Preparation method and application of CMC-PmPD composite membrane

The preparation of CMC-PmPD composite films through chemical oxidation polymerization of m-phenylenediamine and ammonium persulfate was solved, and the problems of small adsorption capacity and environmental pollution in the prior art gold recycling materials were achieved, thus achieving efficient and rapid adsorption and recycling of precious metal ions , suitable for industrial applications.

CN118976472APending Publication Date: 2024-11-19ANQING NORMAL UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411065080.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the prior art, in the method of recovering gold from electronic waste, the adsorption capacity of the adsorption material is small, the adsorption speed is slow, and there are environmental pollution problems. Most methods need to be carried out under vacuum conditions, and the reactants are not environmentally friendly.

Method used

Using m-phenylenediamine as monomer and ammonium persulfate as initiator, polym-phenylenediamine powder is prepared by chemical oxidation polymerization, and a CMC-PmPD composite film is prepared by cross-linking of functional reagents and curing agents for adsorption of precious metal ions. .

Benefits of technology

The prepared CMC-PmPD composite film has high adsorption capacity, fast adsorption rate, strong selectivity, and can be recycled. It is suitable for industrial applications, and the synthesis process is simple, low cost and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004979110390000071
    Figure BDA0004979110390000071
  • Figure BDA0004979110390000072
    Figure BDA0004979110390000072
  • Figure BDA0004979110390000081
    Figure BDA0004979110390000081
Patent Text Reader

Abstract

The invention relates to the field of precious metal recovery, in particular to a preparation method and application of a CMC-PmPD composite membrane, and the preparation method comprises the following steps: by taking m-phenylenediamine as a monomer and ammonium persulfate as an initiator, carrying out chemical oxidative polymerization to obtain black poly (m-phenylenediamine) powder, crosslinking the poly (m-phenylenediamine) powder on a functional reagent, and curing to obtain the composite membrane. The CMC-PmPD composite membrane is of a porous structure, has more adsorption sites, and has high adsorption capacity and high adsorption rate on Au (III) in electronic waste; the adsorbent has selectivity on Au (III) in the electronic waste and has high adsorption efficiency on Au (III); the composite membrane can be recycled and has a wide industrial application prospect, and in addition, the synthetic method of the scheme is simple, low in cost, large in adsorption capacity and green and environment-friendly in the synthetic process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of precious metal recovery, and in particular to a preparation method and application of a CMC-PmPD composite film. Background Art

[0002] The amount of electronic waste in the world has increased year by year with the rapid development of the electronics industry. The environmental pollution and resource waste caused by these electronic wastes have become the focus of attention in today's society. The random discarding of electronic wastes poses a threat to the environment and human health. For example, heavy metal ions released from electronic wastes can pollute soil and water sources. On the other hand, electronic wastes contain a large amount of precious metals, which have become key materials in the global industrial field due to their excellent physical and chemical properties (such as high temperature oxidation resistance and high conductivity). According to literature reports, the gold content in electronic waste generated worldwide each year is about 300 tons, most of which comes from discarded circuit printed boards. Therefore, recovering gold from electronic wastes has important economic and social significance in promoting resource sustainability and environmental protection.

[0003] At present, the main methods for recovering gold from electronic waste are electrolysis, solvent extraction, bioleaching, ion exchange and adsorption. Among these methods, adsorption has attracted more and more attention due to its advantages of simple operation, low cost, high efficiency and recyclable adsorption materials. For example, Wang Shixing et al. synthesized a trithiocyanuric acid-Zr-based MOFs adsorbent (ZT-MOFs) by hydrothermal method. Under the optimal condition of solution pH 7, the adsorption capacity of ZT-MOFs for Au(Ⅲ) can reach 333.34 mg / g. However, it takes a long time for adsorption to reach equilibrium (8 hours), and trithiocyanuric acid is prone to secondary pollution. Jingsong xia et al. prepared a magnetic activated carbon by a one-step solvothermal method and used it to recover gold from cyanide solution. After 5 adsorption-desorption cycles, the adsorption performance of this magnetic activated carbon remained stable, but the maximum adsorption capacity for Au(III) was only 45.2 mg / g. Recently, Jian Shi's team prepared polyphenylglycine membrane using ammonium disulfate as an oxidant. The membrane can selectively recover about 80% of the gold in the leachate of waste printed circuit boards and has a wide pH application range. However, the reaction needs to be carried out under vacuum conditions, and the reactants used are not environmentally friendly. Therefore, it is necessary to develop an adsorption material with a simple synthesis method, large adsorption capacity and high selectivity. Summary of the invention

[0004] In order to solve the problems in the prior art, the present invention provides a preparation method and application of a CMC-PmPD composite membrane.

[0005] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a method for preparing a CMC-PmPD composite film, using meta-phenylenediamine as a monomer and ammonium persulfate as an initiator, and obtaining black poly-meta-phenylenediamine powder through chemical oxidation polymerization, and cross-linking the poly-meta-phenylenediamine powder on a functional reagent, and obtaining the composite film after curing.

[0006] Preferably, the concentration of the m-phenylenediamine solution is 20-80 g / L, and the concentration of the ammonium persulfate solution is 1-200 g / L.

[0007] Preferably, the reaction time of the chemical oxidative polymerization is 10-40 min.

[0008] Preferably, the functional agent includes one or more of sodium carboxymethyl cellulose, potassium carboxymethyl cellulose, magnesium carboxymethyl cellulose, calcium carboxymethyl cellulose or carboxymethyl cellulose.

[0009] Preferably, the mass concentration of the functional reagent solution is 1%.

[0010] Preferably, the curing is carried out using a curing agent, and the curing is carried out using a curing agent, and the curing agent includes one or more of polyaluminum chloride, polyaluminum ferric sulfate, ferric chloride or aluminum nitrate.

[0011] Preferably, the curing reaction temperature is 0-60° C., and the reaction time is 30-300 min.

[0012] Preferably, the curing reaction temperature is 10-50°C, and the reaction time is 240 minutes.

[0013] The second aspect of the present invention provides an application of a CMC-PmPD composite membrane prepared according to the above-mentioned method for preparing the CMC-PmPD composite membrane in adsorbing precious metal ions.

[0014] Preferably, 0.05 g of the CMC-PmPD composite membrane is added to 50 mL of a 10-100 mg / L Au(III) solution to adsorb and separate Au(III).

[0015] The amino group on poly(m-phenylenediamine) (PmPD) is reductive and can reduce metal ions with high potential. In addition, the nitrogen atom on the amino group can also serve as a coordinating atom to provide a lone pair of electrons to combine with heavy metal ions with empty orbitals (d orbitals or hybrid orbitals). Therefore, the present invention uses cheap and readily available m-phenylenediamine (mPD) as a monomer and ammonium persulfate as an initiator to prepare a PmPD polymer adsorption material through chemical oxidation polymerization, which is applied to recover Au (III) in an acidic solution, and a soft and easy-to-separate composite membrane is successfully prepared through physical cross-linking. The CMC-PmPD composite membrane has the following beneficial effects: (1) It has a porous structure, has more adsorption sites, has a large adsorption capacity for Au (III) in electronic waste and has a faster adsorption rate; (2) The CMC-PmPD composite membrane is selective for Au (III) in electronic waste and has a high adsorption efficiency for Au (III); (3) The CMC-PmPD composite membrane can be recycled and has broad industrial application prospects. In addition, the synthesis method of the scheme of the present invention is simple, low-cost, has a large adsorption capacity, and the synthesis process is green and environmentally friendly.

[0016] Other features and advantages of the embodiments of the present invention will be described in detail in the subsequent detailed description. DETAILED DESCRIPTION

[0017] The specific implementation of the embodiment of the present invention is described in detail below. It should be understood that the specific implementation described here is only used to illustrate and explain the embodiment of the present invention, and is not used to limit the embodiment of the present invention.

[0018] Embodiment 1:

[0019] Synthesis of CMC-PmPD composite membrane

[0020] (1) Weigh 1.0 g of m-phenylenediamine and dissolve it in 20 mL of distilled water to obtain a m-phenylenediamine solution. Weigh 2.5 g of ammonium persulfate and dissolve it in 25 mL of distilled water to obtain an ammonium persulfate solution. Under magnetic stirring conditions, use a rubber-tipped dropper to drip the ammonium persulfate solution drop by drop into the m-phenylenediamine solution. After dripping, continue stirring for 16 hours, filter, use ethanol and distilled water to wash to remove residual impurities and oligomers, and then place in an oven at 70°C to dry for 12 hours to finally obtain black poly-m-phenylenediamine (PmPD) powder.

[0021] (2) Weigh 0.5 g of the PmPD powder obtained in step 1 and dissolve it in 10 mL of distilled water. After magnetic stirring for 10 min, add 25 mL of 1% sodium carboxymethyl cellulose solution, continue stirring for 20 min, then add 0.5 mL of glycerol dropwise, continue stirring for 3 h after the addition, pour the mixed solution into a 10×10 cm round glass culture dish, leave it naturally at room temperature for 1 h, transfer it to an oven at 30°C for aging for 6 h, then soak the membrane material in 50 mL of 0.5 mol / L polyaluminium chloride solution for 20 min, take it out and rinse it with water, and finally dry it in an oven at 30°C to obtain the final CMC-PmPD composite membrane.

[0022] Embodiment 2:

[0023] Synthesis of CMC-PmPD composite membrane

[0024] (1) Weigh 1.0 g of m-phenylenediamine and dissolve it in 20 mL of distilled water to obtain a m-phenylenediamine solution. Weigh 2.5 g of ammonium persulfate and dissolve it in 25 mL of distilled water to obtain an ammonium persulfate solution. Under magnetic stirring conditions, use a rubber-tipped dropper to drip the ammonium persulfate solution drop by drop into the m-phenylenediamine solution. After dripping, continue stirring for 16 hours, filter, use ethanol and distilled water to wash to remove residual impurities and oligomers, and then place in an oven at 70°C to dry for 12 hours to finally obtain black poly-m-phenylenediamine (PmPD) powder.

[0025] (2) Weigh 0.5 g of the PmPD powder obtained in step 1 and dissolve it in 10 mL of distilled water. After magnetic stirring for 10 min, add 25 mL of 1% potassium carboxymethyl cellulose solution, continue stirring for 20 min, then add 0.5 mL of glycerol dropwise, continue stirring for 3 h after the addition, pour the mixed solution into a 10×10 cm round glass culture dish, leave it naturally at room temperature for 1 h, transfer it to an oven at 30°C for aging for 6 h, then soak the membrane material in 50 mL of 0.5 mol / L polyaluminium chloride solution for 20 min, take it out and rinse it with water, and finally dry it in an oven at 30°C to obtain the final CMC-PmPD composite membrane.

[0026] The difference between Example 2 and Example 1 is that sodium carboxymethyl cellulose is replaced by potassium carboxymethyl cellulose.

[0027] Embodiment 3:

[0028] Synthesis of CMC-PmPD composite membrane

[0029] (1) Weigh 1.0 g of m-phenylenediamine and dissolve it in 20 mL of distilled water to obtain a m-phenylenediamine solution. Weigh 2.5 g of ammonium persulfate and dissolve it in 25 mL of distilled water to obtain an ammonium persulfate solution. Under magnetic stirring conditions, use a rubber-tipped dropper to drip the ammonium persulfate solution drop by drop into the m-phenylenediamine solution. After dripping, continue stirring for 16 hours, filter, use ethanol and distilled water to wash to remove residual impurities and oligomers, and then place in an oven at 70°C to dry for 12 hours to finally obtain black poly-m-phenylenediamine (PmPD) powder.

[0030] (2) Weigh 0.5 g of the PmPD powder obtained in step 1 and dissolve it in 10 mL of distilled water. After magnetic stirring for 10 min, add 25 mL of 1% carboxymethyl cellulose solution, continue stirring for 20 min, then add 0.5 mL of glycerol dropwise, continue stirring for 3 h after the addition, pour the mixed solution into a 10×10 cm round glass culture dish, leave it naturally at room temperature for 1 h, transfer it to an oven at 30°C for aging for 6 h, then soak the membrane material in 50 mL of 0.5 mol / L polyaluminium chloride solution for 20 min, take it out and rinse it with water, and finally dry it in an oven at 30°C to obtain the final CMC-PmPD composite membrane.

[0031] The difference between Example 3 and Example 1 is that sodium carboxymethyl cellulose is replaced by carboxymethyl cellulose.

[0032] Embodiment 4:

[0033] Synthesis of CMC-PmPD composite membrane

[0034] (1) Weigh 1.0 g of m-phenylenediamine and dissolve it in 20 mL of distilled water to obtain a m-phenylenediamine solution. Weigh 2.5 g of ammonium persulfate and dissolve it in 25 mL of distilled water to obtain an ammonium persulfate solution. Under magnetic stirring conditions, use a rubber-tipped dropper to drip the ammonium persulfate solution drop by drop into the m-phenylenediamine solution. After dripping, continue stirring for 16 hours, filter, use ethanol and distilled water to wash to remove residual impurities and oligomers, and then place in an oven at 70°C to dry for 12 hours to finally obtain black poly-m-phenylenediamine (PmPD) powder.

[0035] (2) Weigh 0.5 g of the PmPD powder obtained in step 1 and dissolve it in 10 mL of distilled water. After magnetic stirring for 10 min, add 25 mL of 1% sodium carboxymethyl cellulose solution, continue stirring for 20 min, then add 0.5 mL of glycerol dropwise, continue stirring for 3 h after the addition, pour the mixture into a 10×10 cm round glass culture dish, leave it naturally at room temperature for 1 h, transfer it to an oven at 30°C for aging for 6 h, then soak the membrane material in 50 mL of 0.5 mol / L ferric chloride solution for 20 min, take it out and rinse it with water, and finally dry it in an oven at 30°C to obtain the final CMC-PmPD composite membrane.

[0036] The difference between Example 4 and Example 1 is that polyaluminium chloride is replaced by ferric chloride.

[0037] Embodiment 5:

[0038] Synthesis of CMC-PmPD composite membrane

[0039] (1) Weigh 1.0 g of m-phenylenediamine and dissolve it in 20 mL of distilled water to obtain a m-phenylenediamine solution. Weigh 2.5 g of ammonium persulfate and dissolve it in 25 mL of distilled water to obtain an ammonium persulfate solution. Under magnetic stirring conditions, use a rubber-tipped dropper to drip the ammonium persulfate solution drop by drop into the m-phenylenediamine solution. After dripping, continue stirring for 16 hours, filter, use ethanol and distilled water to wash to remove residual impurities and oligomers, and then place in an oven at 70°C to dry for 12 hours to finally obtain black poly-m-phenylenediamine (PmPD) powder.

[0040] (2) Weigh 0.5 g of the PmPD powder obtained in step 1 and dissolve it in 10 mL of distilled water. After magnetic stirring for 10 min, add 25 mL of 1% sodium carboxymethyl cellulose solution, continue stirring for 20 min, then add 0.5 mL of glycerol dropwise, continue stirring for 3 h after the addition, pour the mixed solution into a 10×10 cm round glass culture dish, leave it naturally at room temperature for 1 h, transfer it to an oven at 30°C for aging for 6 h, then soak the membrane material in 50 mL of 0.5 mol / L aluminum nitrate solution for 20 min, take it out and rinse it with water, and finally dry it in an oven at 30°C to obtain the final CMC-PmPD composite membrane.

[0041] The difference between Example 5 and Example 1 is that polyaluminium chloride is replaced by aluminium nitrate.

[0042] Embodiment 6:

[0043] The process of this embodiment is the same as that of Embodiment 1, except that the concentration of the m-phenylenediamine solution is 20 g / L, the concentration of the ammonium persulfate solution is 1 g / L, the reaction time of the chemical oxidation polymerization is 10 min, the curing reaction temperature is 60° C., and the reaction time is 30 min.

[0044] Embodiment 7:

[0045] The process of this embodiment is the same as that of Embodiment 1, except that the concentration of the m-phenylenediamine solution is 80 g / L, the concentration of the ammonium persulfate solution is 200 g / L, the reaction time of the chemical oxidative polymerization is 40 min, the curing reaction temperature is 0° C., and the reaction time is 300 min.

[0046] Test Example 1:

[0047] The adsorption rate and maximum adsorption capacity of the CMC-PmPD composite membrane prepared in Example 1 are shown in Table 1 below:

[0048] The specific steps of the adsorption test are as follows:

[0049] (1) Weigh 0.05 g of the CMC-PmPD composite membrane prepared in Example 1 and add it to 100, 200, 400, 600, 800 or 1000 mg / L Au(III) solution respectively;

[0050] (2) Magnetic stirring was performed for 4 h at room temperature, and the remaining Au(III) concentration in the solution was determined by ICP-OES;

[0051] (3) The adsorption rate and adsorption capacity of CMC-PmPD composite film for Au(III) were calculated using the following formula.

[0052]

[0053] C i is the initial concentration of Au(III) in the solution, C f is the remaining Au(III) concentration in the solution after adsorption, and m is the mass of the CMC-PmPD composite film.

[0054] Table 1 Maximum adsorption capacity and adsorption rate of CMC-PmPD composite membrane for Au(III) in Example 1

[0055]

[0056] It can be seen that the maximum adsorption capacity of the CMC-PmPD composite film prepared by the present invention for Au(III) is 421.1 mg / g, and the adsorption rate is as high as 99.8%.

[0057] Test Example 2:

[0058] The adsorption performance of the CMC-PmPD composite membranes prepared in Examples 1-5 was tested, and the results obtained are shown in Table 2 below:

[0059] Table 2 Experimental data of adsorption rate of CMC-PmPD composite membranes prepared in Examples 1-5

[0060]

[0061] It can be seen that the CMC-PmPD composite membrane prepared with sodium carboxymethyl cellulose as the functional reagent and polyaluminium chloride as the curing agent has the best adsorption effect.

[0062] Test Example 3:

[0063] Select mixed ions (Cu 2+ 、Ni2+ 、Cd 2+ 、Zn 2+ ) solution, the composite membrane prepared in Example 1 was added, and the experimental results are shown in Table 3 below:

[0064] The experimental steps are as follows:

[0065] (1) Preparation of Au(III) and Cu in different water samples 2+ 、Ni 2+ 、Cd 2+ 、Zn 2+ To the solutions with concentration ratios of 1:1, 1:4, 1:50, and 1:100, 0.05 g of the CMC-PmPD composite membrane in Example 1 was added respectively;

[0066] (2) Applying the CMC-PmPD composite membrane to treat Au(III) in CPU leachate (the leachate was obtained by soaking a piece of discarded computer CPU in 24 mL of aqua regia for 48 h);

[0067] (3) The solution was stirred magnetically for 4 h at room temperature and the concentration of Au(III) remaining in the solution (1) (2) was determined by ICP-OES to calculate the adsorption rate of Au(III) by the CMC-PmPD composite film.

[0068] Table 3 Adsorption rate of gold by CMC-PmPD composite membrane of Example 1 in different water samples and its application in actual CPU

[0069]

[0070] As shown in Table 3, when the CMC-PmPD composite membrane is used to treat mixed heavy metal ion solutions of different concentrations and compositions, the CMC-PmPD composite membrane can always selectively adsorb more than 90% of Au(Ⅲ) from the solution, showing high selectivity and applicability.

[0071] Test Example 4:

[0072] The CMC-PmPD composite membrane prepared by the present invention is recycled to obtain the following results.

[0073] The operation steps of the cycle experiment are as follows:

[0074] (1) The CMC-PmPD composite membrane adsorbed with Au(III) was immersed in 50 mL of 5% thiourea solution;

[0075] (2) Soak for 4 h at room temperature, rinse with distilled water, and air dry naturally to obtain the regenerated CMC-PmPD composite membrane.

[0076] During 5 adsorption / desorption cycles, the adsorption rate of Au(III) on the CMC-PmPD composite membrane remained at 89±3%, indicating that the CMC-PmPD composite membrane has good cyclic performance and stability.

[0077] In summary, the amino group on poly-m-phenylenediamine (PmPD) has reducing properties and can reduce high-potential metal ions. In addition, the nitrogen atom on the amino group can also serve as a coordinating atom to provide a lone pair of electrons to combine with heavy metal ions with empty orbitals (d orbitals or hybrid orbitals). Therefore, the present invention uses cheap and readily available m-phenylenediamine (mPD) as a monomer and ammonium persulfate as an initiator to prepare a PmPD polymer adsorption material through chemical oxidation polymerization, which is applied to recover Au (III) in an acidic solution, and a soft and easily separable composite membrane is successfully prepared through physical cross-linking. The CMC-PmPD composite membrane has the following beneficial effects: (1) it has a porous structure, has more adsorption sites, has a large adsorption capacity for Au(III) in electronic waste and a faster adsorption rate, and the maximum adsorption capacity for Au(III) is 421.1 mg / g; (2) the CMC-PmPD composite membrane is selective for Au(III) in electronic waste, and has a high adsorption efficiency for Au(III), which can reach up to 99.9%; (3) the CMC-PmPD composite membrane can be recycled and has broad industrial application prospects. In addition, the synthesis method of the scheme of the present invention is simple, low-cost, has a large adsorption capacity, and the synthesis process is green and environmentally friendly.

[0078] The above are only embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application should be included within the scope of the claims of the present application.

Claims

1. A method for preparing a CMC-PmPD composite membrane, characterized in that: Using metaphenylenediamine as a monomer and ammonium persulfate as an initiator, black poly-metaphenylenediamine powder is obtained through chemical oxidation polymerization, and the poly-metaphenylenediamine powder is cross-linked on a functional reagent, and the composite film is obtained after curing.

2. The preparation method according to claim 1, characterized in that: The concentration of the m-phenylenediamine solution is 20-80 g / L, and the concentration of the ammonium persulfate solution is 1-200 g / L.

3. The preparation method according to claim 1, characterized in that: The reaction time of the chemical oxidative polymerization is 10-40 minutes.

4. The preparation method according to claim 1, characterized in that: The functional agent includes one or more of sodium carboxymethyl cellulose, potassium carboxymethyl cellulose, magnesium carboxymethyl cellulose, calcium carboxymethyl cellulose or carboxymethyl cellulose.

5. The preparation method according to claim 4, characterized in that: The mass concentration of the functional reagent solution is 1%.

6. The preparation method according to claim 1, characterized in that: The curing is carried out using a curing agent, and the curing agent includes one or more of polyaluminium chloride, polyaluminium ferric sulfate, ferric chloride or aluminium nitrate.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The curing reaction temperature is 0-60° C., and the reaction time is 30-300 min.

8. The preparation method according to claim 7, characterized in that: The curing reaction temperature is 10-50°C, and the reaction time is 240 minutes.

9. Use of a CMC-PmPD composite membrane prepared according to the method for preparing a CMC-PmPD composite membrane according to any one of claims 1 to 8 in adsorbing noble metal ions.

10. The use according to claim 9, characterized in that: 0.05 g of the CMC-PmPD composite membrane was added into 50 mL of 10-100 mg / L Au(III) solution to separate Au(III) by adsorption.

Citation Information

Patent Citations

  • Method of reclaiming silver from silver containing solution by poly m-phenylenediamine as adsorbent

    CN101016587A

  • Method for embedding adsorbent of poly m-phenylene diamine by using polyvinyl alcohol

    CN101091909A

  • Method for preparing poly-m-phenylenediamine through oxidation of composite oxidation system

    CN102634014A

  • Method for preparing membrane capable of adsorbing and treating cadmium ions in wastewater by using fucoidan and sodium carboxymethyl cellulose as well as product and application of membrane

    CN111482094A

  • Polyaniline nano-material, composite film and preparation method and application of polyaniline nano-material and composite film

    CN116693847A