree of orientation.

[0133] Table 1 shows the haze value of the laminate 1, the total light transmittance of the laminate 2, and the degree of orientation in Examples and Comparative Examples.

[0134] <Moisture and heat resistance test>

[0135] After peeling off the double-sided films of the anisotropic light-diffusing adhesive layers produced in the embodiments and comparative examples, a 38 μm thick release PET film is laminated on one side of the anisotropic light-diffusing adhesive layer and a 5 cm×5 cm glass plate is laminated on the other side to produce a laminated body of film-coated glass (hereinafter referred to as laminated body 3).

[0136] The haze value of the laminate 3 was measured using a haze meter (NDH7000, manufactured by Nippon Denshoku Industries) in accordance with JIS K7136.

[0137] Next, the laminate 3 was left standing for 168 hours in an atmosphere of 85°C and a relative humidity of 85%, and then the haze value after being left standing for 24 hours at room temperature was measured. The moist heat resistance was evaluated based on the difference in haze values ​​before and after this moist heat resistance test.

[0138] Table 1 shows the evaluation results.

[0139] <Evaluation of viewing angle characteristics by measuring contrast ratio at the front and at 60°>

[0140] After peeling off the double-sided films of the anisotropic light diffusion adhesive layers with double-sided films produced in the examples and comparative examples, a TAC film (manufactured by Fujifilm Corporation, FUJITAC TG60UL) was laminated on one side of the anisotropic light diffusion adhesive layer to produce a single-sided TAC laminate (hereinafter referred to as laminate 4).

[0141] Next, the exposed side of the anisotropic light-diffusing adhesive layer of the stack 4 is bonded to the screen surface of the VA (Vertical Alignment) liquid crystal display in such a way that the absorption axis of the upper polarizing plate (visible side) of the VA liquid crystal display is parallel to the orientation axis of the needle-shaped filler in the anisotropic light-diffusing adhesive layer of the stack 4.

[0142] Using a brightness viewing angle meter (manufactured by TEM, CONOMETER 80), the brightness under white display and the brightness under black display in the range of -80° to +80° in the direction orthogonal to the orientation direction of the needle-shaped filler were measured from the TAC film side (visible side) of the laminate 4 bonded to the surface of the VA-type liquid crystal display screen.

[0143] After calculating the contrast (white brightness / black brightness) based on the measured values ​​of white brightness and black brightness at each angle, the front direction contrast is calculated as: ((contrast at 0°) / (contrast of the liquid crystal display at 0°))×100, and the 60° direction contrast is calculated as: ((contrast at 60°) / (contrast of the liquid crystal display at 0°))×100. Table 1 shows the front direction contrast and 60° direction contrast in each embodiment and comparative example.

[0144] Moreover, in Figure 1 In FIG. 1 , the 60° direction contrast is plotted as the X-axis and the front direction contrast is plotted as the Y-axis, showing the relationship between the contrasts in each direction.

[0145] <Evaluation Criteria>

[0146] The evaluation criteria for the evaluation in Table 1 are as follows.

[0147] "Orientation"

[0148] ◎Orientation degree is 18 or more (the filler is fully oriented.)

[0149] ○ The degree of orientation is 10 or more and less than 18 (the orientation property is slightly reduced, but it is a level that does not cause any practical problems.)

[0150] × Orientation degree is less than 10 (the orientation of the filler is poor.)

[0151] "Moisture and heat resistance"

[0152] ○The difference in haze value before and after the moisture and heat resistance test is 2% or less (no problem with moisture and heat resistance.)

[0153] × The difference in haze value before and after the humidity and heat resistance test exceeded 2% (a decrease in haze was observed after the humidity and heat test.)

[0154] [Table 1]

[0155]

[0156] From Table 1 and Figure 1 It is found that the anisotropic light-diffusing adhesive layer of the present invention is excellent in viewing angle characteristics and moisture-heat resistance.

[0157] In addition, regarding the wet heat resistance test in Table 1, it was confirmed that the haze value after the wet heat resistance test decreased in Example 4 and Comparative Example 1 containing a carboxyl group-containing monomer. This is because the carboxyl group contained in the acrylic copolymer reacts (hydrolyzes) with other components including the needle-shaped filler under a wet heat environment, and the diffusibility is deteriorated.

Claims

1. An anisotropic light-diffusing adhesive layer, characterized in that: Include: An adhesive composed of an acrylic copolymer, and Needle-shaped fillers oriented and dispersed in one direction; Among all the monomer components constituting the acrylic copolymer, the ratio of the monomer having a carboxyl group is 1% or less, The content of the needle-shaped filler is 1 to 50 parts by mass, based on 100 parts by mass of the total solid content of the anisotropic light-diffusing adhesive layer. The anisotropic light-diffusing adhesive layer has an orientation degree of 10 or more.

2. The anisotropic light-diffusing adhesive layer according to claim 1, characterized in that: In a moisture and heat resistance test in an atmosphere of 85°C and 85% relative humidity, the difference in haze values ​​before and after 168 hours, i.e., the haze value before 168 hours minus the haze value after 168 hours, was 2% or less.

3. The anisotropic light-diffusing adhesive layer according to claim 1 or 2, characterized in that: The needle-shaped filler contains one or more components selected from carbonates, sulfates, and nitrates.

4. The anisotropic light-diffusing adhesive layer according to any one of claims 1 to 3, wherein The needle-shaped filler has a short diameter of 0.1 μm to 10 μm, a long diameter of 2 μm to 1000 μm, and an aspect ratio of 10 to 100. 5 . The anisotropic light-diffusing adhesive layer according to claim 1 , wherein: The weight average molecular weight of the acrylic copolymer is 200,000 to 1.8 million. 6 . The anisotropic light-diffusing adhesive layer according to claim 1 , wherein: The film thickness is 5μm to 100μm.

7. A liquid crystal display device, characterized in that: With upper polarizer, The anisotropic light-diffusing adhesive layer according to any one of claims 1 to 6 is laminated on the visible side of the upper polarizing plate so that the angle difference between the orientation axis of the needle-shaped filler and the absorption axis of the upper polarizing plate is within ±5°.