Method for manufacturing semiconductor device and plasma processing method

Selective etching in the metal gate cutting process through multi-layer insulating film protection technology, the problems of residual and electrical short circuit of the gate layered film are solved, the distance between the channel and the gate is shortened and the insulation separation is separated, and the transistor is improved. Integration and process stability.

CN118974897APending Publication Date: 2024-11-15HITACHI HIGH TECH CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380013066.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-13
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the metal gate cutting process, vertical etching of the gate laminated film causes residual hole bottom, which easily leads to electrical short circuits, and etching of the interlayer insulating film in the source/drain region results in a decrease in the bonding area, affecting transistor characteristics and process reproducibility .

Method used

Using multi-layer insulating film protection technology, after the first insulating film is etched, the bottom of the cutting area is protected by the first insulating film, and the gate insulating film is gradually etched to prevent metal layer residue and insulating film from remaining, so as to realize gate lamination. Selective etching of the film.

Benefits of technology

Effectively prevent the remaining gate laminated film, shorten the distance between the channel and the gate cutting region, realize insulation separation, reduce the number of process steps, and improve the high integration and process stability of transistors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974897A_ABST
    Figure CN118974897A_ABST
Patent Text Reader

Abstract

In a metal gate dicing process in which a gate stack film is selectively etched with respect to a gate sidewall spacer and an interlayer insulating film of a source / drain region, a metal layer comprising a work function metal and a gate embedded metal is vertically etched, and then the gate stack film is selectively etched with respect to the gate sidewall spacer and the interlayer insulating film of the source / drain region. The side wall is protected by the first insulating film, the residue of the metal layer exposed at the lower part of the cutting region is removed, the side wall of the cutting region is protected by the second insulating film, and the gate insulating film exposed at the bottom part of the cutting region is removed. The present disclosure further provides a technique whereby this series of steps can be continuously performed on the same device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a method for manufacturing a semiconductor element and a plasma processing method. Background Art

[0002] In order to continuously improve the functions and performance of integrated circuit chips, the high integration of transistors is continuously sought. The high integration of transistors has been mainly achieved through the miniaturization of transistor elements. In order to achieve the miniaturization of elements while maintaining or improving the performance of transistors, a large number of improvements have been made to the transistor structure and the materials that constitute the transistor. As examples of such improvements, the introduction of strain in the source region and the drain region of the metal oxide semiconductor field effect transistor (MOSFET: Metal Oxide Semiconductor Field Effect Transistor), the introduction of a high dielectric gate insulating film and metal element metal, and the change of the element structure from a planar type to a fin type with a three-dimensional structure can be cited. Furthermore, if further miniaturized, it is expected that the channel will become a filament (thin line) or sheet-like stack, becoming a gate-around FET (GAA: Gate All Around) in which the channel is covered by a gate.

[0003] These improvements are introduced to suppress the short channel effect caused by the reduction of transistor size, that is, the phenomenon that the leakage current flows between the source and drain electrodes with a shortened distance even when the transistor is turned off. In other words, it is a technical improvement that can achieve the miniaturization of transistors while preventing the degradation of transistor characteristics caused by the short channel effect. However, when miniaturization continues, the manifestation of the short channel effect is inevitable, and further miniaturization becomes difficult.

[0004] In order to eliminate the above-mentioned problems, a method of high integration of transistors that does not rely solely on the miniaturization of transistors has begun to be applied. The most effective method is to reduce the distance between transistors. In previous integration, the distance between adjacent transistors was reduced at approximately the same ratio as the reduction in transistor size, but by further shortening the transistor spacing compared to the reduction rate of the transistor size, further high integration can be achieved. That is, even if the miniaturization speed of the transistor slows down, the high integration speed of the transistor can be maintained by further reducing the spacing between transistors compared to the miniaturization rate of the transistor size. However, the reduction in the above-mentioned transistor spacing is accompanied by the need to change the layout rules determined by considering transistor characteristics, yield, etc., so corresponding process changes are sought. The reduction in the above-mentioned transistor spacing and the accompanying process changes are called DTCO (Design and Technology Co-Optimization), which will become a further important technical concept with the high integration of transistors in the future.

[0005] Non-patent document 1 shows a metal gate cutting technology as one of the DTCO technologies. This technology is a technology that cuts the gate by vertical etching after burying a high-permittivity (high-k) gate insulating film and a work function control metal (work function metal) and a gate buried metal in the gate region. In the past, the gate cutting process was applied to a method of cutting a dummy gate composed of polycrystalline silicon (poly-Si) and filling the cutting area with an insulating film, removing the poly-Si dummy gate, and burying the gate stack film (gate insulating film / work function metal / gate buried metal) in the gate. In the above-mentioned previous methods, it is necessary to fill the gate stack film between the Fin channel of the FinFET or the sheet channel of the GAA FET and the insulating film plug (plug) formed in the cutting area, so it is necessary to set the interval between the channel and the plug to at least twice the total film thickness of the gate stack film. The above-mentioned metal gate cutting technology performs the gate cutting process after the gate stack film is formed, so the above-mentioned channel-plug interval can be reduced compared to the previous gate cutting process. That is, the distance between transistors via the insulating film plug can be reduced without reducing the size of the transistors.

[0006] Patent document 1 discloses a specific example of the above-mentioned metal gate cutting process. In a Fin FET process having a Fin channel, after forming the Fin channel, the element separation insulating film, the dummy gate, the gate sidewall spacer, the source and drain, and the interlayer insulating film of the source / drain region, the dummy gate is removed and replaced with a gate stack film, and then the gate stack film is cut by dry etching using a gate cutting mask. At this time, the gate embedded metal, work function metal, and gate insulating film constituting the gate stack film are selectively etched relative to the insulating film constituting the periphery of the gate, i.e., the gate sidewall spacer, and the interlayer insulating film of the source / drain region. By using selective etching conditions, even if the gate cutting mask extends the gate in the vertical direction of the gate, only the gate can be etched. That is, there is no need to match the gate cutting mask width in the direction perpendicular to the gate with the gate length, i.e., the gate wiring width, and a mask design with a margin can be performed.

[0007] Patent document 2 discloses a specific example of performing etching for gate cutting under non-selective conditions with respect to the peripheral insulating film in the above-mentioned metal gate cutting process. When the gate stack film is vertically etched, the gate sidewall spacer exposed in the area not covered by the gate cutting mask and the interlayer insulating film in the source / drain region are etched simultaneously with the gate stack film. The gate sidewall is also etched simultaneously, thereby suppressing the generation of gate stack film residues that are likely to remain on the gate sidewall.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: European Patent Application Publication No. 3836226

[0011] Patent Document 2: U.S. Patent Application Publication No. 2020 / 0135472

[0012] Non-patent literature

[0013] Non-patent literature 1: A. Greene, et al., "Gate-Cut-Last in RMG to Enable GateExtension Scaling and Parasitic Capacitance Reduction", Proceedings of VLSISymposium 2019, 2019, pp.T144~T145 Summary of the invention

[0014] Problems to be solved by the invention

[0015] In the case of applying the metal gate cutting process disclosed in Patent Document 1, the vertical etching of the gate stack film is selectively performed relative to the gate sidewall spacer and the interlayer insulating film in the source / drain region, so it is necessary to perform hole-shaped processing to open the area surrounded by the gate cutting width and the gate length (gate wiring width). The etching becomes large in aspect ratio, and the gate stack film is likely to remain at the bottom of the hole. In particular, the film deposited on the side wall of the spacer is further difficult to remove at the bottom of the hole. In the case where a metal film such as a work function metal or a gate embedded metal remains as an etching residue along the side wall of the spacer, there is a concern that the cut gates are electrically connected to each other at the bottom of the cut area, resulting in an electrical short circuit.

[0016] In the metal gate cutting process disclosed in Patent Document 2, the gate sidewall spacer adjacent to the gate and the interlayer insulating film in the source / drain region are also etched simultaneously with the gate stack film, so the area etched during gate cutting has a shape that extends linearly in the direction perpendicular to the gate. Compared with the hole-shaped processing shown in Patent Document 1, the aspect ratio is reduced, and the etching and removal of the gate stack film becomes easier. In particular, the gate sidewall spacer is etched at the same time, so the gate stack film residue on the side wall of the spacer is eliminated, so the gate stack film can be completely removed. Therefore, it is possible to prevent electrical short circuits between the cut gates. However, the interlayer insulating film in the source / drain region is also etched at the same time, so when the distance between the channel and the cutting area is shortened, the epitaxial film layer constituting the source / drain is also partially etched, and the surface area and volume of the source / drain are reduced. Therefore, in the case where the source / drain is bonded to the metal contact layer, there is a concern that the bonding area is reduced and the contact resistance is reduced. In addition, the epitaxial growth layer mentioned above has the effect of applying strain to the source / drain to increase the carrier mobility propagating in the channel. Therefore, there is also a concern that a part of the epitaxial growth layer is etched away, thereby reducing the strain amount and causing the transistor characteristics to deteriorate. Moreover, the epitaxial growth layer is exposed during the process, and the exposed surface is also damaged by etching, so that defects may also occur in the epitaxial layer in subsequent processes. Therefore, in order to eliminate these concerns, it is necessary to widen the distance between the channel and the gate cutting area to a certain extent. That is, in the metal gate cutting process disclosed in Patent Document 2, there is a concern that the reduction in the distance between the channel and the gate cutting area caused by the high integration of transistors may produce a trade-off relationship between transistor characteristics and process reproducibility.

[0017] The present disclosure provides the following technology: in a metal gate cutting process in which a gate stack film is selectively etched relative to a gate sidewall spacer and an interlayer insulating film in a source / drain region, after vertically etching a metal layer composed of a work function metal and a gate buried metal, the sidewall is protected by a first insulating film, and the residue of the metal layer exposed at the bottom of the cutting region is removed, and then the sidewall of the cutting region is protected by a second insulating film, and the gate insulating film exposed at the bottom of the cutting region is removed. The present disclosure further provides a technology capable of continuously performing this series of processes in the same device.

[0018] Solutions to Solve Problems

[0019] The outline of the representative aspects of the present disclosure will be briefly described as follows.

[0020] One embodiment of the present disclosure provides a technique (a method for manufacturing a semiconductor element or a plasma processing method) in which, in a structure in which a metal film is stacked on an insulating film, the method comprises:

[0021] In a first step, the metal layer is etched in a vertical direction to form a groove-shaped cutting area;

[0022] A second step is to deposit a protective insulating film on the sidewalls of the cut region formed by the etching;

[0023] A third step is to anisotropically etch the protective insulating film in a vertical direction to expose the surface of the gate insulating film present at the bottom of the metal layer;

[0024] A fourth step of removing a portion of the metal film by isotropic etching;

[0025] A fifth step, in which the fourth step is sandwiched between the cyclic steps consisting of the second step and the third step as needed, and the process is repeated multiple times using an insulating film material different from the protective insulating film, so that a laminated film of a protective insulating film consisting of the protective insulating film and a plurality of protective insulating films different from the protective insulating film is formed on the side wall of the cutting area; and

[0026] In the sixth step, a portion of the gate insulating film exposed at the bottom of the dicing region is removed by etching.

[0027] Effects of the Invention

[0028] According to one embodiment of the present disclosure, in the metal gate cutting process, it is possible to prevent the gate stack film from remaining on the side wall of the spacer while maintaining the condition of selectively etching the gate stack film relative to the gate sidewall spacer and the interlayer insulating film in the source / drain region. That is, the distance between the Fin channel of the Fin FET or the sheet channel of the GAA FET and the gate cutting area can be shortened, and at the same time, the insulation separation between the cut gates can be achieved. In addition, since the device characteristics for implementing multiple processes of the metal gate cutting process can be performed through a continuous process in the same device, the increase in the number of process steps can be suppressed.

[0029] Other objects and novel features will become apparent from the description of this specification and the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a panoramic view showing the manufacturing process of the metal gate cutting process of the FET of Example 1.

[0031] Figure 2 It is a top view showing the manufacturing process of the metal gate cutting process of the FET of Example 1.

[0032] Figure 3AIt is a cross-sectional view of the gate region of the transistor in a direction parallel to the gate, showing the manufacturing process of the metal gate cutting process of the FET of Example 1.

[0033] Figure 3B It is a cross-sectional view of a gate cutting region in a direction perpendicular to the gate, showing a manufacturing process of a metal gate cutting process of the FET of the first embodiment.

[0034] Figure 4A It is a cross-sectional view of the gate region of the transistor in a direction parallel to the gate, showing the manufacturing process of the metal gate cutting process of the FET of Example 1.

[0035] Figure 4B It is a cross-sectional view of a gate cutting region in a direction perpendicular to the gate, showing a manufacturing process of a metal gate cutting process of the FET of the first embodiment.

[0036] Figure 5A It is a cross-sectional view of the gate region of the transistor in a direction parallel to the gate, showing the manufacturing process of the metal gate cutting process of the FET of Example 1.

[0037] Figure 5B It is a cross-sectional view of a gate cutting region in a direction perpendicular to the gate, showing a manufacturing process of a metal gate cutting process of the FET of the first embodiment.

[0038] Fig. 6A It is a cross-sectional view of the gate region of the transistor in a direction parallel to the gate, showing the manufacturing process of the metal gate cutting process of the FET of Example 1.

[0039] Figure 6B It is a cross-sectional view of a gate cutting region in a direction perpendicular to the gate, showing a manufacturing process of a metal gate cutting process of the FET of the first embodiment.

[0040] Fig. 7A It is a cross-sectional view of the gate region of the transistor in a direction parallel to the gate, showing the manufacturing process of the metal gate cutting process of the FET of Example 1.

[0041] Figure 7B It is a cross-sectional view of a gate cutting region in a direction perpendicular to the gate, showing a manufacturing process of a metal gate cutting process of the FET of the first embodiment.

[0042] Fig. 8A It is a cross-sectional view of the gate region of the transistor in a direction parallel to the gate, showing the manufacturing process of the metal gate cutting process of the FET of Example 1.

[0043] Figure 8BIt is a cross-sectional view of a gate cutting region in a direction perpendicular to the gate, showing a manufacturing process of a metal gate cutting process of the FET of the first embodiment.

[0044] Fig. 9A It is a cross-sectional view of the gate region of the transistor in a direction parallel to the gate, showing the manufacturing process of the metal gate cutting process of the FET of Example 1.

[0045] Fig. 9B It is a cross-sectional view of a gate cutting region in a direction perpendicular to the gate, showing a manufacturing process of a metal gate cutting process of the FET of the first embodiment.

[0046] Fig. 10A It is a cross-sectional view of the gate region of the transistor in a direction parallel to the gate, showing the manufacturing process of the metal gate cutting process of the FET of Example 1.

[0047] Fig. 10B It is a cross-sectional view of a gate cutting region in a direction perpendicular to the gate, showing a manufacturing process of a metal gate cutting process of the FET of the first embodiment.

[0048] Fig.11A It is a cross-sectional view of the gate region of the transistor in a direction parallel to the gate, showing the manufacturing process of the metal gate cutting process of the FET of Example 1.

[0049] Fig. 11B It is a cross-sectional view of a gate cutting region in a direction perpendicular to the gate, showing a manufacturing process of a metal gate cutting process of the FET of the first embodiment.

[0050] Fig.12 It is a flow chart of the manufacturing process of the metal gate cutting process of the FET of Example 1.

[0051] Fig.13A This is a cross-sectional view of the gate region of the transistor in a direction parallel to the gate, showing a gate insulating film removal step in a metal gate cutting process of the FET of Example 1.

[0052] Fig. 13B This is a cross-sectional view of a gate cut region of a transistor in a direction perpendicular to the gate, showing a gate insulating film removal step in a metal gate cut process of the FET of Example 1.

[0053] Fig.14A This is a cross-sectional view of the gate region of the transistor in a direction parallel to the gate, showing a gate insulating film removal step in a metal gate cutting process of the FET of Example 1.

[0054] Fig. 14BThis is a cross-sectional view of a gate cut region of a transistor in a direction perpendicular to the gate, showing a gate insulating film removal step in a metal gate cut process of the FET of Example 1.

[0055] Fig.15A This is a cross-sectional view of the gate region of the transistor in a direction parallel to the gate, showing a gate insulating film removal step in a metal gate cutting process of the FET of Example 1.

[0056] Fig. 15B This is a cross-sectional view of a gate cut region of a transistor in a direction perpendicular to the gate, showing a gate insulating film removal step in a metal gate cut process of the FET of Example 1.

[0057] Fig.16 It is a diagram showing a structural example of a plasma processing apparatus.

[0058] Fig.17A This is a cross-sectional view of the gate region of the transistor in a direction parallel to the gate, showing a gate insulating film removal step in a metal gate cutting process of the FET of Example 2.

[0059] Fig. 17B This is a cross-sectional view of a gate cut region of a transistor in a direction perpendicular to the gate, showing a gate insulating film removal step in a metal gate cut process of the FET of the second embodiment.

[0060] Fig.18A This is a cross-sectional view of the gate region of the transistor in a direction parallel to the gate, showing a gate insulating film removal step in a metal gate cutting process of the FET of Example 2.

[0061] Fig.18B This is a cross-sectional view of a gate cut region of a transistor in a direction perpendicular to the gate, showing a gate insulating film removal step in a metal gate cut process of the FET of the second embodiment.

[0062] Fig.19A This is a cross-sectional view of the gate region of the transistor in a direction parallel to the gate, showing a gate insulating film removal step in a metal gate cutting process of the FET of Example 2.

[0063] Fig.19B This is a cross-sectional view of a gate cut region of a transistor in a direction perpendicular to the gate, showing a gate insulating film removal step in a metal gate cut process of the FET of the second embodiment.

[0064] Fig. 20 It is a flowchart showing the manufacturing process of the metal gate cutting process of the FET of the second embodiment.

[0065] Fig.21AThis is a cross-sectional view of the gate region of the transistor in a direction parallel to the gate, showing a gate insulating film removal step in a metal gate cutting process of the FET of the third embodiment.

[0066] Fig. 21B It is a cross-sectional view of a gate cut region of a transistor in a direction perpendicular to the gate, showing a gate insulating film removal step in a metal gate cut process of the FET of the third embodiment.

[0067] Fig.22A This is a cross-sectional view of the gate region of the transistor in a direction parallel to the gate, showing a gate insulating film removal step in a metal gate cutting process of the FET of the third embodiment.

[0068] Fig. 22B It is a cross-sectional view of a gate cut region of a transistor in a direction perpendicular to the gate, showing a gate insulating film removal step in a metal gate cut process of the FET of the third embodiment.

[0069] Fig.23A This is a cross-sectional view of the gate region of the transistor in a direction parallel to the gate, showing a gate insulating film removal step in a metal gate cutting process of the FET of the fourth embodiment.

[0070] Fig. 23B It is a cross-sectional view of a gate cut region of a transistor in a direction perpendicular to the gate, showing a gate insulating film removal step in a metal gate cut process of the FET of the fourth embodiment.

[0071] Fig.24A This is a cross-sectional view of the gate region of the transistor in a direction parallel to the gate, showing a gate insulating film removal step in a metal gate cutting process of the FET of the fourth embodiment.

[0072] Fig. 24B It is a cross-sectional view of a gate cut region of a transistor in a direction perpendicular to the gate, showing a gate insulating film removal step in a metal gate cut process of the FET of the fourth embodiment.

[0073] Fig.25A This is a cross-sectional view of the gate region of the transistor in a direction parallel to the gate, showing a gate insulating film removal step in a metal gate cutting process of the FET of the fourth embodiment.

[0074] Fig.25B It is a cross-sectional view of a gate cut region of a transistor in a direction perpendicular to the gate, showing a gate insulating film removal step in a metal gate cut process of the FET of the fourth embodiment.

[0075] Fig.26 It is a flowchart showing the manufacturing process of the metal gate cutting process of the FET of the fourth embodiment. DETAILED DESCRIPTION

[0076] Hereinafter, the implementation mode of the present disclosure will be described based on the accompanying drawings. It should be noted that the present disclosure is not limited to the embodiments described below, and various modifications can be made within the scope of its technical concept. In all the figures used to illustrate the embodiments, the same figure mark is sometimes used to mark the components with the same function, and the repeated description thereof is omitted. In addition, of course, it is possible to make more changes to the content disclosed as the present embodiment, such as changing the combination of materials and manufacturing processes. In addition, the drawings do not necessarily match the scale accurately, and the important parts are schematically depicted for the sake of logical clarity. In addition, in order to make the description clearer, the drawings are sometimes schematically represented compared to the actual method, but this is only an example and does not limit the interpretation of the present disclosure.

[0077] [Example 1]

[0078] In Example 1, the metal gate cutting process in the manufacturing process (semiconductor device manufacturing method or plasma processing method) of Fin type FET (Fin type Field Effect Transistor) or GAA type FET (Gate All Around type Field Effect Transistor) as a semiconductor device, and the details of the process of selectively etching the gate stacked film containing metal relative to the peripheral film and removing the metal residue in the cutting area by stacking a plurality of sidewall protection films composed of different materials in the above process are described. First, using Figure 1 , Figure 2 , Figure 3A to Figure 11A , Figure 3B to Figure 11B , Fig.12 , Figures 13A to 15A , Figure 13B to Figure 15B The semiconductor device manufacturing method or plasma processing method described in this embodiment is a method for forming a Fin-type FET or GAA-type FET having a Fin-shaped channel or a thin line-shaped or sheet-shaped channel stacked in a direction perpendicular to a substrate in a gate forming region, a gate being cut between channels, and the cut region being insulated and separated by an insulating film.

[0079] Figure 1 as well as Figure 2 The diagrams are respectively a panoramic view and a top view of a structure immediately before the metal gate cutting process is performed in the manufacturing process of the Fin-type FET or the GAA-type FET. Figure 3A to Figure 11A The gate region ( Figure 1 as well as Figure 2 A cross-sectional view taken along line AA' of the embodiment of the present invention. Figure 3B to Figure 11B The gate cutting region ( Figure 1 as well as Figure 2 A cross-sectional view taken along line BB' of FIG. Fig.12 Show Figure 3A to Figure 11A as well as Figure 3B to Figure 11B A flow chart of a series of manufacturing steps is shown. Figures 13A to 15A It is shown in Fig.12 The gate region of the transistor in the direction parallel to the gate in the process of removing the gate insulating film remaining on the gate sidewall spacer after the metal gate cutting process shown in FIG. Figure 1 as well as Figure 2 A cross-sectional view taken along line AA' of the embodiment of the present invention. Figure 13B to Figure 15B It is shown in Fig.12 The gate cutting region ( Figure 1 as well as Figure 2 A cross-sectional view taken along line BB' of FIG.

[0080] exist Figure 1 In the present invention, a single crystal semiconductor substrate 1 has a Fin-type channel structure, and the Fin-type channel structure has a channel composed of a periodic or linear pattern based on the periodic or linear pattern. An element separation (STI: Shallow Trench Isolation) insulating film (referred to as an STI insulating film) 2 constituting an element separation region is formed on the semiconductor substrate 1. Here, the height of the STI insulating film 2 is set in such a way that a portion of the Fin-type channel is exposed. In a gate region oriented in a direction perpendicular to the Fin-type channel, a gate insulating film 3, a work function metal 4, and a gate buried metal 5 are sequentially stacked on the Fin-type channel exposed on the upper part of the STI insulating film 2. A gate sidewall spacer 6 is formed on the sidewall of the gate region, and an etching stop layer 7 and an interlayer insulating film 8 of the source / drain region are deposited on the region surrounded by the STI insulating film 2 and the gate sidewall spacer 6. A hard mask layer 9 for patterning the gate cut region is formed on the gate stack film composed of the gate insulating film 3, the work function metal 4 and the gate buried metal 5, the gate sidewall spacer 6, the etching stop layer 7, and the interlayer insulating film 8 of the source / drain region. In other words, the gate structure is composed of the gate stack film and is set to a shape oriented in a direction perpendicular to the orientation direction of the Fin-type channel. Here, the channel structure can be configured to include a fin-shaped, filament-shaped, or sheet-shaped channel on the semiconductor substrate.

[0081] In the semiconductor substrate 1, for example, silicon (Si) is preferably used. The computer may also be a substrate with silicon germanium (SiGe) film formed on Si, or an SOI (Silicon on Insulator) substrate using an insulating film such as a silicon oxide film (SiO2) and a stacked film of a Si layer on a Si substrate may be used. As a processing technique for forming a Fin-type channel, a method of etching the substrate in a vertical direction after patterning using an etching technique is used. In the case of patterning, for example, using a laser with argon fluoride gas (ArrF) as a light source, if the pattern period is, for example, greater than 40nm and less than 80nm, self-aligned double patterning (SADP: Self-Aligned Double Patterning) can be used. In addition, if the pattern period is, for example, greater than 20nm and less than 40nm, self-aligned quadruple patterning (SAQP: Self-Aligned Quadruple Patterning) can be used. In addition, when performing extreme ultraviolet (EUV) exposure with a wavelength of 13.5nm, single exposure (Single Patterning) can be used when the pattern period is, for example, 40nm or more. If the pattern period is, for example, 20nm or more and 40nm or less, SADP can be used. In the case of Fin-type FET, one transistor is composed of one or more Fin-type channels, but Figure 1 The two Fin-type channels shown become Fin-type channels belonging to different transistors. In this case, Figure 1 The interval between the two Fin-type channels shown is designed to be wider than the minimum interval of the pattern, and one or more Fins are removed by etching after the pattern structure is formed.

[0082] The STI insulating film 2 is formed by, for example, forming an insulating film such as SiO2 film, silicon nitride oxide film (SiON), or silicon carbon oxide film (SiCO) by chemical vapor deposition (CVD) or the like, and etching the insulating film 2 until a portion of the Fin-type channel is exposed.

[0083] The gate sidewall spacer 6 is formed on the sidewall of the dummy gate (not shown). The dummy gate is formed by depositing a dummy gate insulating film composed of SiO2 or an insulating film based on it and amorphous (non-crystalline) Si or polycrystalline (poly) Si on the Fin-type channel and the STI insulating film 2, and performing a periodic pattern processing oriented in a direction perpendicular to the Fin-type channel or a linear pattern processing based on it. In the above patterning, a single exposure and SADP method using the ArF light source are used according to the pattern period. The size of the gate pattern is preferably, for example, to set the gate spacing to 40nm to 70nm, and to set the width of the dummy gate, that is, the gate length, to a range of 10nm to 30nm. Preferably, a SiON film, a silicon carbon nitride oxide film (SiOCN) or a SiCO film as a low relative dielectric constant film is formed on the dummy gate using a CVD method or the like, and then etching is performed to obtain the gate sidewall spacer 6. The film thickness of the gate sidewall spacer 6 is preferably adjusted within a range of 5 nm to 15 nm, for example.

[0084] The etching stop layer 7 and the interlayer insulating film 8 in the source / drain region are formed by forming the source / drain (not shown) of the transistor after the gate sidewall spacer 6 is formed, and are sequentially stacked on the region surrounded by the gate sidewall spacer 6 and the STI insulating film 2. The etching stop layer 7 is obtained by forming a silicon nitride film (SiN), or a silicon carbon nitride film (SiCN), or a SiOCN, or a SiON film using a CVD method or the like. The film thickness of the etching stop layer 7 is preferably adjusted within a range of 2nm to 10nm, for example. The interlayer insulating film 8 is formed in a manner that fills the source / drain region surrounded by the gate sidewall spacer 6 outside the gate region, preferably using a SiO2 film, a SiON film, or a SiOCN film, etc. as the material, and using a CVD method or the like as the film forming method.

[0085] The gate stack film composed of the gate insulating film 3, the work function metal 4 and the gate buried metal 5 is formed on the Fin-type channel after removing the dummy gate and the dummy gate insulating film. The above-mentioned dummy gate removal is performed by exposing the dummy gate by chemical mechanical polishing (CMP) after forming the interlayer insulating film 8 in the source / drain region, and etching and removing the dummy gate and the dummy gate insulating film in sequence. The gate stack film is formed by, for example, CVD or ALD (Atomic Layer Deposition). In the gate insulating film 3, for example, high dielectric materials such as hafnium oxide (HfO2) and aluminum oxide (Al2O3) and stacked films of these high dielectric materials are preferably used. The film thickness of the gate insulating film 3 is preferably adjusted in the range of 1nm to 3nm. The work function metal 4 is determined in consideration of the target transistor performance or the conductivity type of the transistor. For example, in the work function metal 4 that determines the threshold voltage of the p-type FET, for example, titanium nitride (TiN) or tantalum nitride film (TaN) or a metal compound having a work function equivalent to them is preferably used. In the work function metal 4 that determines the threshold voltage of the n-type FET, for example, titanium aluminum (TiAl) or a metal containing carbon (C), oxygen (O), nitrogen (N) and the like in TiAl or a metal compound composed of a metal compound having a work function equivalent to them is preferably used. The work function metal 4 can also be composed of a single film or a plurality of stacked films, and the total film thickness is adjusted in the range of 2nm to 10nm, for example. The gate buried metal 5 is deposited for the purpose of reducing the metal resistance in the gate, and for example, tungsten (W) and other materials can be used.

[0086] After the gate stack film is formed, the work function metal 4 or the gate buried metal 5 is flattened using CMP as a stopper, and a hard mask 9 is deposited. A resist (not shown) is deposited on the hard mask 9, and patterning is performed to open the gate cut region through the resist, and the resist is removed to obtain Figure 1 structure. Here, the above-mentioned resist is preferably a three-layer resist composed of a spin-coated carbon film / spin-coated glass film / organic resist. The spin-coated carbon film is an organic film mainly composed of carbon, and the spin-coated glass film is an organic film containing Si and oxygen. Usually, in the process using the three-layer resist, in most cases, the spin-coated glass film is etched using the resist, and after the spin-coated carbon film is etched using the spin-coated glass film as a mask, the resist and the spin-coated glass film are removed and the spin-coated carbon film is used as a mask. In this case, the hard mask 9 is mainly composed of a spin-coated carbon film. The hard mask 9 can also be an insulating film such as a SiO2 film, a silicon nitride film (Si3N4), etc. In this case, after the three-layer resist is deposited on the hard mask 9, patterning is performed, and the hard mask is etched to remove the three-layer resist, thereby obtaining Figure 1The gate cut pattern is oriented in a direction perpendicular to the gate, and after patterning, the gate sidewall spacer 6, the etching stop layer 7, and the surface of the interlayer insulating film 8 are exposed simultaneously with the gate stack film. In addition, the gate cut width is preferably set to a range of 10nm to 30nm, for example.

[0087] It should be noted that in Figure 1 , but a GAA FET may also be used. In this case, the channel has a structure formed by stacking filamentary or sheet-like semiconductor layers. The stacked channel structure is preferably formed by, for example, using a stacked film formed by alternately forming a Si layer and a SiGe layer to form a Fin shape, and after removing the dummy gate and the dummy gate insulating film, the SiGe layer is selectively etched away relative to the Si layer to form a Fin shape.

[0088] exist Figure 2 Shown in the figure as viewed from above Figure 1 . In the gate region sandwiched between different gate sidewall spacers 6, a gate insulating film 3, a work function metal 4 and a gate buried metal 5 are sequentially formed from the sidewall of the gate sidewall spacer 6, and the gate is filled, and an etching stop layer 7 and an interlayer insulating film 8 of the source / drain region are formed outside the gate sidewall spacer 6. Preferably, the gate sidewall spacer 6, the gate insulating film 3, the work function metal 4, the gate buried metal 5, the etching stop layer 7, and the interlayer insulating film 8 are exposed in the region opened by the hard mask 9.

[0089] Figure 3A as well as Figure 3B They are Figure 1 as well as Figure 2 The gate region of the transistor in the direction parallel to the gate in the structure shown ( Figure 1 as well as Figure 2 AA' line), a cross-sectional view of the gate cutting area in the direction perpendicular to the gate ( Figure 1 as well as Figure 2 BB' line) of the cross-sectional view. Figure 3B As shown, the gate region surrounded by the gate sidewall spacer 6 has a downwardly extending shape near the bottom surface. This is because the dummy gate pattern that serves as a base when forming the gate sidewall spacer 6 tends to have a tapered shape that extends downwardly when dry etching is used.

[0090] from Figure 3A as well as Figure 3B The structure shown in FIG. 1 is anisotropically etched along the gate cutting pattern opened by the hard mask 9 along the vertical direction to obtain the gate buried metal 5 and the work function metal 4. Figure 4A as well as Figure 4BThe structure shown. The anisotropic etching of the gate buried metal 5 and the work function metal 4 is preferably performed by using, for example, halogen-based gases such as tetrafluoromethane (CF4), trifluoromethane (CHF3), or boron trichloride (BCl3), chlorine (Cl2), hydrogen chloride (HCl), or a mixed gas thereof, or a mixed gas in which oxygen (O2), nitrogen (N2), or argon (Ar), helium (He), or methane (CH4) are added. The above etching is performed under conditions such that it is selective etching with respect to the hard mask 9 and the gate sidewall spacer 6, the etching stop layer 7, and the interlayer insulating film 8 of the source / drain region. For example, when selectively etching the gate buried metal 5, when the gate buried metal 5 is composed of a material centered on W, it is preferably to use a mixed gas of CHF3 and O2 or a gas based thereon. When etching the work function metal 4, for example, when the work function metal 4 is TiN or TaN, it is preferred to use a mixed gas of CF4 and O2, a mixed gas of Cl2 and Ar, or a mixed gas of Cl2, O2, He, etc. For example, when the work function metal 4 is composed of TiAl or a material containing C, O, N, etc. in TiAl, it is preferred to use a mixed gas of CF4 and Cl2, a mixed gas of CF4 and HCl, or a mixed gas in which Ar, He, N2, etc. are added to these gases in the etching gas. The anisotropic etching of the gate buried metal 5 and the work function metal 4, i.e. Figure 4A as well as Figure 4B The process shown is equivalent to Fig.12 The gate metal vertical etching 101 of the process flow chart is performed under the etching condition that the gate insulating film 3 is used as a stopper. Figure 4A As shown in FIG. 1 , after the above etching, the upper surface of the gate insulating film 3 is exposed at the bottom of the gate cut region. Figure 4B As shown, the gate sidewall spacer 6 has a tapered shape that expands downward near the bottom, so after the gate metal vertical etching 101, the work function metal 4 and the gate embedded metal 5 are likely to remain in the tapered portion.

[0091] exist Figure 5A as well as Figure 5BIn the embodiment, the first protective insulating film 10 is deposited by using a film forming technology based on the ALD (Atomic Layer Deposition) method. The protective insulating film 10 is deposited on the upper surface and side walls of the hard mask 9, the upper surface and side walls of the gate insulating film 3, the side walls of the gate buried metal 5, the side walls of the work function metal 4, the upper surface of the gate sidewall spacer 6, the upper surface of the etching stop layer 7, and the upper surface of the interlayer insulating film 8 in the source / drain region. The material of the protective insulating film 10 is preferably an insulating film containing nitrogen, for example, preferably a Si3N4 film or a SiON film based thereon, etc. The film thickness of the protective insulating film 10 is controlled to be, for example, about 2nm to 3nm. The ALD method has the advantage of being able to form a thin film with good controllability even for complex shapes with many bumps and depressions. When the protective insulating film 10 is a Si3N4 film formed by the ALD method, the raw material of Si is, for example, bis(tertbutylamino)silane (BTBAS) or bis(diethylamino)silane (BDEAS), or dichlorosilane (SiH2Cl2), and the raw material of nitrogen is N2 gas or a mixed gas of N2 gas and hydrogen H2 gas, or a gas containing nitrogen such as ammonia (NH3) gas. It should be noted that the protective insulating film 10 may also be a film that does not contain nitrogen such as SiO2, or may be formed by a CVD method or the like. Figure 5A The gate height in the direction perpendicular to the substrate, which is composed of the work function metal 4 and the gate buried metal 5, is designed to be within the range of about 50nm to 200nm. The gate cutting width is about 10nm to 30nm, but with the high integration of transistors, the gate cutting width is reduced, so it is assumed that the etching pattern with a pattern width of about 10nm and a depth of about 200nm is conceived. When the protective insulating film 10 is formed on such a narrow and deep pattern, it is assumed that the film thickness in the vertical direction at the bottom of the groove ( Figure 5A t2, Figure 5B t2') is greater than the horizontal film thickness at the side wall ( Figure 5A t1, Figure 5B When the film thickness t1 or t1' of the protective insulating film 10 on the pattern sidewall in the horizontal direction is set to 2 nm to 3 nm, for example, the film thickness t2 or t2' in the vertical direction at the groove bottom is expected to be 3 nm to 6 nm, for example. Figure 5A as well as Figure 5B The process shown is equivalent to Fig.12 The first protective insulating film deposition 102 of the process flow chart is preferably followed by Figure 4A as well as Figure 4BThe gate metal vertical etching 101 is shown to be performed continuously in the chamber of the same device.

[0092] exist Fig. 6A as well as Figure 6B In the process shown, the protective insulating film 10 is etched in the vertical direction. The above etching is performed under selective etching conditions relative to the hard mask 9, the gate insulating film 3, the gate sidewall spacer 6, the etching stop layer 7, and the interlayer insulating film 8. For example, when the protective insulating film 10 is a Si3N4 film, it is preferable to use a gas such as Cl2 added to a mixed gas of a halogen-based gas such as CF4, octafluorocyclobutane (C4F8) and O2, or a gas based on the gas. By this etching, the upper surface of the gate insulating film 3 is exposed at the bottom of the gate cutting area. In this etching, the film thickness of the protective insulating film 10 in the vertical direction at the bottom of the groove is taken into consideration, and attention is paid to exposing the upper surface of the gate insulating film 3, and the etching time is determined in such a way that the upper end of the protective insulating film 10 in contact with the gate sidewall spacer 6 is located between the upper end and the lower end of the hard mask 9 after etching. The vertical thickness of the protective insulating film 10 at the bottom of the groove is thicker than the horizontal thickness of the protective insulating film 10 at the sidewall of the groove. Therefore, at the bottom of the groove after etching, a part of the protective insulating film 10 at the sidewall is also etched away, and a part of the work function metal 4 and the gate buried metal 5 are exposed at the sidewall of the cut gate ( Fig. 6A ), a portion of the work function metal 4 is exposed on the side wall of the gate side wall spacer 6 ( Figure 6B ). At this time, the lower part of the protective insulating film 10 is Fig. 6A as well as Figure 6B As shown in the figure, the side wall of the gate is cut ( Fig. 6A ) and the sidewalls of the gate sidewall spacer 6 ( Figure 6B ) and the eaves, and the angles θ1 and θ1' are both acute angles less than 90 degrees. Fig. 6A as well as Figure 6B The process shown is equivalent to Fig.12 The first protective insulating film is vertically etched 103, preferably followed by Figure 5A as well as Figure 5B The first protective insulating film deposition 102 is shown to be performed continuously in the chamber of the same apparatus.

[0093] Following the above process, the work function metal 4 is partially removed by isotropic etching to obtain Fig. 7A as well as Figure 7BThe structure shown. The above etching is preferably performed under conditions such as selective etching with respect to the protective insulating film 10, the gate insulating film 3, the gate buried metal 5, the hard mask 9, the gate sidewall spacer 6, the etching stop layer 7, and the interlayer insulating film 8, and the work function metal 4 is isotropically etched. For example, in the case where the work function metal 4 is TiN or TaN, it is preferred to use a mixed gas of Cl2, O2 and He, a mixed gas of Cl2 and Ar, or a mixed gas of CF4 and O2. In the case where the work function metal 4 is composed of a material containing C, O, N, etc. in TiA1 or TiA1, in the etching gas, for example, it is preferred to use a mixed gas of CF4 and Cl2, a mixed gas of CF4 and HCl, or a mixed gas in which gases such as Ar, He, and N2 are added to these gases. By this etching, the work function metal 4 remaining on the gate sidewall spacer 6 through the gate insulating film 3 is removed ( Figure 7B ). The etching amount in this step is adjusted to 1 to 2 times the film thickness of the work function metal 4, and the etching time is controlled in such a way that the work function metal 4 on the channel is not removed. Fig. 7A as well as Figure 7B In FIG. 4 , only the work function metal 4 is removed, but in FIG. Figure 6B When the gate embedded metal 5 in addition to the work function metal 4 also remains on the sidewall of the sidewall spacer 6, the remaining gate embedded metal 5 is also removed in this step. Fig. 7A as well as Figure 7B The process shown is equivalent to Fig.12 The work function of the process flow chart is controlled by isotropic etching of the metal film 104, preferably followed by Fig. 6A as well as Figure 6B The first protective insulating film vertical etching 103 shown is performed continuously in the chamber of the same apparatus.

[0094] exist Fig. 8A as well as Figure 8BIn this case, using the ALD method, the second protective insulating film 11 is deposited on the first protective insulating film 10. Through this process, a stacked film of the protective insulating film composed of the first protective insulating film 10 and the second protective insulating film 11 is formed. In the stacked film of the protective insulating film, the first protective insulating film 10 is on the lower layer side, and the second protective insulating film 11 is on the upper layer side. The insulating film material of the second protective insulating film 11 and the insulating film material of the first protective insulating film 10 are set to different insulating film materials. The second protective insulating film 11 is deposited on the side wall and the upper surface of the first protective insulating film 10, the upper surface and the side wall of the hard mask 9, the upper surface and the side wall of the gate insulating film 3, the side wall of the gate buried metal 5, the side wall of the work function metal 4, the upper surface of the gate sidewall spacer 6, the upper surface of the etch stop layer 7, and the upper surface of the interlayer insulating film 8 of the source / drain region. The horizontal film thickness ( Fig. 8A t3 of Figure 8B and Fig. 7A and Figure 7B shown) of the second protective insulating film 11 is preferably equal to the horizontal film thickness t1 or t1' of the first protective insulating film 10 (t3 = t1, t3' == t1'), or set to be thinner (t3 < t1, t3' < t1'). When the film thicknesses t1 and t1' are, for example, 2 nm to 3 nm, the film thicknesses t3 and t3' are, for example, expected to be 1 nm to 3 nm. The second protective insulating film 11 is also deposited on the eaves formed at the lower part of the first protective insulating film 10, and up to Fig. 8A ), and on the side walls of the work function metal 4 and the gate buried metal 5 in the lower region of the first protective insulating film 10 exposed until the process shown in Figure 8B ), and on the side walls of the gate insulating film 3 ( Fig. 8A ). In addition, since the second protective insulating film 11 is deposited isotropically, in the lower part of the eaves of the first protective insulating film 10, the film formation in the vertical direction from the lower part of the eaves overlaps with the film formation in the horizontal direction from the side walls of the work function metal 4 and the gate buried metal 5 ( Figure 8B ) or the side walls of the gate insulating film 3 ( Fig. 8A t4 of Figure 8B and Fig. 8A t3 of Figure 8B and Fig. 8A t5 of Figure 8B The thickness t5') is equal to the sum of the thickness t3 (or t3') and the thickness t1 (or t1') (t3+t1=t5, t3'+t1'=t5'), or is smaller than the sum of the thickness t3 (or t3') and the thickness t1 (or t1') (t3+t1>t5, t3'+t1'>t5'). In the second protective insulating film 11, a film that can be isotropically formed with good controllability even for complex shapes with finer bumps can be used. The second protective insulating film 11 is, for example, an aluminum oxide (Al2O3) film or an aluminum oxynitride (AlON) film based thereon. When forming the Al2O3 film, it is preferred to use, for example, trimethylaluminum (Trimethylaluminum [TMA]: Al(CH3)3) as the raw material of aluminum (Al), and to use vaporized water (H2O) as the raw material of oxygen. The precursor composed of Al(CH3)3 has high reactivity with the hydroxyl groups (OH groups) formed on the surface by the H2O supply, so the Al2O3 film can be formed with good coverage even on the surface with unevenness. Fig. 8A as well as Figure 8B The second protective insulating film 11 may be formed isotropically also inside the pattern. It should be noted that an oxide film or a nitride film without Al may be used as the second protective insulating film 11, and the film may be formed by a CVD method or the like. Fig. 8A as well as Figure 8B The process shown is equivalent to Fig.12 The second protective insulating film deposition 105 of the process flow chart is preferably followed by Fig. 7A as well as Figure 7B The work function controlled metal film isotropic etching 104 shown is performed continuously in the chamber of the same apparatus.

[0095] Next, in Fig. 9A as well as Fig. 9B In the process shown, the second protective insulating film 11 is etched in the vertical direction. The etching is performed under selective etching conditions relative to the first protective insulating film 10, the hard mask 9, the gate insulating film 3, the gate sidewall spacer 6, the etching stop layer 7, and the interlayer insulating film 8. For example, when the second protective insulating film 11 is an Al2o3 film, it is preferred to use BCl3, a mixed gas of BCl3 and Cl2, or a gas in which argon Ar, N2, O2 are mixed with these, or a gas based on these. By this etching, the upper surface of the gate insulating film 3 is exposed. Fig. 8AAs shown, in the structure before this etching process, below the eaves formed by the first protective insulating film 10, the horizontal film thickness of the second protective insulating film 11 is formed to be thinner than the total horizontal film thickness of the first protective insulating film 10 and the second protective insulating film 11 above the eaves (t4 < t3 + t1). Therefore, in this etching process, below the eaves, the sidewall of the second protective insulating film 11 is substantially protected by the eaves formed by the first protective insulating film 10. Even when ions generated by the etching gas are incident in a direction inclined with respect to the direction perpendicular to the substrate 1, the ions are substantially reflected by the sidewall of the first protective insulating film 10 and change the angle ( Fig. 9A a1). Therefore, the etching gas ions do not reach the sidewall of the second protective insulating film 11 below the eaves, and the second protective insulating film 11 is not etched below the eaves. Through the above process, the upper opening of the gate insulating film 3 can be formed while protecting the sidewalls of the work function metal 4 and the gate buried metal 5 in the cutting area. Fig. 9A and Fig. 9B The present process shown is equivalent to Fig.12 the second protective insulating film vertical etching 106 in the process flow chart, and preferably followed by Fig. 8A and Figure 8B the second protective insulating film deposition 105 shown, and is continuously carried out in the chamber of the same device. It should be noted that Fig.12 the cyclic processes shown in processes 102 - 103, 105 - 106 (the gas and film formation conditions can also be changed) are not limited to two cycles, and can also be repeated more times. That is, when the combination of the film formation process (102, 105) and the etching process (103, 106) is considered as one cyclic process, in Fig.12 , it means that the combination of the film formation process and the etching process is implemented for two cycles (the first cycle is process 102 and process 103, and the second cycle is process 105 and process 106), and the process 104 for removing the work function metal 4 is sandwiched between the first cyclic process and the second cyclic process. In the first cyclic process (process 102 and process 103) and the second cyclic process (process 105 and process 106), the gas and film formation conditions can also be changed. In addition, the number of cyclic processes is not limited to two cycles, and can also be repeated multiple times as multiple cycles. In this case, the process 104 for removing the work function metal 4 is implemented once or multiple times, but it is not necessary to implement it every time between each cyclic process.

[0096] In Fig. 10A and Fig. 10BIn the process shown, the gate insulating film 3 is isotropically etched. The above etching is performed under selective etching conditions relative to the second protective insulating film 11, the first protective insulating film 10, the hard mask 9, the STI insulating film 2, the gate sidewall spacer 6, the etching stop layer 7, and the interlayer insulating film 8. When this etching is implemented, the side walls of the work function metal 4 and the gate buried metal 5 are covered by the first protective insulating film 10 and the second protective insulating film 11, so there is no need to consider the etching selectivity relative to these metals (4, 5). In the etching gas, for example, CF4, or a mixed gas of Cl2, hydrogen hydride (HBr) and O2, or these are preferably used as the reference gas. The etching amount in this process is adjusted to about 1 to 2 times the film thickness of the gate insulating film 3, and the etching time is controlled in such a way that the gate insulating film 3 on the channel is not removed. Fig. 10A as well as Fig. 10B The process shown is equivalent to Fig.12 The gate insulating film isotropically etched 107, preferably followed by Fig. 9A as well as Fig. 9B The second protective insulating film vertical etching 106 is shown to be performed continuously in the chamber of the same apparatus.

[0097] exist Fig.11A as well as Fig. 11BIn the process shown, the second protective insulating film 11 and the first protective insulating film 10 are removed in sequence by isotropic etching. The etching of the second protective insulating film 11 is performed under selective etching conditions relative to the first protective insulating film 10, the hard mask 9, the gate insulating film 3, the work function metal 4, the gate buried metal 5, the STI insulating film 2, the gate sidewall spacer 6, the etching stop layer 7, and the interlayer insulating film 8. For example, when the second protective insulating film 11 is an Al2O3 film, it is preferred to use a mixed gas of O2, BCl3 and Ar, or a gas based thereon, in the etching gas. This etching is performed for 1 to 2 times the etching time required to etch the film thickness of the second protective insulating film 11, and is performed under the condition that the second protective insulating film 11 is substantially completely removed. Following the second protective insulating film 11, the first protective insulating film 10 is removed by isotropic etching. This etching is performed under selective etching conditions relative to the hard mask 9, the gate insulating film 3, the work function metal 4, the gate buried metal 5, the STI insulating film 2, the gate sidewall spacer 6, the etching stop layer 7, and the interlayer insulating film 8. For example, when the protective insulating film 10 is a Si3N4 film, it is preferred to use a gas such as CHF3 or difluoromethane (CH2F2) or fluoromethane (CH3F), or a mixed gas of fluorocarbon gases such as CF4, C4F8 and H2, or a gas based on them in the etching gas. Similar to the etching of the second protective insulating film 11, this etching is performed for 1 to 2 times the etching time required to etch the thickness of the first protective insulating film 10, and is performed under the condition that the first protective insulating film 10 is substantially completely removed. Through this process, the side walls of the work function metal 4 and the side walls of the gate buried metal 5 ( Fig.11A ) and the sidewalls of the gate insulating film 3 on the gate sidewall spacer 6 ( Fig. 11B ) is exposed. The sidewalls of the work function metal 4 and the gate buried metal 5 exposed in this process ( Fig.11A ) In its lower part, the opening width of the cut pattern with the work function metal 4 and the gate insulating film 3 is wider than the opening width of the cut pattern covered by the gate buried metal 5 and is curved. This shape contributes to good embedding and isotropic film deposition when the cut region is filled with an insulating film to form a plug structure in the subsequent process, so the film density of the insulating film used for the plug formation in the bottom of the cut region is kept constant. Therefore, it also brings about the effect of suppressing the generation of cavities in the plug caused by the reduction of film density. Fig.11A as well as Fig. 11B The process shown is equivalent to Fig.12 The first / second protective insulating film isotropically etched 108, preferably followed by Fig. 10A as well as Fig. 10B The gate insulating film isotropic etching 107 shown in FIG. 1 is performed continuously in the chamber of the same device. Fig.12 Gate metal vertical etching 101 ( Figure 4A , Figure 4B ) to the first / second protective insulating film isotropically etched 108 ( Fig.11A , Fig. 11B ) are performed continuously in the chamber of the same apparatus.

[0098] By implementing the process consisting of this continuous process, in the metal gate cutting process using selective etching of Fin-type FET or GAA-type FET, the gate can be cut without generating metal residues such as work function metal 4 and gate buried metal 5 on the side wall of the gate sidewall spacer 6 in the gate cutting area, and the distance between the plug that insulates and separates the gates from each other and the channel of the FET can be shortened.

[0099] Considering the insulation and process stability of the insulating film plug formed in the gate cut region, the gate insulating film 3 remaining on the sidewall of the gate sidewall spacer 6 in the gate cut region may also be removed before the insulating film plug is formed. Fig.11A as well as Fig. 11B In the process shown in FIG. 1 , the gate insulating film 3 is continuously removed by isotropic etching in the same device, or by Figures 13A to 15A as well as Figure 13B to Figure 15B In the process shown, the gate insulating film 3 remaining on the side wall of the gate sidewall spacer 6 is removed while protecting the gate insulating film 3 opened at the lower portion of the gate cut region.

[0100] In the process of removing the gate insulating film 3 remaining on the side wall of the gate sidewall spacer 6 while protecting the gate insulating film 3 opened at the lower part of the gate cut region, first, a coating film such as a spin-on carbon film as an organic film is used to fill the groove formed in the gate cut region, and then the carbon film is etched a constant amount in the vertical direction to obtain Fig.13A as well as Fig. 13B The structure shown. Here, the upper end of the etched carbon film 12 is located at a position higher than the boundary position of the work function metal 4 and the gate insulating film 3 at the side wall of the gate cut region, and the etching amount of the carbon film 12 is adjusted in such a manner that a portion of the gate insulating film 3 remaining on the side wall of the gate sidewall spacer 6 is exposed. The gate insulating film 3 remaining on the side wall of the above-mentioned gate sidewall spacer 6 is expected to be exposed as deep as possible in the gate cut region. Therefore, after the etching of the above-mentioned carbon film 12, the height of the carbon film 12 remaining on the STI insulating film 2 is preferably adjusted to about 3nm to 10nm when the film thickness of the gate insulating film 3 is 1nm to 3nm. Through this process, the gate insulating film 3 ( Fig.13A ) is protected by the carbon film 12.

[0101] exist Fig.14Aas well as Fig. 14B In the process shown in FIG. 1 , the gate insulating film 3 is isotropically etched to remove the gate insulating film 3 remaining on the sidewall of the gate sidewall spacer 6 ( Fig. 14B ). The above etching is performed under selective etching conditions relative to the hard mask 9, STI insulating film 2, work function metal 4, gate buried metal 5, gate sidewall spacer 6, etching stop layer 7, and interlayer insulating film 8. Etching can be done by wet etching or dry etching. In the case of wet etching, for example, when the gate insulating film 3 is HfO2, a solution such as hydrofluoric acid (HF) is used. In the case of dry etching, a mixed gas of Cl2, HBr and O2 is used in the etching gas, or they are used as a reference gas. The etching amount in this process is adjusted to about 1 to 5 times the film thickness of the gate insulating film 3, and the etching time is controlled in such a way that the gate insulating film 3 on the channel is not removed.

[0102] Next, in Fig.15A as well as Fig. 15B In the process shown, for example, ashing is performed in an oxygen plasma atmosphere to remove the carbon film 12. Fig.13A as well as Fig. 13B The vertical etching process of the carbon film 12 is shown to Fig.15A as well as Fig. 15B The removal process of the carbon film 12 shown in the figure is continuously carried out in the chamber of the same device. The device used at this time may also be the same as the one used for the removal process from the carbon film 12. Fig.12 Gate metal vertical etching 101 ( Figure 4A , Figure 4B ) to the first / second protective insulating film isotropically etched 108 ( Fig.11A , Fig. 11B ) is the same device as the device of FIG.

[0103] By using a plasma processing device equipped with an ALD film forming function and anisotropic and isotropic etching control functions, it is possible to continuously process from Fig.12 Gate metal vertical etching 101 ( Figure 4A , Figure 4B ) to the first / second protective insulating film isotropically etched 108 ( Fig.11A , Fig. 11B ) and vertically etching the carbon film 12 ( Fig.13A and Fig. 13B ) to remove the etching of carbon film 12 ( Fig.15A and Fig. 15BThe plasma processing apparatus may be an etching apparatus using inductively coupled plasma (ICP: Inductively Coupled Plasma), an etching apparatus using capacitively coupled plasma (CCP: Capacitively Coupled Plasma), or an etching apparatus using microwave electron cyclotron resonance (ECR: Electron Cyclotron Resonance) plasma.

[0104] As an example, in Fig.16 2 shows the structure of a plasma processing device 200 using microwave ECR plasma. The plasma processing device 200 has a processing chamber (chamber) 201, and the processing chamber 201 is connected to a vacuum exhaust device (not shown) via a vacuum exhaust port 202. During the plasma processing, the processing chamber 201 is maintained at a vacuum of about 0.1Pa to 10Pa. In addition, a window portion 203 having the function of allowing microwaves to pass through and the function of airtightly sealing the processing chamber 201 and a porous plate 204 for shielding ions are arranged in the processing chamber 201. The processing chamber 201 is divided into an upper portion 201A of the processing chamber 201 and a lower portion 201B of the processing chamber 201 by the porous plate 204. The material of the window portion 203 is composed of a material that transmits microwaves, for example, a dielectric such as quartz. The porous plate 204 has a plurality of holes, and the material of the porous plate 204 is preferably composed of a dielectric such as quartz or alumina.

[0105] The gas supply mechanism has a gas source 205, a gas supply device 206, and a gas inlet 207, and supplies a raw material gas for plasma processing. The gas source 205 has a plurality of gas types required for processing. The gas supply device 206 has a control valve for controlling the supply and cutoff of the gas and a mass flow controller for controlling the gas flow rate. In addition, the gas inlet 207 is provided between the window 203 and the porous plate 204.

[0106] A waveguide 209 for propagating electromagnetic waves is connected to the upper part of the processing chamber 201, and a high-frequency power supply 208 for plasma generation as a high-frequency power supply is connected to the end of the waveguide 209. The high-frequency power supply 208 for plasma generation is a power supply for generating electromagnetic waves for plasma generation, and for example, microwaves with a frequency of 2.45 GHz are used as electromagnetic waves. The microwaves generated by the high-frequency power supply 208 for plasma generation propagate through the waveguide 209 and enter the processing chamber 201. The waveguide 209 has a vertical waveguide extending in the vertical direction and a waveguide converter that also serves as a corner that bends the direction of the microwave by 90 degrees, so that the microwaves are vertically incident on the processing chamber 201. The microwaves propagate vertically in the processing chamber 201 through the window 203. The magnetic field generating coil 210 arranged on the periphery of the processing chamber 201 forms a magnetic field in the processing chamber 201. The microwaves oscillated from the high-frequency power supply 208 for plasma generation interact with the magnetic field formed by the magnetic field generating coil 210, thereby generating high-density plasma in the processing chamber 201.

[0107] Below the processing chamber 201, a sample table 212 is arranged opposite to the window portion 203. The material of the sample table 212 is, for example, aluminum or titanium. The sample table 212 places and holds a semiconductor substrate 211 as a sample on the upper surface. Here, the central axes of the waveguide 209, the processing chamber 201, the sample table 212, and the semiconductor substrate 211 are consistent. In addition, an electrode for electrostatically adsorbing the semiconductor substrate 211 is provided inside the sample table 212, and the semiconductor substrate 211 is electrostatically adsorbed to the sample table 212 by applying a DC voltage. In addition, a high-frequency voltage is applied to the sample table 212 from an isotropic and anisotropic high-frequency bias power supply 213 for controlling etching. The frequency of the applied high-frequency bias is preferably set to 400 kHz, for example.

[0108] Each mechanism of the plasma processing device 200 is controlled by a control signal 221 from the control unit 220. The control unit 220 controls each mechanism by instructing the execution of a prescribed action using the control signal 221 according to the processing conditions (anisotropic etching processing, isotropic etching processing, ALD film forming processing, etc.) executed by the plasma processing device 200. For example, the control unit 220 controls the high-frequency power supply 208 for plasma generation to control the on-off of the electromagnetic wave used for plasma generation. In addition, the control unit 220 controls the gas supply mechanism to adjust the type and flow rate of the gas introduced into the processing chamber 201. The control unit 220 also controls the high-frequency bias power supply 213 to control the intensity of the high-frequency voltage applied to the semiconductor substrate 211 on the sample stage 212.

[0109] When anisotropic etching is performed using the plasma processing apparatus 200, the control unit 220 controls the magnetic field generating coil 210 so as to generate plasma in the lower portion 201B of the processing chamber 201 below the porous plate 204. The porous plate 204 is formed of a dielectric, so microwaves pass through the porous plate 204 and interact with the magnetic field in the lower portion 201B of the processing chamber 201 to generate plasma. In addition, a high-frequency bias is applied to the sample stage 212 on which the Si substrate 1 as the semiconductor substrate 211 is placed. As a result, the ions in the plasma are pulled toward the Si substrate 1 without being blocked by the porous plate 204 and the like, and anisotropic etching can be performed while maintaining verticality.

[0110] When isotropic etching is performed using the plasma processing apparatus 200, the control unit 220 controls the magnetic field generating coil 210 so that the plasma generation position is the upper portion 201A of the processing chamber 201 above the porous plate 204. Since the ions in the plasma generated in the upper portion 201A of the processing chamber 201 are shielded by the porous plate 204, only the radicals in the plasma are supplied to the lower portion 201B of the processing chamber 201. Thus, isotropic etching using radicals can be performed.

[0111] When the plasma processing apparatus 200 is used to form a film using the ALD method, it is preferred to apply the following cyclic process based on the control of the control unit 220. For example, when forming a Si3N4 film using the ALD method, BTBAS or BDEAS is used as a raw material of Si, or SiH2Cl2 is used as a gaseous gas. When BTBAS or BDEAS is used as a liquid raw material, the liquid raw material is vaporized and sent to the gas line as a gaseous gas. The gaseous gas of the raw material is sent into the processing chamber 201 together with Ar as a carrier gas, and is adsorbed on the surface of the substrate as a precursor of Si. Thereafter, a cleaning gas such as Ar gas is used to exhaust unnecessary precursors in the processing chamber 201. Next, N2 gas or a mixed gas of N2 gas and H2 gas, or a gas containing nitrogen such as NH3 gas is flowed into the processing chamber 201 to be plasmatized and react with the surface of the substrate. After that, an inactive gas such as Ar is flowed into the processing chamber 201 again to clean the processing chamber 201, and unnecessary gases in the processing chamber 201 are exhausted. Through this series of processes, in principle, a Si3N4 film with a film thickness at the atomic layer level is deposited on the surface of the substrate. By repeatedly implementing this series of processes (implementation of a cyclic process), an insulating film of a thin film is formed using the ALD method. For example, in the case of forming an Al2O3 film using the ALD method, it is preferred to use Al(CH3)3 as the precursor of Al and vaporized H2O as the raw material of oxygen, and implement the same cyclic process as the above-mentioned Si3N4 case to form the Al2O3 film.

[0112] [Example 2]

[0113] In Example 2, a process of continuously performing the metal gate cutting process in Example 1 in a chamber of the same device is provided. Fig.12 The process flow of cutting the metal gate is as follows: Fig.13A , FIG. 13B to FIG. 15A , Fig. 15B The method of the step of removing the gate insulating film 3 remaining on the side wall of the gate side wall spacer 6 is shown.

[0114] Figures 17A to 19A The gate region of the transistor in the direction parallel to the gate (the gate region of the first embodiment) is shown in a series of steps of removing the gate insulating film remaining on the gate sidewall spacer in the above-mentioned metal gate cutting process. Figure 1 as well as Figure 2 A cross-sectional view taken along line AA' of FIG. Figures 17B to 19B The gate cutting region in the direction perpendicular to the gate (the gate cutting region of Example 1) is shown in a series of steps for removing the gate insulating film remaining on the gate sidewall spacer in the above-mentioned metal gate cutting process. Figure 1 as well as Figure 2 A cross-sectional view taken along line BB' of FIG. Fig. 20 The present invention is to show that the method of manufacturing the product from Example 1 is carried out by a series of manufacturing steps using the same device. Fig.12 The metal gate cutting process shown in Figures 17A to 19A as well as Figures 17B to 19B FIG. 1 is a flow chart of a process for removing the gate insulating film remaining on the gate sidewall spacer.

[0115] In Example 1 Fig.11A as well as Fig. 11B In the structure shown in FIG. 1 , a third protective insulating film 310 is deposited by using a film forming technique such as an ALD method to obtain Fig.17A as well as Fig. 17B The structure shown. The above-mentioned protective insulating film 310 is deposited on the upper surface and side walls of the hard mask 309, the upper surface and side walls of the gate insulating film 303, the side walls of the gate buried metal 305, the side walls of the work function metal 304, and the upper surface of the gate sidewall spacer 306, the upper surface of the etching stop layer 307, and the upper surface of the interlayer insulating film 308 in the source / drain region. The material of the protective insulating film 310 is preferably set to, for example, Si3N4 film or SiON film based thereon, or SiO2 film, Al2O3 film, etc. In the case where the protective insulating film 310 is, for example, Si3N4 film, BTBAS or BDEAS, or SiH2Cl2 is used as the raw material of Si, and N2 gas or a mixed gas of N2 gas and hydrogen H2 gas, or NH3 gas, etc. is used as the raw material of nitrogen. Figure 5A as well as Figure 5BSimilarly to the process shown, in this process, the gate cut region where the third protective insulating film 310 is deposited has a width of about 10nm to 30nm and a depth of about 50nm to 200nm, forming a narrow and deep pattern. Therefore, at the bottom of the gate cut region, assuming that the film formation from the sidewalls and the bottom surface contributes, the film thickness of the third protective insulating film 310 in the vertical direction at the bottom is thicker than the film thickness of the third protective insulating film 310 in the horizontal direction on the sidewalls of the pattern. When the film thickness of the third protective insulating film 310 in the horizontal direction on the sidewalls of the pattern is set to 2nm to 3nm, for example, the film thickness of the third protective insulating film 310 in the vertical direction at the bottom of the groove becomes 3nm to 6nm, for example. In this way, the phenomenon that the film thickness of the third protective insulating film 310 in the vertical direction from the bottom of the gate cut region is thicker than the film thickness of the third protective insulating film 310 in the horizontal direction on the sidewalls of the pattern can also be intentionally generated by controlling the plasma conditions of the above-mentioned ALD method. For example, when a Si3N4 film is formed as the third protective insulating film 310, after a raw material gas of Si is supplied to the substrate and a precursor of Si is formed on the substrate surface, when a gas containing nitrogen is plasma-formed and reacts with the substrate surface, the formation of the Si3N4 film only in the direction perpendicular to the substrate 301 can be promoted by controlling conditions such as a high-frequency bias applied to the substrate. Thus, the film thickness of the third protective insulating film 310 in the vertical direction from the bottom of the gate cut region can be made thicker than the film thickness of the third protective insulating film 310 in the horizontal direction on the pattern sidewall. In this case, the film thickness of the third protective insulating film 310 at the uppermost surface of the structure such as the upper surface of the hard mask 309 is also thicker than the film thickness of the third protective insulating film 310 in the horizontal direction on the pattern sidewall. When the film thickness of the third protective insulating film 310 in the horizontal direction on the pattern sidewall is set to, for example, 2nm to 3nm, the film thickness of the third protective insulating film 310 in the vertical direction at the bottom of the groove can be increased to, for example, 5nm to 10nm or more. Fig.17A as well as Fig. 17B The process shown is equivalent to Fig. 20 The third protective insulating film deposition 409 of the process flow chart is preferably followed by a series of steps from the gate metal vertical etching 401 to the first / second protective insulating film isotropic etching 408 (equivalent to the first embodiment Fig.12 The continuous processes from 101 to 108 are continuously carried out in the chamber of the same device.

[0116] exist Fig.18A as well as Fig.18BIn the process shown, the third protective insulating film 310 is isotropically etched to remove the third protective insulating film 310 deposited on the side wall of the gate cut region. The above etching is performed under selective etching conditions relative to the hard mask 309, the gate insulating film 303, the work function metal 304, the gate buried metal 305, the gate sidewall spacer 306, the etching stop layer 307, and the interlayer insulating film 308. For example, when the third protective insulating film 310 is a Si3N4 film, it is preferred to use a gas such as CHF3, CH2F2, or CH3F, or a mixed gas of a gas such as CF4, C4F8 and H2, or a gas based on them in the etching gas. This etching is performed under the condition that the third protective insulating film 310 remains on the bottom surface of the gate cut region after etching. In addition, the etching amount is adjusted in such a way that the upper end of the third protective insulating film 310 remaining after etching becomes a position higher than the boundary position of the work function metal 304 and the gate insulating film 303 at the side wall of the gate cut region. For example, when the film thickness of the gate insulating film 303 is 1 nm to 3 nm, it is preferable to adjust the etching time so that the film thickness of the third protective insulating film 310 remaining at the bottom of the gate cut region becomes about 3 nm to 7 nm. The film formation amount and etching amount of the third protective insulating film 310 are adjusted so that the above conditions are satisfied when the etching time is set to 1 to 1.5 times the film thickness of the formed third protective insulating film 310. Through this process, the gate insulating film 303 existing at the bottom of the work function metal 304 is protected by the third protective insulating film 310. Fig.18A as well as Fig.18B The process shown is equivalent to Fig. 20 The third protective insulating film isotropically etched 410 of the process flow chart is preferably followed by Fig.17A as well as Fig. 17B The third protective insulating film deposition 409 is shown to be performed continuously in the chamber of the same apparatus.

[0117] Here, Fig.17A as well as Fig. 17B , Fig.18A as well as Fig.18B It can be considered to correspond to the bottom protection insulating film forming process. The bottom protection insulating film forming process is a process for forming the third protection insulating film 310 by forming a third protection insulating film 310 and isotropically etching the third protection insulating film 310 so that only the bottom of the gate cut region is protected by the third protection insulating film 310. Since the third protection insulating film 310 is formed in a manner to protect only the bottom of the gate cut region, the third protection insulating film 310 that protects the bottom of the gate cut region can be referred to as the bottom protection insulating film. Therefore, Fig.13A as well as Fig. 13BThe carbon film 12 after etching shown can also be regarded as a bottom protective insulating film similar to the third protective insulating film 310 .

[0118] Next, in Fig.19A as well as Fig.19B In the process shown in FIG. 1 , the gate insulating film 303 is isotropically etched to remove the gate insulating film 303 remaining on the sidewall of the gate sidewall spacer 306 ( Fig.19B ). The above etching is performed under selective etching conditions relative to the third protective insulating film 310, the hard mask 309, the STI insulating film 302, the work function metal 304, the gate buried metal 305, the gate sidewall spacer 306, the etching stop layer 307, and the interlayer insulating film 308. In the case of dry etching for this etching, for example, when the gate insulating film 303 is HfO2, a mixed gas of Cl2, HBr and O2 is used in the etching gas, or they are used as a reference gas. The etching amount in this process is adjusted to about 1 to 5 times the film thickness of the gate insulating film 303, and the etching time is controlled in a manner that the gate insulating film 303 on the channel is not removed. Fig.19A as well as Fig.19B The process shown is equivalent to Fig. 20 The process flow chart of the gate insulating film removal etching 411, preferably followed by Fig.18A as well as Fig.18B The third protective insulating film isotropic etching 410 shown is performed continuously in the chamber of the same apparatus.

[0119] then Fig.19A as well as Fig.19B In the process shown, the third protective insulating film 310 is removed by isotropic etching. This etching is performed under selective etching conditions relative to the hard mask 309, the gate insulating film 303, the work function metal 304, the gate buried metal 305, the STI insulating film 302, the gate sidewall spacer 306, the etching stop layer 307, and the interlayer insulating film 308. For example, in the case where the third protective insulating film 310 is a Si3N4 film, it is preferred to use gases such as CHF3, CH2F2, or CH3F in the etching gas, or a mixed gas of gases such as CF4, C4F8 and H2, or a gas based on them. This etching is performed for 1 to 2 times the etching time required to etch the thickness of the third protective insulating film 310, and is performed under the condition that the third protective insulating film 310 is substantially completely removed. This process is equivalent to Fig. 20 The third protective insulating film isotropically etched 412 of the process flow chart is preferably followed by Fig.19A as well as Fig.19B The gate insulating film removal etching 411 shown in the figure is continuously performed in the chamber of the same device. Fig.15A as well as Fig. 15B The structure shown is equivalent to the structure shown.

[0120] In this embodiment, the process can be performed in a continuous process in the chamber of the same device. Fig. 20 The process flow shown in FIG. 1 is from the gate metal vertical etching 401 to the third protective insulating film isotropic etching 412. That is, the process of Example 1 can be performed as a series of continuous processes in the same device without removing the substrate from the device. Fig.12 The process shown in the flow chart includes the metal gate cutting process and the subsequent step of removing the gate insulating film 303 remaining on the sidewall of the gate sidewall spacer 306.

[0121] [Example 3]

[0122] In the third embodiment, the metal gate cutting process in the first embodiment is provided. Fig.13A , FIG. 13B to FIG. 15A , Fig. 15B The method shown is a method of protecting the side walls of the work function metal 4 and the gate embedded metal 5 in the gate cut region during the step of removing the gate insulating film 3 remaining on the side walls of the gate sidewall spacer 6.

[0123] Figures 21A to 22A The gate region of the transistor in the direction parallel to the gate (the gate region of the first embodiment) is shown in a series of steps of removing the gate insulating film remaining on the gate sidewall spacer in the above-mentioned metal gate cutting process. Figure 1 as well as Figure 2 A cross-sectional view taken along line AA' of FIG. Figure 21B to Figure 22B The gate cutting region in the direction perpendicular to the gate (the gate cutting region of Example 1) is shown in a series of steps for removing the gate insulating film remaining on the gate sidewall spacer in the above-mentioned metal gate cutting process. Figure 1 as well as Figure 2 A cross-sectional view taken along line BB' of FIG.

[0124] In Example 1 Fig. 10A as well as Fig. 10B In the structure shown in the figure, a coating film such as a spin-coated carbon film is used to fill the groove formed in the gate cutting area, and then the above carbon film is etched a constant amount in the vertical direction to obtain Fig.21A as well as Fig.21B Here, the etching amount of the carbon film 512 is adjusted so that the upper end of the etched carbon film 512 is located at a position higher than the boundary position of the work function metal 504 and the gate insulating film 503 at the side wall of the gate cut region and becomes a position where the second protective insulating film 511 is exposed. For example, the height of the carbon film 512 remaining on the STI insulating film 502 after etching is preferably adjusted to about 3nm to 20nm. Through this process, the gate insulating film 503 existing at the lower part of the work function metal 504 is protected by the carbon film 512.

[0125] exist Fig.22A as well as Fig. 22B In the process shown in FIG. 1 , the gate insulating film 503 is etched to remove the gate insulating film 503 remaining on the side wall of the gate side wall spacer 506 ( Fig. 22B ). The above etching is performed under selective etching conditions relative to the carbon film 512, the second protective insulating film 511, the first protective insulating film 510, the hard mask 509, the STI insulating film 502, the gate sidewall spacer 506, the etching stop layer 507, and the interlayer insulating film 508. In order to avoid excessive etching of the gate insulating film 503 in the horizontal direction, this etching is mainly performed under vertical etching conditions using dry etching, and only the residues that cannot be completely removed by vertical etching alone are removed by isotropic etching. For example, in the case where the gate insulating film 503 is HfO2, a mixed gas of Cl2, HBr and O2 is used in vertical etching and isotropic etching, or they are used as reference gases. In order to make the etching selectivity relative to other materials higher, in the above etching, a method of repeatedly performing a cycle of selectively depositing carbon-based materials on materials other than the gate insulating film 503 and etching the gate insulating film 503 while protecting these materials can also be used. In this case, it is preferred to use gases such as CH4 and CHF3 in the deposition process of the above-mentioned carbon-based materials. In this process, the etching amount of the gate insulating film 503 based on isotropic etching is adjusted to about 1 to 5 times the film thickness of the gate insulating film 503, and the etching time and the balance with the vertical etching time are controlled in such a way that the gate insulating film 503 on the channel is not removed.

[0126] Next, the carbon film 512 is removed by ashing, for example, in an oxygen plasma atmosphere, and the second protective insulating film 511 and the first protective insulating film 510 are removed in sequence by isotropic etching, thereby obtaining the same structure as in Example 1. Fig.15A as well as Fig. 15B The structure shown is equivalent to the structure shown.

[0127] Preferably, the process is carried out continuously in the same chamber of the apparatus. Fig.21A as well as Fig.21B The process of vertically etching the carbon film 512 shown in the figure to the process of sequentially removing the second protective insulating film 511 and the first protective insulating film 510. The device used at this time may be the same as the device used for vertically etching the gate metal (equivalent to the device used in the embodiment 1). Fig.12 101 of Example 1) to isotropic etching of the gate insulating film (equivalent to the step of Example 1 Fig.12 The same device as the device of step 107).

[0128] In this embodiment, when etching is performed to remove the gate insulating film 503 remaining on the gate sidewall spacer 506 in the gate cutting area, the second protective insulating film 511 and the first protective insulating film 510 are used to protect the side walls of the work function metal 504 and the side walls of the gate embedded metal 505, thereby preventing these metal layers (504, 505) from being etched.

[0129] [Example 4]

[0130] In Example 4, a series of steps of cutting the metal gate from the metal gate cutting process in Example 3 are continuously performed in the chamber of the same device (equivalent to the steps of Example 1). Fig.12 The process of removing the gate insulating film 503 remaining on the side wall of the gate side wall spacer 506 (a series of processes 101 to 107 of Example 3) is performed. Fig.22A as well as Fig. 22B ), and a method of removing the second protective insulating film 511 and the first protective insulating film 510.

[0131] Figures 23A to 25A The gate region of the transistor in the direction parallel to the gate (the gate region of the first embodiment) is shown in a series of steps of removing the gate insulating film remaining on the gate sidewall spacer in the above-mentioned metal gate cutting process. Figure 1 as well as Figure 2 A cross-sectional view taken along line AA' of FIG. Figure 23B to Figure 25B The gate cutting region in the direction perpendicular to the gate (the gate cutting region of Example 1) is shown in a series of steps for removing the gate insulating film remaining on the gate sidewall spacer in the above-mentioned metal gate cutting process. Figure 1 as well as Figure 2 A cross-sectional view taken along line BB' of FIG. Fig.26 The present invention shows a series of manufacturing steps using the same device to perform a series of steps from cutting the metal gate (equivalent to the first embodiment) Fig.12 101 to 107) to the step of removing the gate insulating film remaining on the side wall of the gate sidewall spacer, and removing the second protective insulating film and the first protective insulating film.

[0132] In Example 1 Fig. 10A as well as Fig. 10B In the structure shown in FIG. 1 , a third protective insulating film 612 is deposited by using a film forming technique such as an ALD method to obtain Fig.23A as well as Fig. 23BThe protective insulating film 612 is deposited on the upper surface and sidewalls of the hard mask 609, the sidewalls and upper surface of the first protective insulating film 610, the sidewalls and upper surface of the second protective insulating film 611, the upper surface and sidewalls of the gate insulating film 603, the upper surface of the gate sidewall spacer 606, the upper surface of the etching stop layer 607, and the upper surface of the interlayer insulating film 608 in the source / drain region. The material of the protective insulating film 612 is preferably, for example, a Si3N4 film or a SiON film based thereon, or a SiO2 film, an Al2O3 film, or the like. In the case where the protective insulating film 612 is, for example, a Si3N4 film, for example, BTBAS or BDEAS, or SiH2Cl2 is used as the raw material of Si, and N2 gas or a mixed gas of N2 gas and hydrogen H2 gas, or NH3 gas is used as the raw material of nitrogen. In this process, the gate cut region where the third protective insulating film 612 is deposited is assumed to have a depth of about 50 nm to 200 nm and a width of about 100 nm. Fig.17A as well as Fig. 17B (width of about 10nm to 30nm) is narrower (width of about 5nm to 20nm). At the bottom of the gate cut region having such a narrow and deep pattern, assuming that the film formation from the side walls and the bottom surface contributes, the film thickness of the third protective insulating film 612 in the vertical direction at the bottom is thicker than the film thickness in the horizontal direction on the side walls of the pattern. When the film thickness in the horizontal direction of the third protective insulating film 612 on the side walls of the pattern is set to 2nm to 3nm, for example, the film thickness in the vertical direction at the bottom of the groove becomes, for example, 3nm to 6nm. Similar to Example 2, such a phenomenon that the film thickness of the third protective insulating film 612 in the vertical direction from the bottom of the gate cut region is thicker than the film thickness in the horizontal direction of the third protective insulating film 612 on the side walls of the pattern can also be intentionally produced by controlling the plasma conditions of the above-mentioned ALD method. By using the method shown in Example 2, when the thickness of the third protective insulating film 612 in the horizontal direction on the pattern sidewall is set to 2nm~3nm, for example, the thickness of the third protective insulating film 612 in the vertical direction at the bottom of the groove can be increased to 5nm~10nm or more. Fig.23A as well as Fig. 23B The process shown is equivalent to Fig.26 The third protective insulating film deposition 708 of the process flow chart of the embodiment is preferably followed by a series of steps from the gate metal vertical etching 701 to the gate insulating film isotropic etching 707 (equivalent to the embodiment 1 Fig.12 The continuous processes from 101 to 107 are continuously carried out in the chamber of the same device.

[0133] exist Fig.24A as well as Fig. 24BIn the process shown, the third protective insulating film 612 is isotropically etched to remove the third protective insulating film 612 deposited on the side wall of the gate cut region. The above etching is performed under selective etching conditions relative to the hard mask 609, the first protective insulating film 610 and the second protective insulating film 611, the gate sidewall spacer 606, the etching stop layer 607, and the interlayer insulating film 608. For example, in the case where the third protective insulating film 612 is a Si3N4 film, it is preferred to use a gas such as CHF3, CH2F2, or CH3F in the etching gas, or a mixed gas of a gas such as CF4, C4F8 and H2, or a gas based on them. This etching is performed under the condition that the third protective insulating film 612 remains on the bottom surface of the gate cut region after etching. In addition, the etching amount is adjusted in such a way that the upper end of the third protective insulating film 612 remaining after etching becomes a position higher than the boundary position of the work function metal 604 and the gate insulating film 603 at the side wall of the gate cut region. For example, when the film thickness of the gate insulating film 603 is 1 nm to 3 nm, it is preferable to adjust the etching time so that the film thickness of the third protective insulating film 612 remaining at the bottom of the gate cut region becomes about 3 nm to 7 nm. The film formation amount and etching amount of the third protective insulating film 612 are adjusted so that the above conditions are satisfied when the etching time is set to 1 to 1.5 times the film thickness of the formed third protective insulating film 612. Through this process, the gate insulating film 603 existing at the bottom of the work function metal 604 is protected by the third protective insulating film 612. Fig.24A as well as Fig. 24B The process shown is equivalent to Fig.26 The third protective insulating film isotropically etched 709 of the process flow chart is preferably followed by Fig.23A as well as Fig. 23B The third protective insulating film deposition 708 shown is performed continuously in the chamber of the same apparatus. The third protective insulating film 612 can also be regarded as a bottom protective insulating film similar to the third protective insulating film 310 .

[0134] Next, in Fig.25A as well as Fig.25B In the process shown in FIG. 1 , the gate insulating film 603 is etched to remove the gate insulating film 603 remaining on the side wall of the gate side wall spacer 606 ( Fig.25B). The above etching is performed under selective etching conditions relative to the third protective insulating film 612, the second protective insulating film 611, the first protective insulating film 610, the hard mask 609, the STI insulating film 602, the gate sidewall spacer 606, the etching stop layer 607, and the interlayer insulating film 608. In order to avoid excessive etching of the gate insulating film 603 in the horizontal direction, this etching is mainly performed under vertical etching conditions using dry etching, and only the residues that cannot be completely removed by vertical etching alone are removed by isotropic etching. For example, in the case where the gate insulating film 603 is HfO2, a mixed gas of Cl2, HBr and O2, or these are used as reference gases in vertical etching and isotropic etching. In order to make the etching selectivity relative to other materials higher, in the above etching, a method of repeatedly performing a cycle of selectively depositing carbon-based materials on materials other than the gate insulating film 603 and etching the gate insulating film 603 while protecting these materials can also be used. In this case, it is preferred to use a gas such as CH4 or CHF3 in the deposition process of the carbon-based material. In this process, the etching amount of the gate insulating film 603 based on isotropic etching is adjusted to 1 to 5 times the film thickness of the gate insulating film 603, and the etching time and the balance with the vertical etching time are controlled in such a way that the gate insulating film 603 on the channel is not removed. Fig.25A as well as Fig.25B The process shown is equivalent to Fig.26 The process flow chart of the gate insulating film removal etching 710 is preferably followed by Fig.24A as well as Fig. 24B The third protective insulating film isotropic etching 709 shown is performed continuously in the chamber of the same apparatus.

[0135] Next, the third protective insulating film 612, the second protective insulating film 611, and the first protective insulating film 610 are removed in sequence by isotropic etching, thereby obtaining the same structure as in Example 1. Fig.15A as well as Fig. 15B The etching and removal methods of each film are the same as those of Examples 1 to 3. This step is equivalent to Fig.26 The first / second / third protective insulating film isotropically etched 711, preferably followed by Fig.25A as well as Fig.25B The gate insulating film removal etching 710 shown is performed continuously in the chamber of the same apparatus.

[0136] In this embodiment, the process can be performed in a continuous process in the chamber of the same device. Fig.26The process flow shown in FIG. 1 is from the gate metal vertical etching 701 to the first / second / third protective insulating film isotropic etching 711. That is, the series of steps of cutting the metal gate in Example 3 (equivalent to the steps of Example 1) can be performed as a series of continuous steps in the same device without removing the substrate from the device. Fig.12 A series of steps 101 to 107 of Example 3) to a step of removing the gate insulating film 503 remaining on the side wall of the gate side wall spacer 506 (a series of steps 101 to 107 of Example 3) Fig.22A as well as Fig. 22B ), and a process of removing the second protective insulating film 511 and the first protective insulating film 510.

[0137] Description of Reference Numerals

[0138] 1. 301. 501. 601. Semiconductor substrate; 2. 302. 502. 602. STI insulating film; 3. 303. 503. 603. High-k gate insulating film; 4. 304. 504. 604. Work function control metal (work function metal); 5. 305. 505. 605. Gate buried metal; 6. 306. 506. 606. Gate sidewall spacer; 7. 307. 507. 607. Etching stop layer; 8. 308. 508. 608. Source / drain region interlayer insulating film; 9. 309. 509. 609. Hard mask layer; 10. 510. 610. First protective insulating film; 11. 511. 612. 11: second protective insulating film; 12, 512: carbon film; 310, 612: third protective insulating film; 101, 401, 701: gate metal vertical etching process; 102, 402, 702: first protective insulating film deposition process; 103, 403, 703: first protective insulating film vertical etching process; 104, 404, 704: work function control metal film isotropic etching process; 105, 405, 705: second protective insulating film deposition process; 106, 406, 706: second protective insulating film vertical etching process; 107, 407, 707: gate insulating film isotropic etching process; 108, 408: first / second protective insulating film isotropic etching process; 40 9, 708: third protective insulating film deposition process; 410, 709: third protective insulating film isotropic etching process; 411, 710: gate insulating film removal etching process; 412: third protective insulating film isotropic etching process; 710: first / second / third protective insulating film isotropic etching process; 201: processing chamber (chamber); 201A: upper area of ​​the processing chamber; 201B: lower area of ​​the processing chamber; 202: vacuum exhaust port; 203: window; 204: porous plate; 205: gas source; 206: gas supply device; 207: gas inlet; 208: high-frequency power supply for plasma generation; 209: waveguide; 210: magnetic field generating coil; 211: semiconductor substrate ; 212: sample stage; 213: high-frequency bias power supply; 220: control unit; 221: control signal; t1: horizontal film thickness of the first protective insulating film on the side wall of the metal gate cut section; t1': horizontal film thickness of the first protective insulating film on the side wall of the gate sidewall spacer; t2, t2': vertical film thickness of the first protective insulating film at the bottom of the gate cut region; t3: horizontal film thickness of the second protective insulating film on the side wall of the metal gate cut section; t3': horizontal film thickness of the second protective insulating film on the side wall of the gate sidewall spacer; t4: horizontal film thickness of the second protective insulating film on the side wall of the metal gate cut section at the eaves formed by the first protective insulating film at the bottom of the gate cut region;t4': horizontal thickness of the second protective insulating film on the sidewall of the gate sidewall spacer at the bottom of the gate cut region formed by the first protective insulating film; t5, t5': vertical thickness of the second protective insulating film at the bottom of the gate cut region; θ1: angle between the sidewall of the metal gate cut section and the lower surface of the first protective insulating film after etching; θ1': angle between the sidewall of the gate sidewall spacer and the lower surface of the first protective insulating film after etching; a1: ion irradiation path when etching the second protective insulating film. ;

Claims

1. A method for manufacturing a semiconductor device, wherein a gate stack film is vertically cut and gates are insulated and separated from each other by an insulating film, wherein: The semiconductor device has the following structure: a channel structure is provided on a semiconductor substrate, the channel structure has a fin-shaped, filament-shaped or sheet-shaped channel, a gate stack film is formed on the channel by sequentially forming a gate insulating film and a metal layer, a gate structure formed by the gate stack film has a shape oriented in a direction perpendicular to the orientation direction of the channel, and a gate sidewall spacer is formed on a sidewall of the gate structure, The method for manufacturing a semiconductor device comprises: In a first step, the metal layer is etched in a vertical direction to form a groove-shaped cutting area; A second step is to deposit a protective insulating film on the sidewalls of the cut region formed by the etching; The third step is to anisotropically etch the protective insulating film in a vertical direction to expose the surface of the gate insulating film present at the bottom of the cutting area under the metal layer; A fourth step is to remove a portion of the metal layer by isotropic etching; A fifth step, in which the fourth step is sandwiched between the cyclic steps consisting of the second step and the third step as needed, and the cyclic steps are repeated multiple times using an insulating film material different from the protective insulating film, so that a laminated film of a protective insulating film consisting of the protective insulating film and a plurality of protective insulating films different from the protective insulating film is formed on the side wall of the cutting area; as well as In the sixth step, a portion of the gate insulating film exposed at the bottom of the dicing region is removed by etching.

2. The method for manufacturing a semiconductor device according to claim 1, wherein: The first step to the sixth step are continuously performed in the same plasma processing apparatus.

3. The method for manufacturing a semiconductor device according to claim 1, wherein: The film in contact with the side wall of the gate stacked film in the stacked film of the protective insulating film is composed of a silicon nitride film or a film based thereon, and the film located on the upper side of the stacked film of the protective insulating film is composed of aluminum oxide or a film based thereon.

4. The method for manufacturing a semiconductor device according to claim 1, wherein: After the third process of anisotropically etching the film in the stacked film of the protective insulating film that is in contact with the side wall of the gate stacked film, the side wall of the gate stacked film below the protective insulating film that is in contact with the side wall of the gate stacked film is exposed, and the side wall is covered by the stacked film of the protective insulating film formed in the fifth process.

5. The method for manufacturing a semiconductor device according to claim 1, wherein: After the sixth step, a seventh step is performed to remove the stacked film of the protective insulating film by isotropic etching. The first step to the seventh step are continuously performed in the same plasma processing apparatus.

6. The method for manufacturing a semiconductor device according to claim 5, wherein: After the seventh step, a gate insulating film removing step is performed to remove the gate insulating film remaining on the sidewall of the gate sidewall spacer by isotropic etching. The first step to the seventh step and the gate insulating film removal step are continuously performed in the same plasma processing apparatus.

7. The method for manufacturing a semiconductor device according to claim 5, wherein: After the seventh step, a step of coating an organic film, a step of etching the organic film in a direction perpendicular to the semiconductor substrate and controlling the etching amount in such a manner that the gate insulating film remaining on the side wall of the gate side wall spacer is exposed and the upper surface of the organic film is located at a position higher than the height of the gate insulating film at the bottom of the metal layer, a step of removing the gate insulating film remaining on the side wall of the gate side wall spacer by isotropic etching, and an organic film removal step of removing the organic film are performed. The steps of etching the organic film in the vertical direction and removing the organic film are continuously performed in the same plasma processing apparatus.

8. The method for manufacturing a semiconductor device according to claim 5, wherein: After the seventh step, a bottom protection insulating film forming step is performed in which an insulating film is formed and the insulating film is isotropically etched so that only the bottom of the cut region is protected by the insulating film, a gate insulating film isotropically etching step is performed in which the gate insulating film remaining on the side wall of the gate sidewall spacer is removed by isotropic etching, and a bottom protection insulating film isotropically etching step is performed in which the bottom protection insulating film is removed by isotropic etching. The first step to the seventh step and the step from the step of forming the bottom protective insulating film to the step of isotropically etching the bottom protective insulating film are continuously performed in the same plasma processing apparatus.

9. The method for manufacturing a semiconductor device according to claim 1, wherein: After the sixth step, a step of coating an organic film, a step of etching the organic film in a direction perpendicular to the semiconductor substrate and controlling the etching amount in such a manner that a portion of the stacked film of the protective insulating film is exposed and the upper surface of the organic film is located at a position higher than the height of the gate insulating film at the bottom of the metal layer, a step of removing the gate insulating film remaining on the side wall of the gate sidewall spacer using anisotropic etching and isotropic etching, a step of removing the organic film, and a step of removing the stacked film of the protective insulating film by isotropic etching are performed. The steps of removing the stacked film from the etching in the vertical direction of the organic film to the protective insulating film are continuously performed in the same plasma processing apparatus.

10. The method for manufacturing a semiconductor device according to claim 1, wherein: After the sixth step, a step of forming a bottom protective insulating film by forming an insulating film and isotropically etching the insulating film so that only the bottom of the cut region is protected by the insulating film is performed, a step of removing the gate insulating film remaining on the side wall of the gate sidewall spacer by anisotropic etching and isotropic etching, a step of removing the bottom protective insulating film by isotropic etching, and a step of removing the stacked film of the protective insulating film by isotropic etching are performed. The first step to the sixth step and the step from the step of forming the bottom protective insulating film to the step of removing the stacked film of the protective insulating film by isotropic etching are continuously performed in the same plasma processing apparatus.

11. A plasma treatment method, wherein the plasma treatment is performed on a structure having a channel structure on a semiconductor substrate, the channel structure having a fin-shaped, filament-shaped or sheet-shaped channel, a gate stack film formed by sequentially forming a gate insulating film and a metal layer on the channel, the gate structure formed by the gate stack film having a shape oriented in a direction perpendicular to the orientation direction of the channel, a gate sidewall spacer formed on a sidewall of the gate structure, wherein: The plasma treatment method continuously performs: In a first step, the metal layer is etched in a vertical direction to form a groove-shaped cutting area; A second step is to deposit a protective insulating film on the sidewalls of the cut region formed by the etching; A third step is to anisotropically etch the protective insulating film in a vertical direction to expose the surface of the gate insulating film present at the bottom of the metal layer; A fourth step is to remove a portion of the metal layer by isotropic etching; A fifth step, in which the fourth step is sandwiched between the cyclic steps consisting of the second step and the third step as needed, and the cyclic steps are repeated multiple times using an insulating film material different from the protective insulating film, so that a laminated film of a protective insulating film consisting of the protective insulating film and a plurality of protective insulating films different from the protective insulating film is formed on the side wall of the cutting area; as well as In the sixth step, a portion of the gate insulating film exposed at the bottom of the dicing region is removed by etching.

12. The plasma processing method according to claim 11, wherein: The first to sixth steps and a seventh step of removing the stacked film of the protective insulating film by isotropic etching are continuously performed in one plasma processing apparatus.

13. The plasma processing method according to claim 12, wherein: The first step to the seventh step and the step of removing the gate insulating film remaining on the sidewall of the gate sidewall spacer by isotropic etching are continuously performed in one plasma processing apparatus.

14. The plasma processing method according to claim 12, wherein: The first step to the seventh step are continuously performed in a plasma processing device, the step of forming an insulating film and isotropically etching the insulating film so that only the bottom of the cutting area is protected by the insulating film to form a bottom protective insulating film, the step of removing the gate insulating film remaining on the side wall of the gate sidewall spacer by isotropic etching, and the step of removing the bottom protective insulating film by isotropic etching.

15. The plasma processing method according to claim 11, wherein: The first step to the sixth step are continuously performed in a plasma processing device, including a step of forming an insulating film and isotropically etching the insulating film so that only the bottom of the cutting area is protected by the insulating film to form a bottom protective insulating film, a step of removing the gate insulating film remaining on the side wall of the gate sidewall spacer using anisotropic etching and isotropic etching, a step of removing the bottom protective insulating film by isotropic etching, and a step of removing the stacked film of the protective insulating film by isotropic etching.

16. The plasma processing method according to claim 14 or 15, wherein: In the second step and the fourth step and in the formation of the insulating film, the protective insulating film is deposited using an ALD method.