Adhesive tape for semiconductor processing

By optimizing the structure of the buffer layer and substrate in the adhesive tape for semiconductor processing, improving its fracture performance and cutting properties, the chip cutting problem during the adhesive tape is solved, and a more efficient semiconductor chip thinning and productivity improvement is achieved.

CN118974890APending Publication Date: 2024-11-15LINTEC CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202280094221.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-03-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

During the thinning process of semiconductor chips, chips are easily generated when the adhesive tape for semiconductor processing is cut, resulting in chip rupture, and the prior art is difficult to effectively suppress such defects.

Method used

A bonding tape for semiconductor processing with a specific buffer layer and substrate structure was developed. The fracture energy and stress-strain gradient of the buffer layer reached 15MJ/m3 and 30MPa or more, and the product of the fracture strain and stress of the substrate was more than 60MPa. Moreover, the thickness of the adhesive layer is less than 100 μm to improve the tool cutting property of the adhesive tape.

Benefits of technology

It significantly reduces the generation of chips, prevents chip rupture, improves the yield and flexural strength of semiconductor chips, and enhances the thinning effect of the chip.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974890A_ABST
    Figure CN118974890A_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing an adhesive tape for semiconductor processing having excellent cutting properties by a cutter. The problem is solved by an adhesive tape for semiconductor processing having a laminated structure in which a buffer layer, a base material, and an adhesive layer are laminated in this order, the buffer layer satisfying both the following requirements (alpha) and (beta). Condition (alpha): The breaking energy of the buffer layer at 23 DEG C is 15 MJ / m3 or more. Requirement (beta): When the buffer layer is subjected to a tensile test at a temperature of 23 DEG C, the stress increase gradient [Delta] [Rho] 80-100 from the strain ([Epsilon] 80) of 80% of the fracture strain ([Epsilon] 100) to the fracture strain ([Epsilon] 100) is 30 MPa or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive tape for semiconductor processing. More specifically, the present invention relates to an adhesive tape for semiconductor processing, a method for using the adhesive tape for semiconductor processing, and a method for manufacturing a semiconductor device using the adhesive tape for semiconductor processing. Background Art

[0002] In recent years, with the rapid development of miniaturization and multifunctionalization of various electronic devices, there is a demand for miniaturization and thinning of semiconductor chips mounted in various electronic devices.

[0003] The thinning of semiconductor chips can generally be performed by grinding the back side of a semiconductor wafer. In addition, as a method for obtaining a thinned semiconductor chip, a method called Dicing Before Grinding (DBG) is known. DBG is a method in which a groove of a given depth is formed from the surface side (circuit forming side) of a semiconductor wafer using a dicing knife or the like, and then grinding is performed from the back side of the semiconductor wafer, and the semiconductor wafer is singulated by grinding to obtain a semiconductor chip.

[0004] In DBG, since back grinding of a semiconductor wafer and singulation of the semiconductor wafer can be performed simultaneously, thinned semiconductor chips can be manufactured efficiently.

[0005] In addition, as a deformation method of DBG, the following method has been proposed: instead of forming a groove on the surface side of the semiconductor wafer, a modified area is formed inside the semiconductor wafer using laser or plasma, and the semiconductor wafer is singulated to obtain a semiconductor chip using the stress during the back grinding of the semiconductor wafer. In the case of this method, the semiconductor wafer is cut along the crystal direction starting from the modified area. Therefore, compared with DBG using a cutting knife, the occurrence of edge collapse can be reduced. As a result, a semiconductor chip with excellent flexural strength can be obtained, and further thinning of the semiconductor chip can be achieved. In addition, compared with DBG in which a groove of a given depth is formed on the surface of the semiconductor wafer using a cutting knife, there is no area where the semiconductor wafer is removed by the cutting knife (in other words, because the groove width is extremely small), so it also has the advantage of excellent yield of semiconductor chips.

[0006] However, in the manufacture of semiconductor chips including a back grinding process of a semiconductor wafer such as DBG or a modified method of DBG, an adhesive tape for semiconductor processing called a back grinding sheet is usually affixed to the surface of the semiconductor wafer in order to protect the circuit on the surface of the semiconductor wafer and to hold the semiconductor wafer and the semiconductor chip.

[0007] As such an adhesive tape for semiconductor processing, for example, an adhesive tape for semiconductor processing having a laminated structure in which a buffer layer, a base material, and an adhesive layer are laminated in this order has been proposed (for example, refer to Patent Document 1, etc.).

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2015-183008 Summary of the invention

[0011] Problems to be solved by the invention

[0012] However, when manufacturing semiconductor chips including a back grinding process of a semiconductor wafer such as DBG or a modified method of DBG, when the back of the semiconductor wafer is ground using a grinder, if there is excess semiconductor processing adhesive tape on the periphery of the semiconductor wafer, the grinder may carry the excess semiconductor processing adhesive tape in. Therefore, the semiconductor processing adhesive tape is cut along the periphery of the semiconductor wafer before back grinding.

[0013] However, as semiconductor chips become smaller and thinner, chips generated when cutting the adhesive tape for semiconductor processing may cause defects or breakage of the semiconductor chip (hereinafter referred to as "semiconductor chip breakage").

[0014] Therefore, in order to suppress the occurrence of cracks in semiconductor chips, the inventors of the present invention studied the main cause of the generation of chips. As a result, it was found that when the semiconductor processing adhesive tape is cut with a cutter, the buffer layer is rubbed due to the contact between the cutter and the buffer layer, causing the resin constituting the buffer layer to twist and the cut surface to become rough, thereby generating chips.

[0015] Based on such findings, the present inventors believed that improving the cuttability of the adhesive tape for semiconductor processing by a cutter and suppressing the roughness of the cut surface of the buffer layer are effective methods for suppressing the generation of chips, and further conducted intensive studies to complete the present invention.

[0016] Therefore, an object of the present invention is to provide an adhesive tape for semiconductor processing having excellent cutting properties by a cutter.

[0017] Solution to the problem

[0018] The present inventors have conducted intensive studies and have found that an adhesive tape for semiconductor processing having a buffer layer satisfying specific requirements can solve the above-mentioned problems, thereby completing the present invention.

[0019] That is, the present invention relates to the following [1] to [7].

[0020] [1] An adhesive tape for semiconductor processing, comprising a laminated structure in which a buffer layer, a base material and an adhesive layer are laminated in this order,

[0021] The buffer layer satisfies both the following requirement (α) and the following requirement (β).

[0022] Requirement (α): The breaking energy of the buffer layer at 23°C is 15 MJ / m 3 above.

[0023] Requirement (β): When the buffer layer is subjected to a tensile test at a temperature of 23°C, the breaking strain (ε 100 ) 80% strain (ε 80 ) increases to the above fracture strain (ε 100 ) to the stress increase gradient Δρ 80-100 It is above 30MPa.

[0024] [2] The adhesive tape for semiconductor processing according to the above [1], wherein the substrate satisfies the following requirement (γ).

[0025] · Requirement (γ): Fracture strain at 23°C (ε 100 ) and the fracture stress (ρ 100 ) is greater than 60MPa.

[0026] [3] The adhesive tape for semiconductor processing according to [1] or [2] above, wherein the thickness of the adhesive layer is less than 100 μm.

[0027] [4] A method for using an adhesive tape for semiconductor processing, wherein the adhesive tape for semiconductor processing is the adhesive tape for semiconductor processing described in any one of [1] to [3] above, the method comprising:

[0028] When grinding the back surface of a semiconductor wafer, the adhesive tape for semiconductor processing is affixed to the surface of the semiconductor wafer, and the adhesive tape for semiconductor processing is cut along the outer circumference of the semiconductor wafer.

[0029] [5] A method for manufacturing a semiconductor device, the method comprising:

[0030] Step (S1) of attaching the adhesive tape for semiconductor processing according to any one of [1] to [3] above to the surface of a semiconductor wafer, and cutting the adhesive tape for semiconductor processing along the outer periphery of the semiconductor wafer.

[0031] [6] The method for manufacturing a semiconductor device according to [5] above, further comprising the following step (S2).

[0032] Step (S2) is a step of grinding the semiconductor wafer from the back side.

[0033] [7] The method for manufacturing a semiconductor device according to [6] above, further comprising the following step (S3).

[0034] Step (S3): a step of dicing the semiconductor wafer into individual pieces

[0035] [8] The method for manufacturing a semiconductor device according to [6] above, wherein:

[0036] As the semiconductor wafer, a semiconductor wafer having grooves formed on the surface side is used,

[0037] In the step (S2), the semiconductor wafer is singulated into a plurality of chips using the groove as a starting point.

[0038] [9] The method for manufacturing a semiconductor device according to [6] above, wherein:

[0039] As the semiconductor wafer, a semiconductor wafer having a modified region formed therein is used, or a modified region is formed inside the semiconductor wafer after the step (S1).

[0040] In the step (S2), the semiconductor wafer is singulated into a plurality of chips with the reformed region as a starting point.

[0041] Effects of the Invention

[0042] According to the present invention, it is possible to provide an adhesive tape for semiconductor processing that is excellent in cutting properties by a cutter. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is a schematic cross-sectional view showing an example of the adhesive tape for semiconductor processing of the present invention.

[0044] Figure 2 It is a schematic diagram of the process of the method for manufacturing a semiconductor device of the present invention.

[0045] Figure 3 A diagram showing an analysis model based on Abaqus.

[0046] Figure 4 These are analysis images based on Abaqus of Example 1sim. and Comparative Example 3sim. in “Evaluation of cutting performance by tool (1): Evaluation based on simulation”.

[0047] Figure 5These are the results of observation of the cross sections of Example 1 exp. and Comparative Example 3 exp. in "Evaluation of cutting properties by a tool (2): Evaluation by experiment" using a scanning electron microscope (SEM) (photographs in lieu of drawings).

[0048] Explanation of symbols

[0049] 1 Adhesive tape for semiconductor processing

[0050] 11 Buffer layer

[0051] 12. Substrate

[0052] 13 Adhesive layer DETAILED DESCRIPTION

[0053] The upper limit and lower limit of the numerical range described in this specification can be arbitrarily combined. For example, when "A to B" and "C to D" are described as numerical ranges, the numerical ranges of "A to D" and "C to B" are also included in the scope of the present invention.

[0054] Unless otherwise specified, the numerical range "lower limit value to upper limit value" described in the present specification means more than the lower limit value and less than the upper limit value.

[0055] In the present specification, the numerical values ​​of Examples are numerical values ​​that can be used as upper limit values ​​or lower limit values.

[0056] In this specification, "(meth)acrylate" is a concept including both "acrylate" and "methacrylate", and the same applies to other similar terms. For example, "(meth)acryloyl" is a concept including both "acryloyl" and "methacryloyl".

[0057] In this specification, the weight average molecular weight and the number average molecular weight are polystyrene-equivalent values ​​measured by gel permeation chromatography (GPC).

[0058] [Adhesive tape for semiconductor processing]

[0059] The adhesive tape for semiconductor processing of the present invention has a laminated structure in which a buffer layer, a substrate, and an adhesive layer are laminated in this order. The buffer layer satisfies both the following requirements (α) and (β).

[0060] Requirement (α): The breaking energy of the buffer layer at 23°C is 15 MJ / m 3 above.

[0061] Requirement (β): When the buffer layer is subjected to a tensile test at a temperature of 23°C, the breaking strain (ε 100 ) 80% strain (ε 80 ) increases to the above fracture strain (ε 100) to the stress increase gradient Δρ 80-100 It is above 30MPa.

[0062] Figure 1 A schematic cross-sectional view showing one embodiment of the adhesive tape for semiconductor processing of the present invention. Figure 1 The adhesive tape 1 for semiconductor processing shown has a laminated structure in which a buffer layer 11, a base material 12, and an adhesive layer 13 are laminated in this order.

[0063] Figure 1 In the adhesive tape 1 for semiconductor processing shown, the buffer layer 11, the substrate 12 and the adhesive layer 13 are directly laminated together without interposing other layers. Figure 1 The adhesive tape 1 for semiconductor processing shown is composed only of a buffer layer 11 , a base material 12 , and an adhesive layer 13 .

[0064] However, the semiconductor processing adhesive tape 1 is not necessarily limited to such a mode. For example, other layers may be provided at at least any position between the buffer layer 11 and the substrate 12, or between the substrate 12 and the adhesive layer 13 as required. Examples of such other layers include a primer layer, a layer for embedding bumps formed on the circuit surface of a wafer, and the like. In addition, a release sheet for protecting the adhesive layer 13 until use may be laminated on the surface of the adhesive layer 13. In addition, a coating layer may also be provided on the surface of the buffer layer 11.

[0065] It should be noted that in Figure 1 In the embodiment, the buffer layer 11, the substrate 12 and the adhesive layer 13 each have a single-layer structure, but they may also have a multi-layer structure.

[0066] Hereinafter, the physical properties and configuration of each member of the adhesive tape for semiconductor processing will be described in detail.

[0067] In addition, in the following description, the "adhesive tape for semiconductor processing" may be simply referred to as "adhesive tape".

[0068] [Buffer layer]

[0069] The buffer layer has the function of relieving stress on the semiconductor wafer during back grinding and preventing cracks and defects from being generated in the semiconductor wafer. In addition, after the adhesive tape is attached to the semiconductor wafer and the adhesive tape is cut along the outer periphery of the semiconductor wafer, the semiconductor wafer is placed on the chuck table via the adhesive tape for back grinding, and the adhesive tape having the buffer layer makes it easy to properly hold the semiconductor wafer on the chuck table. In this way, when performing back grinding of the semiconductor wafer, the adhesive tape having the buffer layer has great advantages.

[0070] On the other hand, since the cushion layer is softer than the base material, it also has disadvantages. Specifically, when the adhesive tape is cut, the resin of the cushion layer is tangled, resulting in a rough cut surface and sometimes chips.

[0071] The inventors of the present invention have repeatedly investigated to eliminate the above disadvantages, and as a result, they have come to the conclusion that improving the tool-based cutting property of the adhesive tape and suppressing the roughness of the cut surface of the buffer layer are effective in suppressing chips, and have conducted in-depth research. As a result, by focusing on the fracture energy of the buffer layer and the stress increase gradient near the fracture point in the stress-strain line diagram of the buffer layer, the tool-based cutting property of the buffer layer can be improved. Furthermore, after further repeated research, the above-mentioned requirements (α) and (β) were determined.

[0072] <Requirements (α)>

[0073] In requirement (α), the fracture energy of the buffer layer at 23°C is limited to 15 MJ / m 3 By making the breaking energy of the buffer layer at 23°C 15 MJ / m 3 As described above, if the buffer layer also satisfies the requirement (β), the cutting property of the buffer layer by a cutter can be made excellent. It is estimated that the fracture energy of the buffer layer at 23°C is 15 MJ / m 3 In the above case, the buffer layer is less likely to be deformed even when it contacts the cutter, and twisting of the buffer layer can be suppressed, thereby improving the cutting performance.

[0074] It should be noted that the fracture energy of the buffer layer at 23°C is less than 15MJ / m 3 When the buffer layer is thinner than the buffer layer, the cutting property by the cutter cannot be improved.

[0075] Here, from the viewpoint of making the cutability of the buffer layer by a cutter more excellent, the breaking energy of the buffer layer at 23° C. is preferably 17 MJ / m 3 More preferably 22MJ / m 3 More preferably, 27 MJ / m 3 above.

[0076] In addition, from the viewpoint of preventing wear of the tool, the fracture energy of the buffer layer at 23° C. is preferably 150 MJ / m 3 the following.

[0077] It should be noted that the breaking energy of the buffer layer at 23°C is a value obtained by integrating the stress and strain line diagram obtained by tensile testing at 23°C based on JIS K7161:1994 and JIS K7127:1999 until the breaking point. The strain can be obtained by the initial test piece length (mm) × elongation (%). It should be noted that the breaking stress and breaking strain described later are the stress and strain at the time of breaking (breaking point) in the above-mentioned tensile test, respectively.

[0078] <Requirements (β)>

[0079] The requirement (β) specifies that when the buffer layer is subjected to a tensile test at a temperature of 23°C, the breaking strain (ε 100 ) 80% strain (ε 80 ) increases to the above fracture strain (ε 100 ) to the stress increase gradient Δρ 80-100 The stress increase gradient Δρ is 30 MPa or more. 80-100 When the pressure is 30 MPa or more, the degree of curing of the buffer layer during the process of cutting by the cutter is improved during the process of processing curing (strain curing), and the deformation (elongation) of the buffer layer during the cutting by the cutter can be suppressed. Therefore, it can be inferred that the twisting of the buffer layer is suppressed, and the cutting property becomes good.

[0080] It should be noted that the stress increase gradient Δρ of the buffer layer 80-100 When the pressure is less than 30 MPa, the cuttability of the buffer layer by a cutter cannot be made excellent.

[0081] Here, from the viewpoint of improving the cutting performance of the buffer layer by the cutter, the stress increase gradient Δρ 80-100 It is preferably 50 MPa or more, more preferably 70 MPa or more, further preferably 75 MPa or more, further preferably 80 MPa or more, further preferably 85 MPa or more, further preferably 90 MPa or more, further preferably 95 MPa or more, further preferably 100 MPa or more. In addition, the stress increase gradient Δρ 80-100 Usually below 200 MPa.

[0082] <Other physical properties>

[0083] The buffer layer is a softer layer than the base material, and thus can appropriately alleviate the stress during back grinding of the semiconductor wafer.

[0084] It should be noted that from the perspective of more appropriately alleviating the stress during back grinding of the semiconductor wafer, the elastic modulus of the buffer layer at 23°C is preferably below 1200 MPa, more preferably below 1000 MPa, further preferably below 800 MPa, further preferably below 700 MPa, and further preferably below 500 MPa.

[0085] In addition, it is easy to obtain the above-mentioned fracture energy and stress increase gradient Δρ 80-100 From the viewpoint of strength, the breaking stress of the buffer layer is preferably 30 MPa or more, more preferably 50 MPa or more, further preferably 55 MPa or more, and further preferably 60 MPa or more.

[0086] In addition, the stress increase gradient Δρ is easily obtained from 80-100 From the perspective of 100 ) is preferably 0.50 or more, more preferably 1.0 or more, further preferably 1.1 or more, further preferably 1.2 or more, further preferably 1.3 or more, and further preferably 1.4 or more.

[0087] <Thickness of buffer layer>

[0088] From the viewpoint of appropriately relaxing stress during back grinding of the semiconductor wafer, the thickness of the buffer layer is preferably 1 μm to 100 μm, more preferably 5 μm to 80 μm, and even more preferably 10 μm to 60 μm.

[0089] <Composition of buffer layer>

[0090] As long as the buffer layer has the function of appropriately alleviating the stress of the semiconductor wafer during back grinding and satisfies the above-mentioned requirements (α) and (β), it can be used without particular restrictions. From the perspective of making it easier to exert the effects of the present invention, the buffer layer is preferably a cured product of a buffer layer forming composition containing an energy-ray polymerizable compound.

[0091] Hereinafter, each component contained in the layer formed from the composition for forming a buffer layer containing an energy beam polymerizable compound will be described in order.

[0092] <<Layer formed from a buffer layer-forming composition containing an energy-ray-polymerizable compound>>

[0093] The buffer layer-forming composition containing the energy-ray-polymerizable compound is cured by irradiation with energy rays.

[0094] In this specification, "energy ray" refers to a ray having energy particles in an electromagnetic wave or a charged particle beam, and examples of energy ray include ultraviolet rays, radiation, electron beams, etc. Ultraviolet rays can be irradiated by using, for example, a high-pressure mercury lamp, a fusion lamp, a xenon lamp, a black light lamp, or an LED lamp as an ultraviolet source. Electron beams can be irradiated by electron beams generated by an electron beam accelerator, etc.

[0095] More specifically, the buffer layer-forming composition containing an energy-ray-polymerizable compound preferably contains urethane (meth)acrylate (a1). The buffer layer-forming composition contains the component (a1), which makes it easy to adjust the breaking energy of the buffer layer to the above range.

[0096] It is more preferred that the buffer layer-forming composition contains, in addition to the above (a1), at least one selected from a polymerizable compound (a2) having an alicyclic group or heterocyclic group having 6 to 20 ring atoms and a polymerizable compound (a3) ​​having a functional group.

[0097] Moreover, the buffer layer-forming composition may contain a polyfunctional polymerizable compound (a4) in addition to the above-mentioned components (a1) to (a3).

[0098] Furthermore, the buffer layer-forming composition preferably contains a photopolymerization initiator, and may contain other additives and resin components within a range not impairing the effects of the present invention.

[0099] Hereinafter, each component contained in the buffer layer-forming composition containing an energy-ray-polymerizable compound will be described in detail.

[0100] (Urethane (meth)acrylate (a1))

[0101] Urethane (meth)acrylate (a1) is a compound having at least a (meth)acryloyl group and a urethane bond, and has the property of being polymerized and cured by energy ray irradiation. Urethane (meth)acrylate (a1) is an oligomer or a polymer, and is preferably an oligomer in the present embodiment.

[0102] In addition, in the following description, "urethane (meth)acrylate (a1)" is also referred to as "component (a1)".

[0103] The weight average molecular weight (Mw) of the component (a1) is preferably 1,000 to 100,000, more preferably 2,000 to 60,000, and even more preferably 2,000 or more and less than 10,000.

[0104] The number of (meth)acryloyl groups in the component (a1) (hereinafter also referred to as "the number of functional groups") may be monofunctional, difunctional, or trifunctional or higher, and is preferably monofunctional or difunctional.

[0105] Component (a1) can be obtained, for example, by reacting an isocyanate-terminated urethane prepolymer obtained by reacting a polyol compound with a polyisocyanate compound with a (meth)acrylate having a hydroxyl group. Component (a1) may be used alone or in combination of two or more.

[0106] The polyol compound used as the raw material of component (a1) is not particularly limited as long as it has two or more hydroxyl groups. Specific polyol compounds include, for example, alkylene glycols, polyether polyols, polyester polyols, polycarbonate polyols, etc. Among them, polyester polyols or polycarbonate polyols are preferred.

[0107] The polyol compound may be any of bifunctional diols, trifunctional triols, and tetrafunctional or higher polyols, preferably bifunctional diols, and more preferably polyester diols or polycarbonate diols.

[0108] Examples of the polyisocyanate compound include aliphatic polyisocyanates such as tetramethylene diisocyanate, hexamethylene diisocyanate, and trimethylhexamethylene diisocyanate; alicyclic diisocyanates such as isophorone diisocyanate, norbornane diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, dicyclohexylmethane-2,4'-diisocyanate, and ω,ω'-diisocyanate dimethylcyclohexane; and aromatic diisocyanates such as 4,4'-diphenylmethane diisocyanate, toluene diisocyanate, xylylene diisocyanate, tolidine diisocyanate, tetramethylene xylylene diisocyanate, and naphthalene-1,5-diisocyanate.

[0109] Among them, isophorone diisocyanate, hexamethylene diisocyanate, and xylylene diisocyanate are preferred.

[0110] The urethane (meth)acrylate (a1) can be obtained by reacting a (meth)acrylate having a hydroxyl group with the isocyanate-terminated urethane prepolymer obtained by reacting a polyol compound with a polyisocyanate compound. The (meth)acrylate having a hydroxyl group is not particularly limited as long as it is a compound having a hydroxyl group and a (meth)acryloyl group in at least one molecule.

[0111] Specific examples of (meth)acrylates having a hydroxyl group include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 4-hydroxycyclohexyl (meth)acrylate, 5-hydroxycyclooctyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, pentaerythritol tri(meth)acrylate, polyethylene glycol mono(meth)acrylate, and polypropylene glycol mono(meth)acrylate; hydroxyl group-containing (meth)acrylamides such as N-hydroxymethyl (meth)acrylamide; and reactants obtained by reacting (meth)acrylic acid with diglycidyl esters of vinyl alcohol, vinyl phenol, and bisphenol A.

[0112] Among them, hydroxyalkyl (meth)acrylate is preferred, and 2-hydroxyethyl (meth)acrylate is more preferred.

[0113] As conditions for reacting the isocyanate-terminated urethane prepolymer and the (meth)acrylate having a hydroxyl group, it is preferable to react at 60° C. to 100° C. for 1 to 4 hours in the presence of a solvent and a catalyst added as needed.

[0114] The content of the component (a1) in the buffer layer-forming composition is preferably 10 to 80% by mass, more preferably 30 to 80% by mass, and even more preferably 40 to 80% by mass, based on the total amount (100% by mass) of the buffer layer-forming composition.

[0115] (Polymerizable compound (a2) having an alicyclic group or a heterocyclic group having 6 to 20 ring atoms)

[0116] The polymerizable compound (a2) having an alicyclic group or heterocyclic group having 6 to 20 ring atoms (hereinafter also referred to as "component (a2)") is a polymerizable compound having an alicyclic group or heterocyclic group having 6 to 20 ring atoms, preferably a compound further having at least one (meth)acryloyl group, and more preferably a compound having one (meth)acryloyl group. By using component (a2), the film-forming property of the obtained buffer layer-forming composition can be improved.

[0117] It should be noted that the definition of component (a2) overlaps with the definition of component (a3) ​​described later, but the overlapping part is included in component (a3). For example, a compound having at least one (meth)acryloyl group, an alicyclic group or heterocyclic group having 6 to 20 ring atoms, and a functional group such as a hydroxyl group, an epoxy group, an amide group, or an amino group is included in the definitions of both component (a2) and component (a3), but in the present invention, the compound is deemed to be included in component (a3).

[0118] The number of ring atoms of the alicyclic group or heterocyclic group possessed by component (a2) is preferably 6 to 20, more preferably 6 to 18, and even more preferably 6 to 16. Examples of atoms constituting the ring structure of the heterocyclic group include carbon atoms, nitrogen atoms, oxygen atoms, and sulfur atoms.

[0119] It should be noted that the number of ring atoms refers to the number of atoms that constitute the ring itself in a compound in which atoms are bonded to form a ring structure, and the number of ring atoms does not include atoms that do not constitute the ring (for example, hydrogen atoms bonded to atoms that constitute the ring) and atoms contained in the substituent when the ring is substituted by a substituent.

[0120] Specific examples of component (a2) include: (meth)acrylates containing alicyclic groups such as isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxy (meth)acrylate, cyclohexyl (meth)acrylate, and adamantyl (meth)acrylate; (meth)acrylates containing heterocyclic groups such as tetrahydrofurfuryl (meth)acrylate and morpholine (meth)acrylate; and the like.

[0121] In addition, the component (a2) may be used individually by 1 type, or may use 2 or more types together.

[0122] Among the (meth)acrylates containing an alicyclic group, isobornyl (meth)acrylate is preferred, and among the (meth)acrylates containing a heterocyclic group, tetrahydrofurfuryl (meth)acrylate is preferred.

[0123] When the buffer layer forming composition contains component (a2), the content of component (a2) in the buffer layer forming composition is preferably 10 to 80% by mass, more preferably 20 to 70% by mass, based on the total amount (100% by mass) of the buffer layer forming composition.

[0124] (Polymerizable compound having a functional group (a3))

[0125] The polymerizable compound (a3) ​​having a functional group (hereinafter also referred to as "component (a3)") is a polymerizable compound containing functional groups such as a hydroxyl group, an epoxy group, an amide group, an amino group, etc., and is preferably a compound further having at least one (meth)acryloyl group, and more preferably a compound having one (meth)acryloyl group.

[0126] Component (a3) ​​has good compatibility with component (a1), and the viscosity of the buffer layer forming composition is easily adjusted to a suitable range. In addition, the energy at break of the buffer layer formed by the composition is easily adjusted to the above range, and even if the buffer layer is thin, the cushioning performance is also good.

[0127] Examples of the component (a3) ​​include hydroxyl group-containing (meth)acrylates, epoxy group-containing compounds, amide group-containing compounds, and amino group-containing (meth)acrylates.

[0128] Examples of the hydroxyl group-containing (meth)acrylate include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, phenyl hydroxypropyl (meth)acrylate, cyclohexanol (meth)acrylate, 4-tert-butylcyclohexanol acrylate, and 2-hydroxy-3-phenoxypropyl acrylate.

[0129] Examples of the epoxy group-containing compound include glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, and allyl glycidyl ether. Among them, epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate and methyl glycidyl (meth)acrylate are preferred.

[0130] Examples of the amide group-containing compound include (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methylolpropane(meth)acrylamide, N-methoxymethyl(meth)acrylamide, and N-butoxymethyl(meth)acrylamide.

[0131] Examples of the amino group-containing (meth)acrylate include primary amino group-containing (meth)acrylate, secondary amino group-containing (meth)acrylate, and tertiary amino group-containing (meth)acrylate.

[0132] Among them, hydroxyl-containing (meth)acrylates are preferred, hydroxyl-containing (meth)acrylates having an aromatic ring such as phenylhydroxypropyl (meth)acrylate, hydroxyl-containing (meth)acrylates having an alicyclic ring such as cyclohexanol (meth)acrylate and 4-tert-butylcyclohexanol acrylate are more preferred, and hydroxyl-containing (meth)acrylates having an alicyclic ring are further preferred. The number of carbon atoms in the alicyclic ring is preferably 6 to 20, more preferably 6 to 18, and even more preferably 6 to 16.

[0133] In addition, the component (a3) ​​may be used individually by 1 type, or may use 2 or more types together.

[0134] When the buffer layer forming composition contains component (a3), from the viewpoint of easily adjusting the fracture energy of the buffer layer to the above-mentioned range and easily improving the film-forming property of the buffer layer forming composition, the content of component (a3) ​​in the buffer layer forming composition is preferably 5% by mass to 50% by mass, more preferably 10% by mass to 40% by mass, and further preferably 20% by mass to 30% by mass relative to the total amount (100% by mass) of the buffer layer forming composition.

[0135] In addition, when the buffer layer forming composition contains both components (a2) and (a3), the content ratio of component (a2) to component (a3) ​​in the buffer layer forming composition [(a2) / (a3)] is preferably 0.5 to 3.0, more preferably 1.0 to 3.0, further preferably 1.3 to 3.0, and further preferably 1.5 to 2.8 in terms of mass ratio.

[0136] From the viewpoint of easily preparing a buffer layer satisfying the above requirements (α) and (β), the buffer layer-forming composition preferably contains component (a3), and the component (a3) ​​is preferably a hydroxyl-containing (meth)acrylate having an alicyclic ring.

[0137] (Multifunctional polymerizable compound (a4))

[0138] The multifunctional polymerizable compound (a4) (hereinafter also referred to as "component (a4)") refers to a compound having two or more photopolymerizable unsaturated groups. The photopolymerizable unsaturated group is a functional group containing a carbon-carbon double bond, and examples thereof include: (meth)acryloyl, vinyl, allyl, vinylbenzyl, etc. Two or more photopolymerizable unsaturated groups can be combined. By reacting the photopolymerizable unsaturated group in the multifunctional polymerizable compound with the (meth)acryloyl group in component (a1) and reacting the photopolymerizable unsaturated groups in component (a4) with each other, a three-dimensional mesh structure (cross-linked structure) can be formed. When a multifunctional polymerizable compound is used, the cross-linked structure formed by energy ray irradiation increases compared to the case of using a compound containing only one photopolymerizable unsaturated group, so that the buffer layer exhibits specific viscoelasticity and it is easy to adjust the fracture energy to the above range.

[0139] It should be noted that the definition of component (a4) overlaps with the definitions of the above-mentioned components (a2) and (a3), but the overlapping parts are included in component (a4). For example, a compound having an alicyclic group or heterocyclic group with 6 to 20 ring atoms and having two or more (meth)acryloyl groups is included in the definitions of both component (a4) and component (a2), but in the present invention, the compound is included in component (a4). In addition, a compound containing functional groups such as hydroxyl, epoxy, amide, and amino and having two or more (meth)acryloyl groups is included in the definitions of both component (a4) and component (a3), but in the present invention, the compound is included in component (a4).

[0140] From the above viewpoints, the number of photopolymerizable unsaturated groups (number of functional groups) in the polyfunctional polymerizable compound is preferably 2 to 10, more preferably 3 to 6.

[0141] The weight average molecular weight of the component (a4) is preferably 30 to 40,000, more preferably 100 to 10,000, and even more preferably 200 to 1,000.

[0142] Specific examples of component (a4) include diethylene glycol di(meth)acrylate, ethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, divinylbenzene, vinyl (meth)acrylate, divinyl adipate, N,N'-methylenebis(meth)acrylamide, and the like.

[0143] Among them, dipentaerythritol hexa(meth)acrylate is preferred.

[0144] In addition, the component (a4) may be used individually by 1 type, or may use 2 or more types together.

[0145] The content of the component (a4) in the buffer layer-forming composition is preferably 0 to 40% by mass, more preferably 0 to 20% by mass, and even more preferably 0 to 15% by mass, based on the total amount (100% by mass) of the buffer layer-forming composition.

[0146] (Polymerizable compound (a5) other than components (a1) to (a4))

[0147] The buffer layer-forming composition may contain a polymerizable compound (a5) (hereinafter also referred to as “component (a5)”) as a component other than the above-mentioned components (a1) to (a4) within a range not impairing the effects of the present invention.

[0148] Examples of the component (a5) include (meth)acrylic acid alkyl esters having an alkyl group having 1 to 20 carbon atoms; vinyl compounds such as styrene, hydroxyethyl vinyl ether, hydroxybutyl vinyl ether, N-vinylformamide, N-vinylpyrrolidone, and N-vinylcaprolactam.

[0149] In addition, the component (a5) may be used individually by 1 type, or may use 2 or more types together.

[0150] The content of the component (a5) in the buffer layer-forming composition is preferably 0 to 20% by mass, more preferably 0 to 10% by mass, further preferably 0 to 5% by mass, and still further preferably 0 to 2% by mass.

[0151] (Photopolymerization Initiator)

[0152] The buffer layer-forming composition preferably further contains a photopolymerization initiator from the viewpoint of shortening the polymerization time by light irradiation and reducing the light irradiation amount when forming the buffer layer.

[0153] Examples of the photopolymerization initiator include benzoin compounds, acetophenone compounds, acylphosphine oxide compounds, titanocene compounds, thioxanthone compounds, peroxide compounds, and photosensitizers such as amines and quinones. More specifically, examples include 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzyl phenyl sulfide, tetramethylthiuram monosulfide, azobisisobutyronitrile, bibenzyl, diacetyl, β-chloroanthraquinone, and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.

[0154] These photopolymerization initiators may be used alone or in combination of two or more.

[0155] The content of the photopolymerization initiator in the buffer layer-forming composition is preferably 0.05 to 15 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 0.3 to 5 parts by mass, based on 100 parts by mass of the total amount of the energy ray-polymerizable compounds.

[0156] (Other additives)

[0157] The buffer layer forming composition may also contain other additives within the range that does not damage the effect of the present invention. As other additives, for example, one or more selected from antistatic agents, antioxidants, softeners (plasticizers), fillers, rust inhibitors, pigments, dyes, etc. can be cited. In the case of coordinating these additives, the content of each additive in the buffer layer forming composition is preferably 0.01 to 6 parts by mass, more preferably 0.1 to 3 parts by mass relative to 100 parts by mass of the total amount of the energy ray polymerizable compound.

[0158] (Resin component)

[0159] The buffer layer forming composition may contain a resin component within a range that does not impair the effects of the present invention. Examples of the resin component include polyene-thiol resins, polyolefin resins such as polybutene, polybutadiene, and polymethylpentene, and thermoplastic resins such as styrene copolymers.

[0160] The content of these resin components in the buffer layer-forming composition is preferably 0 to 20% by mass, more preferably 0 to 10% by mass, further preferably 0 to 5% by mass, and still further preferably 0 to 2% by mass.

[0161] The buffer layer formed of the buffer layer forming composition containing an energy ray polymerizable compound can be obtained by polymerizing and curing the buffer layer forming composition of the above composition by energy ray irradiation. That is, the buffer layer is a cured product of the buffer layer forming composition.

[0162] Therefore, the buffer layer contains polymerized units from component (a1). In addition, the buffer layer preferably contains at least one of polymerized units from component (a2) and polymerized units from component (a3). In addition, the buffer layer may contain at least one of polymerized units from component (a4) and polymerized units from component (a5).

[0163] The content ratio of each polymerized unit in the buffer layer is usually consistent with the ratio (feed ratio) of each component constituting the buffer layer forming composition. For example, when the content of component (a1) in the buffer layer forming composition is 10% to 70% by mass relative to the total amount (100% by mass) of the buffer layer forming composition, the buffer layer contains 10% to 70% by mass of polymerized units from component (a1). In addition, when the content of component (a2) in the buffer layer forming composition is 10% to 80% by mass relative to the total amount (100% by mass) of the buffer layer forming composition, the buffer layer contains 10% to 80% by mass of polymerized units from component (a2). The same is true for components (a3) ​​to (a5).

[0164] When the buffer layer is a cured product of a buffer layer-forming composition containing an energy-ray-polymerizable compound, the breaking energy of the buffer layer at 23° C. can be controlled, for example, by adjusting the weight average molecular weight of the above-mentioned urethane (meth)acrylate (a1), the thickness of the buffer layer, and appropriately selecting the type of monomer.

[0165] [Base material]

[0166] The substrate functions as a support for the pressure-sensitive adhesive tape.

[0167] As the substrate, various resin films can be cited. Specifically, a resin film formed by one or more of polyethylene selected from low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), high-density polyethylene (HDPE), polypropylene, polybutene, polybutadiene, polymethylpentene, ethylene-norbornene copolymer, norbornene resin, etc.; ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylate copolymer, etc.; polyvinyl chloride, vinyl chloride copolymer, etc.; polyesters such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, and wholly aromatic polyester; polyurethane, polyimide, polyamide, polycarbonate, fluororesin, polyacetal, modified polyphenylene ether, polyphenylene sulfide, polysulfone, polyether ketone, acrylic polymer, etc. can be cited. In addition, modified films such as their cross-linked films and ionomer films can also be used. The substrate may be a single-layer film of a resin film formed of one or more resins selected from these resins, or may be a laminated film in which two or more of these resin films are laminated.

[0168] It should be noted that the substrate is harder than the buffer layer and is therefore less likely to have rough cut surfaces when cut with a tool than the buffer layer. From the perspective of obtaining a substrate with better cuttability with a tool, the substrate preferably satisfies the following requirement (γ).

[0169] · Requirement (γ): Fracture strain at 23°C (ε 100 ) and the fracture stress (ρ 100 ) is greater than 60MPa.

[0170] The elastic modulus of the substrate at 23° C. is preferably 200 MPa or more, more preferably 500 MPa or more, and further preferably 1000 MPa or more. It is preferably 30000 MPa or less, more preferably 10000 MPa or less, and further preferably 6000 MPa or less.

[0171] The thickness of the substrate is not particularly limited, but is preferably 110 μm or less, more preferably 15 μm to 110 μm, and further preferably 20 μm to 105 μm. By making the thickness of the substrate 110 μm or less, it is easy to control the peeling force of the adhesive tape. In addition, by making the thickness of the substrate 15 μm or more, the substrate is easy to function as a support for the adhesive tape.

[0172] In addition, the substrate may contain a plasticizer, a lubricant, an infrared absorber, an ultraviolet absorber, a filler, a colorant, an antistatic agent, an antioxidant, a catalyst, etc. within the range that does not impair the effect of the present invention. In addition, the substrate may be transparent or opaque, and may be colored or vapor-deposited as desired.

[0173] In order to improve the adhesion with at least one of the buffer layer and the adhesive layer, at least one surface of the substrate may be subjected to an adhesive treatment such as a corona treatment. In addition, the substrate may have the above-mentioned resin film and an easy-adhesion layer coated on at least one surface of the resin film.

[0174] The composition for forming the easy-adhesion layer is not particularly limited, and examples thereof include compositions containing polyester resins, urethane resins, polyester urethane resins, acrylic resins, etc. The composition for forming the easy-adhesion layer may also contain a crosslinking agent, a photopolymerization initiator, an antioxidant, a softener (plasticizer), a filler, a rust inhibitor, a pigment, a dye, etc. as required.

[0175] As the thickness of the easy bonding layer, preferably 0.01 μm to 10 μm, more preferably 0.03 μm to 5 μm. It should be noted that the thickness of the easy bonding layer in the embodiment of the present application is relatively small relative to the thickness of the substrate, therefore, the thickness of the resin film with the easy bonding layer is substantially the same as the thickness of the substrate. In addition, since the material of the easy bonding layer is soft, therefore, the influence on the elastic modulus is small, and the elastic modulus of the substrate is also substantially the same as the Young's modulus of the resin film when having the easy bonding layer.

[0176] For example, the fracture strain (ε) at a temperature of 23°C specified in requirement (γ) 100 ) and the fracture stress (ρ 100 ) product, and the elastic modulus of the substrate can be controlled by the selection of the resin composition, the addition of the plasticizer, the stretching conditions during the manufacture of the resin film, etc. Specifically, when a polyethylene terephthalate film is used as the substrate, when the proportion of the ethylene component in the copolymerization component increases, there is a tendency that the elastic modulus of the substrate decreases. In addition, when the amount of the plasticizer increases relative to the resin composition constituting the substrate, there is a tendency that the elastic modulus of the substrate decreases.

[0177] [Adhesive layer]

[0178] The adhesive layer is not particularly limited as long as it has moderate pressure-sensitive adhesiveness at room temperature, and the shear storage modulus at 23°C is preferably 0.05MPa to 0.50MPa. Circuits are formed on the surface of semiconductor wafers, etc., and they usually have bumps. By making the shear storage modulus of the adhesive layer within the above range, when the adhesive tape is pasted on the surface of the wafer with bumps, the bumps on the wafer surface can be fully contacted with the adhesive layer, and the adhesion of the adhesive layer can be properly exerted. Therefore, the adhesive tape can be reliably fixed to the semiconductor wafer, and the wafer surface can be properly protected during back grinding. From these viewpoints, the shear storage modulus of the adhesive layer is more preferably 0.12 to 0.35MPa. It should be noted that, in the case where the adhesive layer is formed by an energy-ray-curable adhesive, the shear storage modulus of the adhesive layer refers to the shear storage modulus before curing by energy-ray irradiation.

[0179] The shear storage modulus can be measured by the following method. An adhesive layer having a thickness of about 0.5 to 1 mm is punched into a circle having a diameter of 7.9 mm to prepare a measurement sample. A dynamic viscoelasticity measuring device ARES manufactured by Rheometric Corporation is used to measure the elastic modulus of the measurement sample at a temperature range of -30°C to 150°C at a temperature increase rate of 3°C / min at a frequency of 1 Hz. The elastic modulus at a measurement temperature of 23°C is taken as the shear storage modulus at 23°C.

[0180] The thickness of the adhesive layer is preferably less than 100 μm, more preferably 5 to 80 μm, and even more preferably 10 to 70 μm. When the adhesive layer is thinned in this way, the generation of chips during cutting of the adhesive tape can be suppressed, and the cracking of the semiconductor chip during back grinding can be easily prevented.

[0181] The adhesive layer can be formed of, for example, an acrylic adhesive, a urethane adhesive, a rubber adhesive, a silicone adhesive, etc., and is preferably an acrylic adhesive.

[0182] In addition, the adhesive layer is preferably formed of an energy-ray-curable adhesive. By forming the adhesive layer of an energy-ray-curable adhesive, the shear storage modulus at 23° C. can be set to the above range before curing by energy-ray irradiation, and the peeling force can be easily set to 1000 mN / 50 mm or less after curing.

[0183] Specific examples of the adhesive are described in detail below, but these are non-limiting examples, and the adhesive layer in the present invention is not to be interpreted in a limiting sense.

[0184] As the energy-ray-curable adhesive, for example, in addition to the non-energy-ray-curable adhesive resin (also referred to as "adhesive resin I"), an energy-ray-curable adhesive composition containing an energy-ray-curable compound other than the adhesive resin (hereinafter also referred to as "X-type adhesive composition") can also be used. In addition, as the energy-ray-curable adhesive, an adhesive composition containing an energy-ray-curable adhesive resin having an unsaturated group introduced into the side chain of the non-energy-ray-curable adhesive resin (hereinafter also referred to as "adhesive resin II") as a main component and not containing an energy-ray-curable compound other than the adhesive resin (hereinafter also referred to as "Y-type adhesive composition") can also be used.

[0185] In addition, as an energy-ray-curable adhesive, in addition to the energy-ray-curable adhesive resin II that contains a combination of X-type and Y-type, an energy-ray-curable adhesive composition (hereinafter also referred to as "XY-type adhesive composition") that also contains energy-ray-curable compounds other than the adhesive resin can be used.

[0186] Among them, an XY type adhesive composition is preferably used. By using an XY type adhesive composition, sufficient adhesive properties can be obtained before curing, and on the other hand, the peeling force with respect to the semiconductor wafer can be sufficiently reduced after curing.

[0187] Among them, as an adhesive, it can be formed by a non-energy ray-curable adhesive composition that does not cure even when irradiated with energy rays. The non-energy ray-curable adhesive composition contains at least a non-energy ray-curable adhesive resin I, and on the other hand, does not contain the above-mentioned energy ray-curable adhesive resin II and energy ray-curable compound.

[0188] It should be noted that, in the following description, "adhesive resin" is used as a term to represent one or both of the above-mentioned adhesive resin I and adhesive resin II. Specific examples of the adhesive resin include acrylic resin, urethane resin, rubber resin, silicone resin, etc., preferably acrylic resin.

[0189] Hereinafter, an acrylic pressure-sensitive adhesive using an acrylic resin as the adhesive resin will be described in more detail.

[0190] <Acrylic resin>

[0191] The acrylic resin may use an acrylic polymer (b). The acrylic polymer (b) is obtained by polymerizing a monomer containing at least an alkyl (meth)acrylate, and contains a structural unit derived from the alkyl (meth)acrylate. Examples of the alkyl (meth)acrylate include alkyl (meth)acrylates having an alkyl group with 1 to 20 carbon atoms, and the alkyl group may be a linear chain or a branched chain. Specific examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, and dodecyl (meth)acrylate. The alkyl (meth)acrylate may be used alone or in combination of two or more.

[0192] In addition, from the viewpoint of improving the adhesive strength of the pressure-sensitive adhesive layer, the acrylic polymer (b) preferably contains a structural unit derived from an alkyl (meth)acrylate having an alkyl group with 4 or more carbon atoms. The alkyl (meth)acrylate preferably has 4 to 12 carbon atoms, and more preferably has 4 to 6 carbon atoms. The alkyl (meth)acrylate having an alkyl group with 4 or more carbon atoms is preferably an alkyl acrylate.

[0193] In the acrylic polymer (b), the (meth)acrylic acid alkyl ester having an alkyl group with 4 or more carbon atoms is preferably 40 to 98% by mass, more preferably 45 to 95% by mass, and even more preferably 50 to 90% by mass, based on the total amount of monomers constituting the acrylic polymer (b) (hereinafter, also simply referred to as "total amount of monomers").

[0194] In order to adjust the elastic modulus and adhesive properties of the adhesive layer, the acrylic polymer (b) is preferably a copolymer containing structural units derived from an alkyl (meth)acrylate having 1 to 3 carbon atoms in addition to structural units derived from an alkyl (meth)acrylate having 4 or more carbon atoms in the alkyl group. It should be noted that the alkyl (meth)acrylate is preferably an alkyl (meth)acrylate having 1 or 2 carbon atoms, more preferably methyl (meth)acrylate, and further preferably methyl methacrylate. In the acrylic polymer (b), the alkyl (meth)acrylate having 1 to 3 carbon atoms in the alkyl group is preferably 1% to 30% by mass, more preferably 3% to 26% by mass, and further preferably 6% to 22% by mass relative to the total amount of the monomers.

[0195] Preferably, the acrylic polymer (b) has a structural unit derived from a monomer containing a functional group in addition to the structural unit derived from the (meth) alkyl ester described above. Examples of the functional group of the monomer containing a functional group include a hydroxyl group, a carboxyl group, an amino group, an epoxy group, etc. The monomer containing a functional group can react with a crosslinking agent described later to become a crosslinking starting point, or react with a compound containing an unsaturated group to introduce an unsaturated group into the side chain of the acrylic polymer (b).

[0196] As the monomer containing a functional group, there can be listed: a monomer containing a hydroxyl group, a monomer containing a carboxyl group, a monomer containing an amino group, a monomer containing an epoxy group, etc. These monomers can be used alone or in combination of two or more. Among them, preferably a monomer containing a hydroxyl group, a monomer containing a carboxyl group, and more preferably a monomer containing a hydroxyl group.

[0197] Examples of the hydroxyl group-containing monomer include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and unsaturated alcohols such as vinyl alcohol and allyl alcohol.

[0198] Examples of the carboxyl group-containing monomer include ethylenically unsaturated monocarboxylic acids such as (meth)acrylic acid and crotonic acid; ethylenically unsaturated dicarboxylic acids such as fumaric acid, itaconic acid, maleic acid, and citraconic acid and their anhydrides; and 2-carboxyethyl methacrylate.

[0199] The amount of the monomer containing a functional group is preferably 1 to 35% by mass, more preferably 3 to 32% by mass, and even more preferably 6 to 30% by mass, based on the total amount of monomers constituting the acrylic polymer (b).

[0200] In addition to the above, the acrylic polymer (b) may contain structural units derived from monomers copolymerizable with the above acrylic monomers, such as styrene, α-methylstyrene, vinyltoluene, vinyl formate, vinyl acetate, acrylonitrile, and acrylamide.

[0201] The acrylic polymer (b) can be used as a non-energy ray-curable adhesive resin I (acrylic resin). In addition, as an energy ray-curable acrylic resin, there can be mentioned an acrylic resin obtained by reacting a compound having a photopolymerizable unsaturated group (also referred to as an unsaturated group-containing compound) with a functional group of the acrylic polymer (b).

[0202] The compound containing an unsaturated group is a compound having both a substituent capable of bonding to the functional group of the acrylic polymer (b) and a photopolymerizable unsaturated group. Examples of the photopolymerizable unsaturated group include (meth)acryloyl, vinyl, allyl, vinylbenzyl, etc., preferably (meth)acryloyl.

[0203] In addition, as the substituent capable of bonding to the functional group possessed by the compound containing an unsaturated group, there can be mentioned an isocyanate group, a glycidyl group, etc. Therefore, as the compound containing an unsaturated group, there can be mentioned, for example: (meth)acryloyloxyethyl isocyanate, (meth)acryloyl isocyanate, (meth)glycidyl (meth)acrylate, etc.

[0204] In addition, the unsaturated group-containing compound is preferably reacted with a part of the functional groups of the acrylic polymer (b). Specifically, the unsaturated group-containing compound is preferably reacted with 50 to 98 mol % of the functional groups of the acrylic polymer (b), and more preferably reacted with 55 to 93 mol %. In this way, in the energy-ray-curable acrylic resin, a part of the functional groups is not reacted with the unsaturated group-containing compound and remains, so that crosslinking by a crosslinking agent is easy.

[0205] The weight average molecular weight (Mw) of the acrylic resin is preferably 300,000 to 1,600,000, more preferably 400,000 to 1,400,000, and even more preferably 500,000 to 1,200,000.

[0206] <Energy beam curable compound>

[0207] The energy-ray-curable compound contained in the X-type or XY-type adhesive composition is preferably a monomer or oligomer having an unsaturated group in the molecule and capable of being polymerized and cured by energy-ray irradiation.

[0208] Examples of such energy-ray-curable compounds include poly(meth)acrylate monomers such as trimethylolpropane tri(meth)acrylate, pentaerythritol (meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4-butanediol di(meth)acrylate, and 1,6-hexanediol (meth)acrylate, and oligomers such as urethane (meth)acrylate, polyester (meth)acrylate, polyether (meth)acrylate, and epoxy (meth)acrylate.

[0209] Among these, urethane (meth)acrylate oligomers are preferred because they have a relatively high molecular weight and are less likely to cause a decrease in the shear storage modulus of the pressure-sensitive adhesive layer.

[0210] The molecular weight (in the case of an oligomer, weight average molecular weight) of the energy beam curable compound is preferably 100 to 12,000, more preferably 200 to 10,000, further preferably 400 to 8,000, and further preferably 600 to 6,000.

[0211] The content of the energy-ray curable compound in the X-type adhesive composition is preferably 40 to 200 parts by mass, more preferably 50 to 150 parts by mass, and even more preferably 60 to 90 parts by mass based on 100 parts by mass of the adhesive resin.

[0212] On the other hand, the content of the energy-ray curable compound in the XY-type adhesive composition is preferably 1 to 30 parts by mass, more preferably 2 to 20 parts by mass, and further preferably 3 to 15 parts by mass relative to 100 parts by mass of the adhesive resin. In the XY-type adhesive composition, since the adhesive resin is energy-ray curable, even if the content of the energy-ray curable compound is small, the peeling force can be sufficiently reduced after energy-ray irradiation.

[0213] <Cross-linking agent>

[0214] The adhesive composition preferably further contains a crosslinking agent. The crosslinking agent, for example, reacts with a functional group of a monomer containing a functional group possessed by the adhesive resin, thereby crosslinking the adhesive resins with each other. Examples of the crosslinking agent include isocyanate crosslinking agents such as toluene diisocyanate, hexamethylene diisocyanate, and their adducts; epoxy crosslinking agents such as ethylene glycol glycidyl ether; aziridine crosslinking agents such as hexa[1-(2-methyl)-aziridine]triphosphatriazine; chelate crosslinking agents such as aluminum chelates; etc. These crosslinking agents can be used alone or in combination of two or more.

[0215] Among them, isocyanate crosslinking agents are preferred from the viewpoints of improving cohesive force to improve adhesive force and from the viewpoint of easy availability.

[0216] From the viewpoint of promoting the crosslinking reaction, the amount of the crosslinking agent is preferably 0.01 to 10 parts by mass, more preferably 0.03 to 7 parts by mass, and even more preferably 0.05 to 4 parts by mass based on 100 parts by mass of the adhesive resin.

[0217] <Photopolymerization initiator>

[0218] In addition, when the adhesive composition is energy-ray-curable, it is preferred that the adhesive composition further contain a photopolymerization initiator. By containing a photopolymerization initiator, the curing reaction of the adhesive composition can be sufficiently carried out even by energy rays with relatively low energy such as ultraviolet rays.

[0219] As the photopolymerization initiator, for example, benzoin compounds, acetophenone compounds, acylphosphine oxide compounds, titanocene compounds, thioxanthone compounds, peroxide compounds, and photosensitizers such as amines and quinones, etc., more specifically, for example, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzyl phenyl sulfide, tetramethylthiuram monosulfide, azobisisobutyronitrile, bibenzyl, diacetyl, 8-chloroanthraquinone, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, etc.

[0220] These photopolymerization initiators may be used alone or in combination of two or more.

[0221] The amount of the photopolymerization initiator to be added is preferably 0.01 to 10 parts by mass, more preferably 0.03 to 5 parts by mass, and even more preferably 0.05 to 5 parts by mass, based on 100 parts by mass of the adhesive resin.

[0222] <Other additives>

[0223] The adhesive composition may also contain other additives within the scope of not impairing the effect of the present invention. As other additives, for example, antistatic agents, antioxidants, softeners (plasticizers), fillers, rust inhibitors, pigments, dyes, etc. can be cited. When these additives are used, the amount of the additives is preferably 0.01 to 6 parts by mass relative to 100 parts by mass of the adhesive resin.

[0224] In addition, from the viewpoint of improving coating properties on a substrate, a cushion layer, or a release sheet, the adhesive composition may be further diluted with an organic solvent to be in the form of a solution of the adhesive composition.

[0225] Examples of the organic solvent include methyl ethyl ketone, acetone, ethyl acetate, tetrahydrofuran, Alkane, cyclohexane, n-hexane, toluene, xylene, n-propanol, isopropanol, etc.

[0226] The organic solvent used in the synthesis of the adhesive resin may be used as such, or one or more organic solvents other than the organic solvent used in the synthesis may be added to achieve uniform coating of the adhesive composition solution.

[0227] [Peel sheet]

[0228] The surface of the adhesive tape may be attached with a release sheet. Specifically, the release sheet may be attached to the surface of the adhesive layer of the adhesive tape. The release sheet is attached to the surface of the adhesive layer to protect the adhesive layer during transportation and storage. The release sheet is attached to the adhesive tape in a removable manner and is removed by peeling from the adhesive tape before using the adhesive tape (i.e., before attaching the wafer).

[0229] The release sheet may be a release sheet at least one surface of which has been subjected to a release treatment. Specifically, the release sheet may be a release sheet obtained by coating a release agent on the surface of a release sheet substrate.

[0230] As the release sheet substrate, a resin film is preferred, and examples of the resin constituting the resin film include polyester resin films such as polyethylene terephthalate resin, polybutylene terephthalate resin, and polyethylene naphthalate resin, and polyolefin resins such as polypropylene resin and polyethylene resin. Examples of the release agent include rubber elastomers such as silicone resins, olefin resins, isoprene resins, and butadiene resins, long-chain alkyl resins, alkyd resins, and fluorine resins.

[0231] The thickness of the release sheet is not particularly limited, but is preferably 10 μm to 200 μm, more preferably 20 μm to 150 μm.

[0232] [Method for producing adhesive tape for semiconductor processing]

[0233] The method for producing the pressure-sensitive adhesive tape for semiconductor processing of the present invention is not particularly limited, and the pressure-sensitive adhesive tape can be produced by a known method.

[0234] For example, a method for producing a pressure-sensitive adhesive tape having a laminated structure in which a cushion layer, a substrate, and a pressure-sensitive adhesive layer are laminated in this order is as follows.

[0235] When the buffer layer is formed of a buffer layer-forming composition containing an energy-ray-polymerizable compound, the buffer layer formed by coating the buffer layer-forming composition on a release sheet and curing the composition can be laminated to a substrate and the release sheet can be removed to obtain a laminate of the buffer layer and the substrate.

[0236] Then, the adhesive layer provided on the release sheet can be bonded to the substrate side of the laminate to produce an adhesive tape having the release sheet bonded to the surface of the adhesive layer. The release sheet bonded to the surface of the adhesive layer can be appropriately peeled off and removed before using the adhesive tape.

[0237] As a method for forming a buffer layer on a release sheet, a buffer layer-forming composition can be directly coated on the release sheet using a known coating method to form a coating film, and the coating film is irradiated with energy rays to form the buffer layer. Alternatively, the buffer layer can be formed by directly coating a buffer layer-forming composition on one side of the substrate and heating and drying it or irradiating the coating film with energy rays.

[0238] As the coating method of the buffer layer forming composition, for example, spin coating, spray coating, rod coating, knife coating, roll coating, blade coating, die coating, gravure coating, etc. can be listed. In addition, in order to improve the coating property, an organic solvent can be combined with the buffer layer forming composition and applied on the release sheet in the form of a solution.

[0239] In the case where the buffer layer forming composition includes an energy ray polymerizable compound, it is preferably cured by irradiating the coating film of the buffer layer forming composition with energy rays to form a buffer layer. The curing of the buffer layer can be carried out by a single curing treatment, or it can be carried out in multiple times. For example, the coating film on the release sheet can be completely cured to form a buffer layer and then attached to the substrate, or the coating film can be formed without completely curing the coating film to form a semi-cured buffer layer. After the buffer layer is attached to the substrate, the energy ray is irradiated again to completely cure it to form a buffer layer. As the energy ray irradiated in the curing treatment, ultraviolet rays are preferably used. It should be noted that when curing, the coating film of the buffer layer forming composition can also be exposed, but it is preferably covered with a release sheet and a substrate to cover the coating film, and the coating film is irradiated with energy rays in a non-exposed state to cure.

[0240] As a method for forming the adhesive layer on the release sheet, the adhesive layer can be formed by directly applying the adhesive (adhesive composition) on the release sheet by a known coating method and then heating and drying the coated film.

[0241] In addition, adhesive (adhesive composition) can be directly applied on one side of substrate to form adhesive layer. As the coating method of adhesive, spray coating, rod coating, knife coating, roll coating, scraper coating, die coating, gravure coating etc. shown in the manufacture method of buffer layer can be enumerated.

[0242] [How to use adhesive tape for semiconductor processing]

[0243] The adhesive tape for semiconductor processing of the present invention can be adhered to the surface (circuit formation surface) of a semiconductor wafer when grinding the back surface of the semiconductor wafer, and can be used by cutting along the outer periphery of the semiconductor wafer.

[0244] In one embodiment of the present invention, the adhesive tape for semiconductor processing of the present invention can be adhered to the surface (circuit forming surface) of a semiconductor wafer when the back side of the semiconductor wafer is ground (more specifically, when a semiconductor chip is manufactured including a back side grinding process of the semiconductor wafer), and can be cut along the periphery of the semiconductor wafer for use.

[0245] Examples of a method for manufacturing a semiconductor chip including a backside grinding step of a semiconductor wafer include a method of grinding the backside of a semiconductor wafer and then dicing the semiconductor wafer into individual pieces, and the above-mentioned DBG or a modified DBG method.

[0246] The semiconductor processing adhesive tape of the present invention has excellent cutting properties by a cutter. Therefore, when the semiconductor processing adhesive tape is cut along the periphery of a semiconductor wafer, it is difficult to generate chips, and during the manufacture of semiconductor chips including a back grinding process of the semiconductor wafer, the occurrence of defects and breakage of the semiconductor chip caused by the chips can be suppressed.

[0247] Therefore, in one embodiment of the present invention, the following method of use (1) or (2) can be provided.

[0248] (1) A method for using the adhesive tape for semiconductor processing of the present invention, the method comprising: attaching the adhesive tape for semiconductor processing to the surface of a semiconductor wafer when back grinding the semiconductor wafer, and cutting the adhesive tape for semiconductor processing along the outer periphery of the semiconductor wafer.

[0249] (2) In the method of use of (1) above, as the semiconductor wafer, a semiconductor wafer having grooves formed on the surface side or a semiconductor wafer having a reformed region formed inside is used.

[0250] [Method for manufacturing semiconductor device]

[0251] The manufacturing method of the semiconductor device of the present invention is a manufacturing method of a semiconductor chip including a back grinding process of a semiconductor wafer, the method including a process (S1): adhering the semiconductor processing adhesive tape of the present invention to the surface (circuit forming surface) of the semiconductor wafer, and cutting the semiconductor processing adhesive tape along the outer periphery of the semiconductor wafer.

[0252] The adhesive tape for semiconductor processing of the present invention has excellent cutting properties by a cutter. Therefore, in the above step (S1), cutting chips are less likely to be generated, and the occurrence of cracks in the semiconductor chip caused by the cutting chips can be suppressed.

[0253] The process schematic diagram of the method for manufacturing a semiconductor device of the present invention is shown in Figure 2 .

[0254] The manufacturing method of the semiconductor device of the present invention generally includes: a process (S1) of sticking a semiconductor processing adhesive tape to the surface (circuit forming surface) of a semiconductor chip, and cutting the semiconductor processing adhesive tape along the outer periphery of the semiconductor chip; and a process (S2) of grinding the semiconductor chip from the back side.

[0255] The semiconductor wafer may be diced into individual pieces after the step (S2) (method 1).

[0256] In addition, the semiconductor wafer may be singulated in step (S2) (method 2).

[0257] Specifically, as the semiconductor wafer, a semiconductor wafer having grooves formed on the surface side may be used, and in step (S2), the semiconductor wafer is singulated into a plurality of chips using the grooves as starting points.

[0258] In addition, as the above-mentioned semiconductor chip, a semiconductor chip having a modified region formed inside can be used, or a modified region is formed inside the above-mentioned semiconductor chip after the above-mentioned process (S1), and in process (S2), the above-mentioned semiconductor chip is singulated into multiple chips with the modified region as the starting point.

[0259] Hereinafter, each step will be described in detail.

[0260] <Step (S1)>

[0261] In step (S1), the adhesive tape for semiconductor processing of the present invention is attached to the surface (circuit formation surface) of a semiconductor wafer, and the adhesive tape for semiconductor processing is cut along the outer periphery of the semiconductor wafer.

[0262] The semiconductor processing adhesive tape is pasted in a manner that covers the surface (circuit forming surface) of the semiconductor wafer and the peripheral workbench extending to the periphery thereof. Then, the semiconductor processing adhesive tape is cut along the periphery of the semiconductor wafer by cutting from the surface of the buffer layer side using a cutter such as a cutter. The cutting speed is usually 10 to 300 mm / s. The temperature of the cutter during cutting can be room temperature, and the cutter can also be heated and cut.

[0263] Examples of the semiconductor wafer used in the present production method include silicon wafers, gallium arsenic wafers, silicon carbide wafers, lithium tantalate wafers, lithium niobate wafers, gallium nitride wafers, indium phosphide wafers, and glass wafers.

[0264] The thickness of the semiconductor wafer before back grinding is not particularly limited, but is usually about 500 μm to 1000 μm.

[0265] In addition, circuit formation on the surface of a semiconductor wafer can be performed by various methods including conventionally used methods such as etching and lift-off.

[0266] When DBG is used in the present production method, the semiconductor wafer to which the adhesive tape for semiconductor processing is attached in step (S1) is a semiconductor wafer having grooves formed on the surface.

[0267] A semiconductor wafer having grooves formed on its surface can be produced by laser dicing, blade dicing, etc. using a conventionally known wafer dicing device, etc. The grooves serve as a starting point for dividing the semiconductor wafer into individual pieces to form semiconductor chips.

[0268] When the DBG modification method is adopted in the present manufacturing method, the semiconductor wafer to which the semiconductor processing adhesive tape is attached in step (S1) is a semiconductor wafer having a modified region formed therein. The modified region may be formed after step (S1).

[0269] The reformed region is a brittle portion in the semiconductor wafer and serves as a starting point for division when the semiconductor wafer is separated into semiconductor chips.

[0270] A semiconductor wafer having a modified region formed therein can be produced by irradiating a laser or plasma focused on the inside of the semiconductor wafer. The irradiation of the laser or plasma can be performed from the front side or the back side of the semiconductor wafer.

[0271] The semiconductor wafer with the semiconductor processing adhesive tape that has completed the step (S1) is placed on the chuck table and is adsorbed and held on the chuck table. At this time, the semiconductor wafer with the semiconductor processing adhesive tape is placed on the chuck table in direct contact with the chuck table and the buffer layer of the semiconductor processing adhesive tape. That is, the surface side of the semiconductor wafer is arranged on the chuck table side.

[0272] <Method 1>

[0273] In method 1, after step ( S2 ) is performed, step ( S3 ) is performed to separate the semiconductor wafer into pieces.

[0274] In the first aspect, a semiconductor wafer having no division starting point, such as a semiconductor wafer having grooves formed on the surface or a semiconductor wafer having a reformed region formed inside, is not used. Instead, a semiconductor wafer having no division starting point is used.

[0275] (Step (S2))

[0276] In step (2), the back surface of the semiconductor wafer on the chuck table is ground.

[0277] The thickness of the semiconductor wafer after back grinding is not particularly limited, but is preferably about 5 μm to 100 μm, more preferably 10 μm to 45 μm.

[0278] (Step (S3))

[0279] In step (S3), the semiconductor wafer subjected to step (S2) is diced into individual pieces. The dicing can be appropriately performed by a conventionally known method such as blade dicing or laser dicing.

[0280] The shape of the semiconductor chip after singulation may be square or elongated such as rectangular. The thickness of the semiconductor chip after singulation is not particularly limited, but is preferably about 5 μm to 100 μm, more preferably 10 μm to 45 μm.

[0281] The area of ​​the semiconductor chip after singulation is not particularly limited, but is preferably less than 600 mm 2 , more preferably less than 400mm 2 , further preferably less than 300mm 2 .

[0282] <Method 2>

[0283] In the method 2, the back side of the semiconductor wafer is ground in the step (S2) to separate the semiconductor wafer into individual pieces.

[0284] (Step (S2))

[0285] In step (S2), the back surface of the semiconductor wafer on the chuck table is ground to separate the semiconductor wafer into a plurality of semiconductor chips.

[0286] Here, in the first embodiment of the second embodiment, a semiconductor wafer having grooves formed on the surface can be used. In this case, the back surface of the semiconductor wafer is ground until at least the bottom of the groove is reached. By the back surface grinding, the groove becomes a cut that penetrates the semiconductor wafer, and the semiconductor wafer is divided by the cut to be singulated into individual semiconductor chips.

[0287] In addition, in the second embodiment of the second mode, a semiconductor wafer having a modified region formed therein can be used. Alternatively, a modified region can be formed inside the semiconductor wafer after the above step (S1). In the second embodiment of the second mode, back grinding can be performed until the modified region is reached, or it can be performed without strictly reaching the modified region. That is, back grinding can be performed until the position close to the modified region is reached, so that the semiconductor wafer is destroyed starting from the modified region and singulated into semiconductor chips.

[0288] Furthermore, the plurality of semiconductor chips thus obtained may be attached to a pickup tape, which will be described later, and then the pickup tape may be stretched to expand the gaps between the chips.

[0289] In addition, dry polishing may be performed after the back grinding is completed and before the chip is picked up.

[0290] The shape, thickness, and area of ​​the semiconductor chips after singulation are as described in Embodiment 1.

[0291] In addition, when using a semiconductor wafer having a reformed region formed therein, it is easy to make the thickness of the semiconductor chip after singulation 50 μm or less, more preferably 10 μm to 45 μm.

[0292] The semiconductor processing adhesive tape of the present invention has excellent cutter-based cutting properties. Therefore, in the above-mentioned step (S1), it is not easy to generate chips. Therefore, in the step (S2) of mode 1 and the step (S2) of mode 2, even when a thinned / miniaturized semiconductor chip is manufactured, the occurrence of defects and damage to the semiconductor chip caused by the chips can be suppressed.

[0293] <Peeling of adhesive tape for semiconductor processing>

[0294] After step ( S2 ), the adhesive tape for semiconductor processing is peeled off from the individualized semiconductor wafer (ie, a plurality of semiconductor chips).

[0295] This step is performed, for example, by the following method.

[0296] In the case where the adhesive layer of the adhesive tape for semiconductor processing is formed of an energy-ray-curable adhesive, the adhesive layer is cured by irradiating with energy rays. Next, a pick-up tape is attached to the back side of the singulated semiconductor wafer, and the position and direction are aligned in a manner that the wafer can be picked up. At this time, the annular frame arranged on the outer peripheral side of the wafer is also attached to the pick-up tape, and the outer peripheral edge of the pick-up tape is fixed to the annular frame. The wafer and the annular frame can be attached to the pick-up tape at the same time, or at different times. Next, the adhesive tape is peeled off from the plurality of semiconductor chips held on the pick-up tape.

[0297] Then, the plurality of semiconductor chips on the pickup tape are picked up and fixed on a substrate or the like to manufacture a semiconductor device. It should be noted that the pickup tape is not particularly limited, and for example, may be composed of an adhesive tape having a base material and an adhesive layer provided on at least one side of the base material.

[0298] In addition, an adhesive tape may be used instead of the pickup tape. Examples of the adhesive tape include a laminate of a film adhesive and a release sheet, a laminate of a dicing tape and a film adhesive, and a dicing / die bonding tape having the functions of both a dicing tape and a die bonding tape and composed of an adhesive layer and a release sheet. In addition, before attaching the pickup tape, a film adhesive may be attached to the back side of the singulated semiconductor wafer. When a film adhesive is used, the film adhesive may be in the same shape as the wafer.

[0299] When using an adhesive tape, or when a film adhesive is applied to the back side of the singulated semiconductor wafer before attaching the pickup tape, multiple semiconductor chips on the adhesive tape or the pickup tape can be picked up together with the adhesive layer divided into the same shape as the semiconductor chip. Then, the semiconductor chip is fixed to a substrate or the like via the adhesive layer to manufacture a semiconductor device. The division of the adhesive layer can be performed by laser or wafer expansion.

[0300] The semiconductor device manufacturing method of the present invention has been described above. The semiconductor processing adhesive tape of the present invention can be particularly preferably used for a DBG deformation method for obtaining a semiconductor chip group with a small groove width and further thinning when singulating a semiconductor wafer.

[0301] It should be noted that the semiconductor processing adhesive tape of the present invention can also be used to temporarily hold the workpiece during processing of glass, ceramics, etc. It can also be used as various removable adhesive tapes.

[0302] Example

[0303] The present invention will be specifically described with reference to the following examples, but the present invention is not limited to the following examples.

[0304] [Manufacturing Examples A1 to A4, Comparative Manufacturing Examples B1 to B3, Reference Examples C1 to C2]

[0305] <Production Example A1: Formation of Buffer Layer A-1>

[0306] A composition for a buffer layer was obtained by adding 2.0 parts by mass of a photopolymerization initiator ("Irgacure 1173", 2-hydroxy-2-methyl-1-phenylpropane-1-one, manufactured by BASF) to a total of 100 parts by mass of 75 parts by mass of a urethane acrylate oligomer (CN8888, manufactured by Arkema) and 25 parts by mass of 4-tert-butyl cyclohexanol acrylate.

[0307] The obtained buffer layer composition was applied to a PET film ("COSMOSHINE A4300" manufactured by Toyobo Co., Ltd., PET film with an easy-adhesion layer on both sides, thickness: 50 μm) as a substrate by a doctor blade coating method to a thickness of 28 μm to form a buffer layer composition layer. Immediately after the coating, a high-pressure mercury lamp was used to illuminate the surface of the film at an illumination of 160 mW / cm 2 、Irradiation 500mJ / cm 2 The buffer layer composition layer was irradiated with ultraviolet rays under conditions of , thereby curing the buffer layer composition layer to form a buffer layer A-1 with a thickness of 28 μm on one side of the PET film serving as the substrate, thereby producing a PET substrate with a buffer layer A-1.

[0308] <Production Example A2: Formation of Buffer Layer A-2>

[0309] The composition of the cushion layer composition was changed as follows, and a cushion layer A-2 having a thickness of 28 μm was formed on a PET film as a substrate by the same method as in Production Example A1.

[0310] Urethane acrylate oligomer (CN8888, manufactured by Arkema): 50 parts by mass

[0311] · 4-tert-Butyl cyclohexanol acrylate: 40 parts by mass

[0312] Dipentaerythritol hexaacrylate: 10 parts by mass

[0313] Photopolymerization initiator ("Irgacure 1173" manufactured by BASF): 2.0 parts by mass

[0314] <Production Example A3: Formation of Buffer Layer A-3>

[0315] The composition of the cushion layer composition was changed as follows, and a cushion layer A-3 having a thickness of 28 μm was formed on a PET film as a substrate by the same method as in Production Example A1.

[0316] Urethane acrylate oligomer (CN8888, manufactured by Arkema): 50 parts by mass

[0317] · 4-tert-Butyl cyclohexanol acrylate: 45 parts by mass

[0318] Dipentaerythritol hexaacrylate: 5 parts by mass

[0319] Photopolymerization initiator ("Irgacure 1173" manufactured by BASF): 2.0 parts by mass

[0320] <Production Example A4: Formation of Buffer Layer A-4>

[0321] The composition of the cushion layer composition was changed as follows, and a cushion layer A-4 having a thickness of 28 μm was formed on a PET film as a substrate by the same method as in Production Example A1.

[0322] Urethane acrylate oligomer (CN8888, manufactured by Arkema): 50 parts by mass

[0323] Isobornyl acrylate: 45 parts by mass

[0324] Dipentaerythritol hexaacrylate: 5 parts by mass

[0325] Photopolymerization initiator ("Irgacure 1173" manufactured by BASF): 2.0 parts by mass

[0326] <Comparative Production Example B1: Production and Formation of Buffer Layer B-1>

[0327] The composition of the cushion layer composition was changed as follows, and a cushion layer B-1 having a thickness of 28 μm was formed on a PET film as a substrate by the same method as in Production Example A1.

[0328] Urethane acrylate oligomer (CN8888, manufactured by Arkema): 50 parts by mass

[0329] 3,3,5-Trimethylcyclohexanol acrylate: 50 parts by mass

[0330] Photopolymerization initiator ("Irgacure 1173" manufactured by BASF): 2.0 parts by mass

[0331] <Comparative Production Example B2: Formation of Buffer Layer B-2>

[0332] The composition of the cushion layer composition was changed as follows, and a cushion layer B-2 having a thickness of 28 μm was formed on a PET film as a substrate by the same method as in Production Example A1.

[0333] Urethane acrylate oligomer (CN8888, manufactured by Arkema): 50 parts by mass

[0334] Isobornyl acrylate: 45 parts by mass

[0335] ·Tricyclodecane dimethanol diacrylate: 5 parts by mass

[0336] Photopolymerization initiator ("Irgacure 1173" manufactured by BASF): 2.0 parts by mass

[0337] <Comparative Production Example B3: Formation of Buffer Layer B-3>

[0338] The composition of the cushion layer composition was changed as follows, and a cushion layer B-3 having a thickness of 28 μm was formed on a PET film as a substrate by the same method as in Production Example A1.

[0339] Urethane acrylate oligomer (CN8888, manufactured by Arkema): 50 parts by mass

[0340] Cyclic trimethylolpropane formal acrylate: 50 parts by mass

[0341] Photopolymerization initiator ("Irgacure 1173" manufactured by BASF): 2.0 parts by mass

[0342] <Reference Example C1: Base Material C-1>

[0343] As substrate C-1, a PET film ("COSMOSHINE A4300" manufactured by Toyobo Co., Ltd., a PET film with an easy-adhesion layer on both sides, thickness: 50 μm) was prepared.

[0344] <Reference Example C2: Base Material C-2>

[0345] As substrate C-2, a polyolefin (PO) film (low-density polyolefin film, thickness: 25 μm)) was prepared.

[0346] [Measurement method and evaluation method]

[0347] <Measurement / calculation of various physical properties of buffer layer and substrate>

[0348] The elastic modulus, fracture energy, fracture stress, and fracture strain of the substrate and the buffer layer were measured using a precision universal testing machine ("Autograph AG-IS" manufactured by Shimadzu Corporation).

[0349] Specifically, for buffer layers A-1 to A-4, buffer layers B-1 to B-3, and substrates C-1 to C-2, measurement samples with a width of 1.5 mm × a length of 150 mm × a thickness of 0.2 mm were prepared. Then, for the measurement samples, the measurement was carried out under the conditions of 100 mm between chucks (the two ends of the measurement sample in the length direction were fixed to the device 25 mm each), a tensile speed of 200 mm / sec, 23°C, and 50% RH. In addition, based on the stress-strain data obtained at this time, the fracture strain (ε 100 ) 80% strain (ε 80 ) increases to the fracture strain (ε 100 ) to the stress increase gradient Δρ 80-100 In addition, the fracture stress and fracture strain (ε100 )

[0350] <Evaluation of cutting performance by tool (1): Evaluation by simulation>

[0351] The state of the cross section when the adhesive tape for semiconductor processing is cut by a cutter was evaluated by simulation using the general-purpose finite element analysis software "Abaqus".

[0352] The analysis model is shown in Figure 3 .

[0353] An analysis model of an adhesive tape for semiconductor processing is assumed in which a semiconductor wafer is rectangular and a laminated structure composed of a buffer layer and a substrate is laminated on the semiconductor wafer. It should be noted that in this analysis model, it is assumed that the end of one side of the adhesive tape for semiconductor processing is in a state constrained by the semiconductor wafer, and the end of the other side is in a state completely constrained by the peripheral worktable side. Then, the state of the cross section of the adhesive tape for semiconductor processing is analyzed when the angle between the buffer layer surface and the tip of the tool is set to 57.2° and the tool is moved in a straight line direction along the semiconductor wafer at a cutting speed of 80 mm / s.

[0354] It should be noted that in the above analysis model, the tool properties are set as a rigid body.

[0355] In addition, as for the cutter, it was assumed that a utility knife (manufactured by OLFA, model "XB10") was used, and only the portion of the utility knife involved in cutting was modeled and its dimensions were input.

[0356] The buffer layer and the substrate were analyzed according to the following combinations.

[0357] Example 1sim.: Buffer layer A-1 / PET

[0358] Example 2sim.: Buffer layer A-2 / PET

[0359] Example 3sim.: Buffer layer A-3 / PET

[0360] Example 4sim.: Buffer layer A-4 / PET

[0361] Comparative Example 1sim.: Buffer layer B-1 / PET

[0362] Comparative Example 2sim.: Buffer layer B-2 / PET

[0363] Comparative Example 3sim.: Buffer layer B-3 / PET

[0364] Reference Example 1sim.: PET

[0365] Reference Example 2sim.: PO

[0366] The thickness of the buffer layer was set to 28 μm, and the thickness of the substrate was set to 50 μm.

[0367] In addition, as the physical property values ​​of the buffer layer and the base material, stress-strain data measured by the above-mentioned precision universal testing machine, and elastic modulus, yield stress, and breaking point based on the data were input.

[0368] It should be noted that the friction coefficient between the tool and the buffer layer is set to 0.25.

[0369] The evaluation criteria are as follows, and 3 or more are considered to be acceptable.

[0370] 1: The cross section of the sheet is very rough.

[0371] 2: The cross section of the piece is rough.

[0372] 3: The cross section of the sheet is slightly rough.

[0373] 4: Slight roughness can be observed on the cross section of the sheet.

[0374] 5: No roughness was observed in the sheet cross section.

[0375] <Evaluation of cutting performance by tool (2): Evaluation based on experiments>

[0376] An adhesive tape for semiconductor processing having the following structure was prepared.

[0377] Example 1 exp.: buffer layer A-1 / PET / adhesive layer

[0378] Comparative Example 3 exp.: Buffer layer B-3 / PET / adhesive layer

[0379] (Formation of Adhesive Layer)

[0380] An acrylic polymer obtained by copolymerizing 65 parts by mass of n-butyl acrylate (BA), 20 parts by mass of methyl methacrylate (MMA) and 15 parts by mass of 2-hydroxyethyl acrylate (2HEA) was reacted with 2-methacryloyloxyethyl isocyanate (MOI) and 80 mol % of hydroxyl groups in all hydroxyl groups of the acrylic polymer were added to obtain an energy-ray-curable acrylic resin (Mw: 500,000).

[0381] 6 parts by mass of a multifunctional urethane acrylate as an energy-ray-curable compound, 0.375 parts by mass of an isocyanate crosslinking agent ("Coronate L" manufactured by Tosoh Corporation), and 1 part by mass of bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide as a photopolymerization initiator were added to 100 parts by mass of the energy-ray-curable acrylic resin, and the mixture was diluted with methyl ethyl ketone to prepare a coating liquid of an adhesive composition having a solid content concentration of 32% by mass.

[0382] (Manufacturing of adhesive tape for semiconductor processing)

[0383] The coating liquid of the adhesive composition obtained above was applied to the release-treated surface of a release sheet (trade name "SP-PET381031" manufactured by Lintec Corporation) and dried by heating to form a 30 μm thick adhesive layer on the release sheet.

[0384] Then, an adhesive layer was bonded to the PET substrate side of the PET substrate with cushion layer A-1 formed in Production Example A1 to prepare an adhesive tape for semiconductor processing having a laminated structure of cushion layer A-1 / PET substrate / adhesive layer.

[0385] Similarly, an adhesive layer was bonded to the PET substrate side of the PET substrate with the buffer layer B-3 formed in Comparative Manufacturing Example B3 to produce an adhesive tape for semiconductor processing having a laminated structure of buffer layer B-3 / PET substrate / adhesive layer.

[0386] (evaluate)

[0387] The semiconductor processing adhesive tapes of Example 1 exp. and Comparative Example 3 exp. were adhered to a silicon wafer having a diameter of 12 inches and a thickness of 775 μm using a back grinding tape laminator (manufactured by Lintec Corporation, device name "RAD-3510F / 12"). Then, the semiconductor processing adhesive tape was cut along the periphery of the silicon wafer using a utility knife (manufactured by OLFA, model "XB10"). The utility knife cuts into the buffer layer side of the semiconductor processing adhesive tape. The angle between the buffer layer surface and the tip of the tool was set to 57.2°. In addition, the cutting speed was set to 80 mm / s. The cross section of the semiconductor processing adhesive tape after cutting was observed using a scanning electron microscope (SEM) and evaluated using the same criteria as the evaluation of the sheet cross section (1).

[0388] In the results of “Evaluation of cutting properties by a tool (1): Evaluation by simulation”, the results of Examples and Comparative Examples are shown in Table 1, and the results of Reference Examples are shown in Table 2.

[0389] Table 3 shows the results of “Evaluation of cutting properties by a cutter (2): Evaluation by experiment”.

[0390] In addition, the analysis images of Example 1sim. and Comparative Example 3sim. in "Evaluation of cutting performance by a tool (1): Evaluation by simulation" are shown in FIG. Figure 4 The results of observation using a scanning electron microscope (SEM) in "Evaluation of cutting performance by a tool (2): Evaluation based on experiments" are shown in Figure 5 .

[0391]

[0392] [Table 2]

[0393]

[0394] ※Fracturing coefficient = fracture stress × fracture strain value

[0395] [Table 3]

[0396]

[0397] ※Fracturing coefficient = fracture stress × fracture strain value

[0398] The following results can be obtained from Table 1.

[0399] It is understood that in Examples 1sim., 2sim., 3sim., and 4sim., in which the buffer layers satisfy the requirements (α) and (β), the cutting properties by the cutter are all good.

[0400] In contrast, it can be seen that in Comparative Examples 1sim. and 2sim., the buffer layer does not satisfy the requirement (β), and the cutting properties by the cutter are both poor.

[0401] In addition, it is understood that in Comparative Example 3sim., the buffer layer satisfies neither the requirement (α) nor the requirement (β), and the cutting property by a cutter is extremely poor.

[0402] The following results can be obtained from Table 2.

[0403] It is understood that in both Reference Examples 1sim. and 2sim., in which the base material satisfies the requirement (γ), the cutting properties by the cutter are good.

[0404] Here, in reference example 2sim., although requirement (β) is not satisfied, the cutting property by the cutter is good. Therefore, it is understood that the cutting property based on requirements (α) and (β) cannot be judged for the base material.

[0405] The following results can be obtained from Table 3.

[0406] Example 1exp. and Comparative Example 3exp. shown in Table 3 are the results of experimental confirmation of Example 1sim. and Comparative Example 3sim. It can be seen that the evaluation results of the cutting properties based on the tool discussed in Example 1exp. and Comparative Example 3exp. are completely consistent with the evaluation results of the cutting properties based on the tool discussed in Example 1sim. and Comparative Example 3sim.

[0407] This can be done by Figure 4 and Figure 5 The results shown are clear.

Claims

1. An adhesive tape for semiconductor processing, which has a laminated structure in which a buffer layer, a substrate and an adhesive layer are laminated in sequence, The buffer layer satisfies both the following requirement (α) and the following requirement (β): Requirement (α): The breaking energy of the buffer layer at 23°C is 15 MJ / m 3 above; Requirement (β): When the buffer layer is subjected to a tensile test at a temperature of 23°C, the breaking strain (ε 100 ) 80% strain (ε 80 ) increases to the fracture strain (ε 100 ) to the stress increase gradient Δρ 80-100 It is above 30MPa.

2. The adhesive tape for semiconductor processing according to claim 1, wherein The substrate satisfies the following requirement (γ): · Requirement (γ): Fracture strain at 23°C (ε 100 ) and the fracture stress (ρ 100 ) is greater than 60MPa.

3. The adhesive tape for semiconductor processing according to claim 1 or 2, wherein: The thickness of the adhesive layer is less than 100 μm.

4. A method for using an adhesive tape for semiconductor processing, wherein the adhesive tape for semiconductor processing is the adhesive tape for semiconductor processing according to any one of claims 1 to 3, the method comprising: When back grinding of a semiconductor wafer is performed, the adhesive tape for semiconductor processing is affixed to the surface of the semiconductor wafer, and the adhesive tape for semiconductor processing is cut along the outer circumference of the semiconductor wafer.

5. A method for manufacturing a semiconductor device, the method comprising: The step (S1) is to stick the adhesive tape for semiconductor processing according to any one of claims 1 to 3 on the surface of a semiconductor wafer, and cut the adhesive tape for semiconductor processing along the outer periphery of the semiconductor wafer.

6. The method for manufacturing a semiconductor device according to claim 5, further comprising the following step (S2): Step (S2) is a step of grinding the semiconductor wafer from the back side.

7. The method for manufacturing a semiconductor device according to claim 6, further comprising the following step (S3): Step (S3) is a step of dicing the semiconductor wafer into individual pieces.

8. The method for manufacturing a semiconductor device according to claim 6, wherein: Using a semiconductor wafer having grooves formed on the surface side as the semiconductor wafer, In the step (S2), the semiconductor wafer is singulated into a plurality of chips using the groove as a starting point.

9. The method for manufacturing a semiconductor device according to claim 6, wherein: As the semiconductor wafer, a semiconductor wafer having a modified region formed therein is used, or a modified region is formed inside the semiconductor wafer after the step (S1), In the step (S2), the semiconductor wafer is singulated into a plurality of chips with the reformed region as a starting point.

Citation Information

Patent Citations

  • Adhesive sheet

    JP2015183008A