Furfural water-phase rearrangement hydrogenation catalyst, preparation method thereof and method for preparing cyclopentanol by catalyzing furfural water-phase rearrangement hydrogenation

The preparation of cyclopentanone and cyclopentanol in the prior art is solved by using supported catalysts (such as Cu/SiO2, Ni/SiO2, Co/SiO2 or Cu-Zn/SiO2) in biomass. The catalyst surface is easy to decompose and selectively control the problem, which improves the yield of cyclopentol and the stability of the catalyst.

CN118976493AActive Publication Date: 2024-11-19GUANGDONG UNIV OF TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411070764.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The prior art faces the problems of easy decomposition of the catalyst surface and difficult product selectivity when effectively preparing cyclopentanone and cyclopentanol from biomass, which limits the high-quality utilization of furfural in industrial applications.

Method used

Silica-supported metal catalysts, specifically Cu/SiO2, Ni/SiO2, Co/SiO2 or Cu-Zn/SiO2, promote the aqueous phase retention of furfural Reaction to prepare cyclopentol. The preparation method of the catalyst includes metal salt dissolution, ammonia water complexation, deposition, ammonia distillation, calcination and reduction steps to form a supported catalyst to improve activity and dispersion.

Benefits of technology

The high activity and conversion rate of catalytic reaction are achieved. The zinc metal catalyst has strong hydrogenation ability in five-membered ring synthesis, which enhances the interaction between copper and support, promotes the formation of cyclopentanone and hydrogenates into cyclopentanol, and The catalyst is easy to reuse and has a stable yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976493A_ABST
    Figure CN118976493A_ABST
Patent Text Reader

Abstract

The invention discloses a furfural water-phase rearrangement hydrogenation catalyst, a preparation method thereof and a method for preparing cyclopentanol by catalyzing furfural water-phase rearrangement hydrogenation. The catalyst is silicon dioxide loaded metal; the metal is at least one of copper, nickel, cobalt and zinc; the metal accounts for 0.25-11% of the total weight of the catalyst; adding the catalyst, furfural and water into an intermittent closed high-pressure reaction kettle, and performing catalytic selective hydrogenation under stirring to prepare cyclopentanol; the zinc-doped copper silicate catalyst is prepared, the original copper silicate phase is not damaged after the catalyst is modified, and the acidity of the catalyst, especially the Lewis acid site, is obviously improved; and the modified copper silicate catalyst has the advantages of uniform particles, improved specific surface area and acidity, low price, renewability and wide industrial application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of catalysts, in particular to a furfural aqueous phase rearrangement hydrogenation catalyst. The invention also relates to a method for preparing the catalyst and a method for preparing cyclopentanol by furfural aqueous phase rearrangement selective hydrogenation using the catalyst. Background Art

[0002] As the consumption of non-renewable fossil fuels continues to increase, the effective utilization of renewable biomass resources has become increasingly attractive. Biomass can be converted into fuels and chemicals. The industrial application of biomass is based on improving the competitiveness of biomass resources, developing methods for the preparation of inexpensive platform molecules, and effectively converting platform molecules into fuels and chemicals. Furfural is an important platform molecule that can be obtained from hemicellulose in lignocellulosic biomass and can be further converted into a series of liquid fuels, fuel additives and other chemicals, such as furfuryl alcohol (FOL), tetrahydrofurfuryl alcohol (THFOL), 2-methyltetrahydrofuran (MTHF), 2-methylfuran, isoprene, pentanediol, levulinic acid, etc. At present, furfural is mainly used to produce furfuryl alcohol, but its development in the development of high-quality utilization of other downstream industrial products is limited. Therefore, further research on expanding the high-quality utilization of furfural is of great practical significance. Cyclopentanone (CPO) and cyclopentanol (CPL) are fine chemical raw materials that have been widely used as synthetic raw materials and solvents. For example, cyclopentanone and cyclopentanol have been used to prepare perfumes and pharmaceutical materials. In addition, cyclopentanone is widely used as a solvent in the electronics industry because it can easily dissolve various resins. Cyclopentyl methyl ether and cyclopentyl ethyl ether have the characteristics of high hydrophobicity, low latent heat of solvent evaporation, difficulty in peroxide formation, and easy drying, and have been used as solvents for important chemical reactions such as Grignard reaction and coupling reaction. The demand for cyclopentanone and cyclopentanol exceeds 1 million tons per year. Therefore, it would be very valuable if both cyclopentanone and cyclopentanol could be effectively prepared from biomass-based furfural. Although the research on furan compounds has a history of several decades, the process is very challenging due to two situations: furan is easily decomposed into small oxygen-containing compounds and oligomers accumulate on the catalyst surface; product selectivity is difficult to control. Summary of the invention

[0003] The first object of the present invention is to provide a furfural aqueous phase rearrangement hydrogenation catalyst, which realizes the close combination of hydrogenation sites and acid sites, so that active intermediates can complete a series of tandem reactions such as hydrogenation rearrangement ring opening on the catalyst surface.

[0004] The second object of the present invention is to provide a method for preparing the above-mentioned furfural aqueous phase rearrangement hydrogenation catalyst.

[0005] The third object of the present invention is to provide a method for preparing cyclopentanol by catalyzing the aqueous phase rearrangement and hydrogenation of furfural by the above catalyst.

[0006] To this end, the first technical solution provided by the present invention is as follows:

[0007] A furfural water-phase rearrangement hydrogenation catalyst is a silicon dioxide-supported metal; the metal is at least one of copper, nickel, cobalt and zinc; the metal accounts for 0.25-11% of the total weight of the catalyst.

[0008] Furthermore, the furfural aqueous phase rearrangement hydrogenation catalyst is Cu / SiO 2 , or Ni / SiO 2 , or Co / SiO 2 , or Cu.Zn / SiO 2 .

[0009] Furthermore, the above-mentioned furfural aqueous rearrangement hydrogenation catalyst is calculated based on 100% of the total mass of the furfural aqueous rearrangement hydrogenation catalyst, and the Cu / SiO 2 、Ni / SiO 2 、Co / SiO 2 Cu, Ni and Co in the catalyst each account for 10% of the corresponding catalyst mass.

[0010] Furthermore, the above-mentioned furfural aqueous rearrangement hydrogenation catalyst is calculated based on 100% of the total mass of the furfural aqueous rearrangement hydrogenation catalyst, and the Cu.Zn / SiO 2 In the catalyst, Cu accounts for 10% of the total mass of the catalyst, and Zn accounts for 0.25-1% of the total mass of the catalyst.

[0011] The second technical solution provided by the present invention is a method for preparing the above-mentioned furfural aqueous phase rearrangement hydrogenation catalyst, which comprises the following steps in sequence: dissolving the metal salt in water, adding ammonia water for complexation and then depositing it on silica sol, distilling ammonia at 70-100°C for 4 hours, filtering and washing, drying at 60-120°C for 12 hours, calcining in air first, and then reducing it in a reducing atmosphere.

[0012] Furthermore, in the above-mentioned method for preparing the furfural aqueous phase rearrangement hydrogenation catalyst, the pH of the ammonia evaporation system environment is 5-9.

[0013] Furthermore, in the preparation method of the above-mentioned furfural aqueous phase rearrangement hydrogenation catalyst, the calcination temperature is 450-550°C, the heating rate is 5°C / min, and the time is 4-6 hours.

[0014] Furthermore, in the preparation method of the above-mentioned furfural aqueous phase rearrangement hydrogenation catalyst, the reduction temperature is 260-500°C, the heating rate is 5°C / min, and the time is 2-4 hours.

[0015] Furthermore, in the above-mentioned method for preparing the furfural aqueous phase rearrangement hydrogenation catalyst, the reducing atmosphere comprises a hydrogen atmosphere or a hydrogen-argon mixture; and the flow rate of the reducing atmosphere is 40-50 mL / min.

[0016] The last technical scheme provided by the present invention is a method for preparing cyclopentanol by rearrangement and hydrogenation of furfural in water phase. Furfural, water and the catalyst provided by the first technical scheme are added into an intermittent closed high-pressure reactor, and a catalytic selective hydrogenation reaction is carried out under stirring. The amount of furfural is 3-5 mmol, the amount of catalyst is 20-300 mg, the initial pressure of hydrogen is 1-6 MPa, the reaction temperature is 120-200° C., and the reaction time is 30 min-720 min.

[0017] Furthermore, in the above-mentioned method for preparing cyclopentanol by furfural aqueous phase rearrangement hydrogenation, furfural, water and catalyst are added into an intermittent closed high-pressure reactor under the condition of the catalyst described in claim 8, and catalytic selective hydrogenation is carried out under stirring, wherein the amount of furfural is 5 mmol, the amount of catalyst is 300 mg, the initial pressure of hydrogen is 4 MPa, the reaction temperature is 140°C, and the reaction time is 6 hours.

[0018] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0019] 1. The supported catalyst provided by the present invention has a smaller particle size and good dispersion, provides more adsorption sites and active sites for the catalytic reaction, increases the contact area between the reactants and the active metal, and has higher catalytic activity and conversion;

[0020] 2. The zinc metal catalyst provided in the present application has strong hydrogenation ability and good ring-closing ability in the synthesis of the five-membered ring. At the same time, the doping of zinc enhances the interaction between copper and the carrier, realizes the close combination of the hydrogenation site and the acid site, and does not destroy the original layered copper silicate structure. At the same time, it makes it easier for the catalyst to promote the rearrangement of furfuryl alcohol to generate the important intermediate cyclopentanone and then hydrogenate it into cyclopentanol.

[0021] 3. The technical solution provided by the present invention uses furfural as raw material and non-precious metal copper and zinc as catalysts, so that the active intermediates complete a series of tandem reactions such as hydrogenation, rearrangement and ring opening on the catalyst surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The X-ray diffraction analysis diagram of the catalyst comparing copper phyllosilicate with different zinc doping amounts in Examples 1, 4-6;

[0023] Figure 2 The infrared spectra of the catalysts of copper phyllosilicate with different zinc doping amounts in Examples 1 and 4-6 are compared.

[0024] Figure 3 The results of ammonia adsorption and desorption after reduction of different zinc-doped copper silicate catalysts are compared in Examples 1 and 4-6.

[0025] Figure 4 The infrared images of pyridine after reduction by different zinc-doped copper silicate catalysts are compared in Examples 1 and 4-6.

[0026] Figure 5 Cyclic stability test results for Example 11 DETAILED DESCRIPTION

[0027] The claims of the present invention are further described in detail below in conjunction with specific implementations, but do not constitute any limitation to the present invention.

[0028] Example 1

[0029] Weigh 0.5 g furfural and 12 mL water and put them into the reactor, then add 0.3 g catalyst Cu / SiO 2 (Among them, SiO 2 The catalyst is prepared by replacing the air in the reactor with hydrogen for 3-4 times, introducing hydrogen until the initial pressure is 4MPa, and turning on the stirring device at about 400r / min. The reaction is carried out at 140°C for 8 hours, and the reaction is cooled after the reaction is completed. The product is obtained by filtering and centrifugal separation. Quantitative and qualitative analysis is carried out by gas chromatography-mass spectrometry, and the results show that the furfural conversion rate is 100%, the cyclopentanone yield is 15.9%, and the cyclopentanol yield is 35%.

[0030] Cu / SiO 2 The catalyst was prepared by the following method:

[0031] Weigh 4.53 g of Cu(NO 3 ) 2 ·3H 2 O is dissolved in 150mL of deionized water, followed by adding 40mL of 28wt% ammonia solution and stirring for 30min. Then add 40.0g of silica sol, stir and mix to obtain a suspension, and then transfer the suspension to a preheated oil bath and heat to 70°C, stir for 4 hours to allow the ammonia to evaporate slowly until the pH of the solution drops to 6-7. The product is washed three times with deionized water and placed in an oven, and then dried at 100°C for 12 hours. First place it in a muffle furnace, heat it to 550°C at a heating rate of 5°C / min, and calcine for 5 hours. Then place it in a hydrogen atmosphere, heat it to 260°C at a heating rate of 5°C / min, and reduce it for 2 hours.

[0032] Example 2

[0033] The preparation process and reaction conditions are similar to those in Example 1, except that Ni / SiO 2 (where SiO 2 The catalyst was prepared by using a catalyst having a catalyst as carrier and Ni as active ingredient, wherein the weight of the active ingredient Ni was 10% of the total mass of the catalyst). The results showed that the furfural conversion rate was 100%, the yield of tetrahydrofurfuryl alcohol was 95%, and the yields of cyclopentanone and cyclopentanol were both 0%.

[0034] Ni / SiO 2 The catalyst was prepared by the following method:

[0035] Weigh 5.94 g of Ni(NO 3 ) 2 ·3H 2 O was dissolved in 150 mL of deionized water, followed by addition of 40 mL of 28 wt% ammonia solution and stirring for 30 min. Then 40.0 g of silica sol was added, stirred and mixed to obtain a suspension, and then the suspension was transferred to a preheated oil bath and heated to 70 ° C, stirred for 4 hours to allow the ammonia to evaporate slowly until the pH of the solution dropped to 6-7. The product was washed three times with deionized water and placed in an oven, and then dried at 100 ° C for 12 hours. First placed in a muffle furnace, heated to 550 ° C at a heating rate of 5 ° C / min, and calcined for 5 hours. Then placed in a hydrogen atmosphere, heated to 500 ° C at a heating rate of 5 ° C / min, and reduced for 2 hours.

[0036] Example 3

[0037] The preparation process and reaction conditions are similar to those in Example 1, except that the catalyst used is Co / SiO 2 (Among them, SiO 2 The catalyst was prepared by using a catalyst having a catalyst as carrier and Co as active ingredient. The weight of the active ingredient Co was 10% of the total mass of the catalyst. The results showed that the furfural conversion rate was 100%, the yield of tetrahydrofurfuryl alcohol was 89%, and the yields of cyclopentanone and pentanol were both 5%.

[0038] Co / SiO 2 The catalyst was prepared by the following method:

[0039] Weigh 5.93 g of Co(NO 3 ) 2 ·3H 2O was dissolved in 150 mL of deionized water, followed by addition of 40 mL of 28 wt% ammonia solution and stirring for 30 min. Then 40.0 g of silica sol was added, stirred and mixed to obtain a suspension, and the suspension was transferred to a preheated oil bath and heated to 70 ° C. Stir for 4 hours to allow the ammonia to evaporate slowly until the pH of the solution dropped to 6-7. The product was washed three times with deionized water and placed in an oven and dried at 60 ° C for 12 hours. First placed in a muffle furnace, heated to 550 ° C at a heating rate of 5 ° C / min, and calcined for 5 hours. Then placed in a hydrogen atmosphere, heated to 450 ° C at a heating rate of 5 ° C / min, and reduced for 2 hours.

[0040] Example 4

[0041] Weigh 0.5g furfural and 12mL water and put them into the reactor, then add 0.3g catalyst Cu.Zn / SiO 2 (where SiO 2 The catalyst is a carrier, and the active ingredients are Cu and Zn. The weight of the active ingredient Cu is 10% of the total mass of the catalyst, and Zn is 0.25% of the total mass of the catalyst). The air in the kettle is replaced with hydrogen 3-4 times, and hydrogen is introduced to an initial pressure of 4MPa. The stirring device is turned on at about 400r / min, and the reaction is carried out at 140°C for 8 hours and then cooled. The product is obtained by filtration and centrifugation, and quantitative and qualitative analysis is performed using gas chromatography-mass spectrometry. The results show that the furfural conversion rate is 100%, the yield of cyclopentanone is 27.1%, and the yield of cyclopentanol is 71.9%.

[0042] Cu.Zn / SiO 2 The catalyst was prepared by the following method:

[0043] Weigh 4.53 g of Cu(NO 3 ) 2 ·3H 2 O and weigh 0.13g Zn(NO 3 ) 2 6H 2 O was dissolved in 150 mL of deionized water, followed by addition of 40 mL of 28 wt% ammonia solution and stirring for 30 min. Then 40.0 g of silica sol was added, stirred and mixed to obtain a suspension, and the suspension was transferred to a preheated oil bath and heated to 70 ° C. Stir for 4 hours to allow the ammonia to evaporate slowly until the pH of the solution dropped to 6-7. The product was washed three times with deionized water and placed in an oven and dried at 100 ° C for 12 hours. First placed in a muffle furnace, heated to 550 ° C at a heating rate of 5 ° C / min, and calcined for 5 hours. Then placed in a hydrogen atmosphere, heated to 260 ° C at a heating rate of 5 ° C / min, and reduced for 2 hours.

[0044] Example 5

[0045] The preparation process and reaction conditions are similar to those in Example 5, except that the catalyst used is Cu.Zn / SiO 2 (Among them, SiO 2 The catalyst was prepared by using a catalyst as a carrier, and the active ingredients were Cu and Zn, wherein the weight of the active ingredient Cu was 10% of the total mass of the catalyst, and the weight of Zn was 0.5% of the total mass of the catalyst). The results showed that the furfural conversion rate was 100%, the yield of cyclopentanone was 3.1%, and the yield of cyclopentanol was 94.0%.

[0046] Cu.Zn / SiO 2 The catalyst was prepared by the following method:

[0047] Weigh 4.53 g of Cu(NO 3 ) 2 ·3H 2 O and weigh 0.27g Zn(NO 3 ) 2 6H 2 O was dissolved in 150 mL of deionized water, and 40 mL of 28 wt% ammonia solution was added and stirred for 30 min. Then 40.0 g of silica sol was added, and the mixture was stirred to obtain a suspension, and the suspension was transferred to a preheated oil bath and heated to 100 ° C. It was stirred for 4 hours to allow the ammonia to evaporate slowly until the pH of the solution dropped to 6-7. The product was washed three times with deionized water and placed in an oven, and then dried at 100 ° C for 12 hours. First, it was placed in a muffle furnace, heated to 550 ° C at a heating rate of 5 ° C / min, and calcined for 5 hours. Then it was placed in a hydrogen atmosphere, heated to 260 ° C at a heating rate of 5 ° C / min, and calcined for 2 hours.

[0048] Example 6

[0049] The preparation process and reaction conditions are similar to those in Example 5, except that the catalyst used is Cu.Zn / SiO 2 (Among them, SiO 2 The catalyst was used as the carrier, and the active ingredients were Cu and Zn. The weight of the active ingredient Cu was 10% of the total mass of the catalyst, and the weight of Zn was 1% of the total mass of the catalyst. The results showed that the furfural conversion rate was 100%, the yield of cyclopentanone was 17.0%, and the yield of cyclopentanol was 80.9%.

[0050] Cu.Zn / SiO 2 The catalyst was prepared by the following method:

[0051] Weigh 4.53 g of Cu(NO 3 ) 2 ·3H 2 O and weigh 0.54 g Zn(NO 3 ) 2 6H 2O was dissolved in 150 mL of deionized water, followed by addition of 40 mL of 28 wt% ammonia solution and stirring for 30 min. Then 40.0 g of silica sol was added, stirred and mixed to obtain a suspension, and then the suspension was transferred to a preheated oil bath and heated to 70 ° C, stirred for 4 hours to allow the ammonia to evaporate slowly until the pH of the solution dropped to 6-7. The product was washed three times with deionized water and placed in an oven, and then dried at 100 ° C for 12 hours. First placed in a muffle furnace, heated to 550 ° C at a heating rate of 5 ° C / min, and calcined for 5 hours. Then placed in a hydrogen atmosphere, heated to 260 ° C at a heating rate of 5 ° C / min, and calcined for 2 hours.

[0052] Example 7

[0053] The preparation process and reaction conditions were similar to those in Example 5, except that the initial reaction pressure was 3 MPa. The results showed that the furfural conversion rate was 100%, the yield of cyclopentanone was 7.9%, and the yield of cyclopentanol was 89.3%.

[0054] Example 8

[0055] The preparation process and reaction conditions were similar to those in Example 5, except that the initial reaction pressure was 5 MPa. The results showed that the furfural conversion rate was 100%, the yield of cyclopentanone was 11.3%, and the yield of cyclopentanol was 85.2%.

[0056] Example 9

[0057] The preparation process and reaction conditions were similar to those in Example 5, except that the reaction temperature was 200° C. The results were as follows: the furfural conversion rate was 100%, the yield of cyclopentanone was 23.7%, and the yield of cyclopentanol was 75.1%.

[0058] Example 10

[0059] The preparation process and reaction conditions were similar to those of Example 5, except that the reaction temperature was 120° C. The results were as follows: furfural conversion was 80%, furfuryl alcohol yield was 40%, cyclopentanone yield was 25.1%, and cyclopentanol yield was 14.9%.

[0060] Embodiment 11

[0061] The catalyst and reaction conditions used in Example 5 were used to perform a cyclic stability reaction test. After the reaction, the catalyst was separated by simple centrifugation. The recovered catalyst was directly used in the next reaction without any other treatment. After the catalyst was reused 7 times, the yield of cyclopentanol remained essentially unchanged, with a fluctuation of about 95%.

[0062] By X-ray diffraction spectrum Figure 1 and infrared spectroscopy Figure 2 The formation of layered copper silicate was confirmed. Figure 2 Medium, 670cm-1 The peak position at is attributed to δ OH The presence of bands at 1040 cm -1 The shoulder peak ν SiO , thus 10Cu / SiO 2 There is layered copper silicate in the precursor, and it can be seen that the Zn doping does not destroy the layered copper silicate structure of the catalyst, and the structure is preserved. At the same time, when the Zn doping amount increases, the 670cm -1 The intensity of the peak at 1040cm -1 The peaks at the bottom are more obvious. When the Zn content is 0.5%, the peak intensity is the highest, indicating that the highest content of phyllosilicate phase is generated. The presence of characteristic peaks at 2θ of 30.8°, 57.5°, and 62.4° in the XRD spectrum also proves that the structure of the catalyst phyllosilicate is not destroyed.

[0063] The surface acidity of different catalysts after reduction was detected by ammonia adsorption and desorption. Figure 3 All catalysts show two broad peaks in the range of 150-550℃, belonging to weak acid and medium-strong acid sites respectively. It can be seen that the distribution range of ammonia adsorption and desorption area is obviously different, and the corresponding total acid points are different. 2 The total acid content of the acid sites of the catalyst increases with the doping of Zn.

[0064] By pyridine infrared Figure 4 The results showed that with the addition of zinc, the B acid (1540 cm -1 ) sites gradually increase. -1 The sites are attributed to L-acid sites. With the doping of zinc, the differentiation of L-acid sites becomes more obvious, which indicates that the type of L-acid is changing. In previous studies, the hydrogenolysis of furfural to cyclopentanol requires the synergistic effect of metal and acid to promote the rearrangement of furfural to cyclopentanone, which may be the reason for the formation of cyclopentanone in 10Cu0.5Zn / SiO 2 The reason why the catalyst exhibits excellent performance in hydrogenolysis of furfural to produce cyclopentanol.

[0065] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A furfural aqueous phase rearrangement hydrogenation catalyst, It is characterized in that The furfural aqueous phase rearrangement hydrogenation catalyst is a silicon dioxide-supported metal; the metal is at least one of copper, nickel, cobalt and zinc; and the metal accounts for 0.25-11% of the total weight of the catalyst.

2. The furfural aqueous phase rearrangement hydrogenation catalyst according to claim 1, It is characterized in that The aldehyde water phase rearrangement hydrogenation catalyst is Cu / SiO 2 , or Ni / SiO 2 , or Co / SiO 2 , or Cu.Zn / SiO 2 .

3. The furfural aqueous phase rearrangement hydrogenation catalyst according to claim 2, It is characterized in that Calculated based on the total mass of furfural aqueous rearrangement hydrogenation catalyst as 100%, the Cu / SiO 2 、Ni / SiO 2 、Co / SiO 2 Cu, Ni and Co in the catalyst each account for 10% of the corresponding catalyst mass.

4. The furfural aqueous phase rearrangement hydrogenation catalyst according to claim 2, It is characterized in that Calculated based on the total mass of furfural aqueous phase rearrangement hydrogenation catalyst as 100%, the Cu.Zn / SiO 2 In the catalyst, Cu accounts for 10% of the total mass of the catalyst, and Zn accounts for 0.25-1% of the total mass of the catalyst.

5. The preparation method of the furfural aqueous phase rearrangement hydrogenation catalyst according to claim 1, It is characterized in that The method comprises the following steps in sequence: dissolving the metal salt in water, adding ammonia water for complexation and then depositing on silica sol, steaming ammonia at 70-100°C for 2-4 hours, filtering and washing, drying at 60-120°C for 12 hours, calcining in air first, and then reducing in a reducing atmosphere.

6. The preparation method of the furfural aqueous phase rearrangement hydrogenation catalyst according to claim 5, It is characterized in that The pH value of the ammonia evaporation system environment is 5-9.

7. The preparation method of the furfural aqueous phase rearrangement hydrogenation catalyst according to claim 5, It is characterized in that The calcination temperature is 260-500° C., the heating rate is 5° C. / min, and the calcination time is 2-4 hours.

8. The preparation method of the furfural aqueous phase rearrangement hydrogenation catalyst according to claim 5, It is characterized in that The calcination temperature is 450-550°C.

9. The method for preparing the furfural aqueous phase rearrangement hydrogenation catalyst according to claim 5, It is characterized in that The reducing atmosphere comprises a hydrogen atmosphere or a hydrogen-inert gas mixture; the flow rate of the reducing atmosphere is 40-50 mL / min.

10. A method for preparing cyclopentanol by aqueous phase rearrangement and hydrogenation of furfural, It is characterized in that Furfural, water and the catalyst described in claim 1 are added into an intermittent closed high-pressure reactor, and catalytic selective hydrogenation is carried out under stirring. The amount of furfural is 3-5 mmol, the amount of catalyst is 20-300 mg, the initial pressure of hydrogen is 1-6 MPa, the reaction temperature is 120-200° C., and the reaction time is 30 min-720 min.

Citation Information

Patent Citations

  • Method for preparing cyclopentanone and / or cyclopentanol by furfural or furfuryl alcohol

    CN102807483A

  • Catalyst for catalyzing furfural or furfuryl alcohol to prepare cyclopentanol through hydrogenation rearrangement and preparation method and application method thereof

    CN104998659A

  • Method for preparing cyclopentanone and cyclopentanol from furfural by hydrogenation

    CN110041168A