Fluorine-chlorine exchange reaction catalyst, preparation method thereof and application of fluorine-chlorine exchange reaction catalyst in preparation of 2, 3, 3, 3-tetrafluoropropene
By setting up a core layer, hollow layer and shell structure in the fluorochloro exchange reaction catalyst, and using the hollow layer to connect the pores and carbon fiber network, the problem of the catalyst's carbon deposit activity is solved, and efficient fluorochloro exchange reaction and accumulation prevention is achieved Carbon effect, allowing two-step reactions to be combined.
Patent Information
- Application Number
- CN202410892840.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-19
AI Technical Summary
The existing fluorine-chloro-exchange reaction catalysts are prone to decrease in catalytic activity due to carbon deposits after long-term use, and the effect of preventing carbon deposits is poor, so they cannot effectively maintain catalytic activity.
Design a fluorine-chloro exchange reaction catalyst, including a core layer, a hollow layer and a shell layer from the inside to the outside, with a connected hollow layer and an outer pore distributed in the shell layer. The hollow layer contains a carbon fiber network, and the hollow layer and a shell are arranged. The structure of the layer increases the reaction rate and slows down the formation of carbon deposits.
It can maintain high catalytic activity and prevent carbon deposits after long-term use, so that the catalyst's reaction rate in the HCFC exchange reaction is accelerated and the carbon deposit formation is reduced. HCC-240db→HCFO-1233xf and HCFO-1233xf→ The reaction of HFO-1234yf was carried out in the same reaction vessel.
Smart Images

Figure BDA0004928112040000121 
Figure BDA0004928112040000122
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of synthesis of 2,3,3,3-tetrafluoropropene, and in particular to a fluorine-chlorine exchange reaction catalyst, a preparation method thereof and application of the catalyst in the preparation of 2,3,3,3-tetrafluoropropene. Background Art
[0002] 2,3,3,3-tetrafluoropropene (HFO-1234yf) is a fourth-generation green and environmentally friendly refrigerant with an ozone depletion potential (ODP) of 0 and a global warming potential (GWP) of 4, which is much lower than the previously large-scale use of 1,1,1,2-tetrafluoroethane (HFC-134a, GWP = 1300). It has similar refrigeration performance to HFC-134a and is currently considered to be an ideal substitute for HFC-134a. In addition to being a refrigerant, HFO-1234yf can also be used as a monomer to prepare various fluorinated polymers.
[0003] Fluorine-chlorine exchange reaction is one of the commonly used reactions in the preparation of HFO-1234yf, and one of the routes is as follows: CCl4→CCl3CH2CH2Cl(HCC-250fb)→CCl3CHClCH2Cl(HCC-240db)→CF3CCl=CH2(HCFO-1233xf)→CF3CF=CH2(HFO-1234yf). The third and fourth steps can be carried out under the action of chromium catalyst, so they can be combined in the same reactor.
[0004] For example, patent CN202010715374.7 uses a loaded (the carrier can be selected from fluorinated alumina, fluorinated chromium oxide, fluorinated activated carbon or graphite carbon) or unloaded chromium catalyst, which can catalyze the reaction of HCC-240db→HCFO-1233xf→HFO-1234yf, thereby completing these two steps of reaction using a reactor equipped with a chromium catalyst. However, there are the following problems: HCFO-1233xf and HFO-1234yf are both short-chain olefins, which are easily polymerized to form carbon deposits, causing the active sites in the chromium catalyst to be covered and the catalytic activity to be reduced. Summary of the invention
[0005] In order to solve the technical problem that the existing fluorine-chlorine exchange reaction catalyst has poor anti-carbon deposition effect, the present invention provides a fluorine-chlorine exchange reaction catalyst. The catalyst can achieve good anti-carbon deposition effect, can still maintain good catalytic activity after long-term use, and can also improve the catalytic performance of the supported chromium catalyst and accelerate the reaction rate.
[0006] The specific technical scheme of the present invention is: In the first aspect, the present invention provides a fluorine-chlorine exchange reaction catalyst, which includes a core layer, a hollow layer and a shell layer from the inside to the outside; the core layer and the shell layer are both loaded with chromium fluoride oxide; the shell layer is distributed with channels connecting the hollow layer with the outside; and the hollow layer is distributed with a carbon fiber network.
[0007] The present invention provides a hollow layer between the core layer and the shell layer, and provides a pore in the shell layer that connects the hollow layer with the outside (i.e., the outside of the catalyst). The hollow layer can be used to connect the pores in the shell layer to each other. When used to catalyze the fluorine-chlorine exchange reaction, it helps to accelerate the adsorption of the substrate and the desorption process of the product, thereby increasing the reaction rate. At the same time, it can also shorten the residence time of olefins (substrate and product) in the catalyst, slow down the formation of carbon deposits, and enable the catalyst to maintain a high activity after long-term use.
[0008] When the catalyst only has a hollow shell layer and no core layer, although the internal cavity can also be used to interconnect the pores in the shell layer, the cavity size is too large, and the hollow cage-like structure formed will cause the reaction substrate and product to stay in the internal cavity of the catalyst for too long, resulting in a weak anti-carbon deposition effect of the catalyst. The present invention, by providing a core layer inside the catalyst, can reduce the space of the hollow structure, thereby effectively shortening the residence time of the reaction substrate and product inside the catalyst and achieving a better anti-carbon deposition effect.
[0009] In addition, the catalyst of the present invention has good catalytic effect and anti-carbon deposition effect when used in the fluorine-chlorine exchange reaction of 1,1,1,2,3-pentachloropropane (HCC-240db)→2-chloro-3,3,3-trifluoropropene (HCFO-1233xf) and the fluorine-chlorine exchange reaction of 2-chloro-3,3,3-trifluoropropene→2,3,3,3-tetrafluoropropene (HFO-1234yf). Therefore, when using the catalyst of the present invention to prepare HFO-1234yf, the above two steps of reaction can be combined in the same reaction container.
[0010] Preferably, the diameter of the core layer carrier is 5 to 15 μm, the thickness of the hollow layer is 0.5 to 1 μm, and the thickness of the catalytic shell layer is 0.5 to 10 μm.
[0011] To a certain extent, increasing the thickness of the hollow layer is conducive to the circulation of substrates and products in and out of the catalyst, thereby improving the reaction rate and the anti-carbon deposition effect; however, when the thickness of the hollow layer is too large, the retention time of the product and substrate in the hollow layer will be prolonged, so further increasing the thickness of the hollow layer will cause the anti-carbon deposition effect to decrease. Based on this, the present invention, on the basis of setting a hollow layer to improve the reaction rate and the anti-carbon deposition effect, can further improve the anti-carbon deposition effect of the catalyst by controlling the thickness of the hollow layer within the range of 0.5 to 1 μm.
[0012] Preferably, the core layer and the shell layer both include a porous support and chromium fluoride oxide supported on the porous support.
[0013] Furthermore, the core layer and the shell layer also include a promoter supported on a porous carrier; the promoter contains one or more elements selected from the group consisting of Ni, Zn, Co, Cu, Mn and Mg.
[0014] Furthermore, the porous carriers in the core layer and the shell layer are both fluorinated aluminum oxide.
[0015] In a second aspect, the present invention provides a method for preparing the fluorine-chlorine exchange reaction catalyst, comprising the following steps: (1) After the inorganic porous microspheres are coated with a bacterial cellulose / SiO2 composite layer, the bacterial cellulose is calcined to carbonize the bacterial cellulose to obtain double-layer structure particles; (2) coating the double-layer structure particles with a shell carrier to obtain a three-layer structure particle; (3) reacting the three-layer structure particles with HF to remove SiO2 and obtain hollow particles; (4) Chromium oxide is loaded on the hollow particles by impregnation and calcination, and then activated with HF to prepare a fluorine-chlorine exchange reaction catalyst.
[0016] In the above preparation process, by coating SiO2 on the outside of the inorganic porous microspheres, then coating the shell layer carrier, and then using HF to remove SiO2, a hollow layer can be formed between the inorganic porous microspheres and the shell layer; at the same time, in the process of using HF to remove SiO2, the two react to generate SiF4 gas, which when released can form channels in the shell layer that connect the hollow layer with the outside world.
[0017] In addition, the present invention introduces bacterial cellulose when coating the SiO2 layer. The bacterial cellulose has a relatively large branched structure and can form a carbon fiber network after carbonization, thereby playing a supporting role between the shell layer and the inorganic porous microspheres, and helping to prevent the shell structure from being damaged or collapsed during the process of HF removing SiO2 and generating SiF4 gas, thereby ensuring that the shell layer and the hollow layer can better play their role in increasing the reaction rate and preventing carbon deposition.
[0018] Preferably, in step (1), the process of coating the inorganic porous microspheres with a bacterial cellulose / SiO2 composite layer specifically comprises the following steps: mixing the inorganic porous microspheres, bacterial cellulose and solvent I, adding a silicon source dropwise thereto, performing a hydrolysis condensation reaction, and separating the product; the mass ratio of the silicon source in terms of Si to the bacterial cellulose is 1:0.2-0.6.
[0019] Preferably, in step (1), the inorganic porous microspheres are spherical γ-Al2O3.
[0020] Preferably, in step (1), the calcination process specifically includes the following steps: in an oxygen-free atmosphere, heating to 250-350°C at a rate of 1-3°C / min and keeping warm for 1-2h, then heating to 400-500°C at a rate of 2-5°C / min and keeping warm for 1-2h, and then heating to 700-800°C at a rate of 5-10°C / min and keeping warm for 2-3h.
[0021] Preferably, in step (2), the shell layer carrier is alumina.
[0022] Furthermore, step (2) specifically includes the following steps: after mixing the aluminum source, the double-layer structure particles and the solvent II, adding an alkali solution, performing a coating reaction, separating the product, repeating the above process, and then calcining.
[0023] Preferably, step (3) specifically comprises the following steps: placing the three-layer structure particles in an HF solution and reacting at 70-80° C. for 2-3 hours.
[0024] Furthermore, the concentration of the HF solution is 15-20wt%.
[0025] Preferably, in step (4), the process of loading chromium oxide on the hollow particles by impregnation and calcination specifically comprises the following steps: placing the hollow particles in Cr 3+ After being fully immersed in the solution, take it out and calcine it at 400-450°C in an oxygen-free atmosphere for 5-8 hours.
[0026] Preferably, in step (4), the activation temperature is 350-400° C. and the activation time is 8-10 h.
[0027] In a third aspect, the present invention provides an application of the fluorine-chlorine exchange reaction catalyst in the preparation of 2,3,3,3-tetrafluoropropene, wherein the fluorine-chlorine exchange reaction catalyst is used to catalyze the reaction of 1,1,1,2,3-pentachloropropane with HF to generate 2,3,3,3-tetrafluoropropene.
[0028] Preferably, the application comprises the following steps: placing the fluorine-chlorine exchange reaction catalyst in a reaction container, introducing 1,1,1,2,3-pentachloropropane and HF into the reaction container to carry out a fluorine-chlorine exchange reaction, separating 2,3,3,3-tetrafluoropropene from the product and returning the product to the reaction container, introducing 1,1,1,2,3-pentachloropropane and HF into the reaction container to carry out a fluorine-chlorine exchange reaction to generate 2,3,3,3-tetrafluoropropene.
[0029] Under the action of the catalyst of the present invention, the fluorine-chlorine exchange reaction of HCC-240db→HCFO-1233xf and the fluorine-chlorine exchange reaction of HCFO-1233xf→HFO-1234yf can be combined and carried out in the same reaction container. Specifically, when the materials (HCC-240db and HF) are first introduced into the reaction container, the reaction of HCC-240db→HCFO-1233xf mainly occurs, and at the same time, part of HCFO-1233xf is further converted into HFO-1234yf. In addition, A side reaction of HFO-1234yf→1,1,1,2,2-pentafluoropropane (HFC-245cb) will occur. After HFO-1234yf is separated from the product, the remaining gas containing HCFO-1233xf and HFC-245cb is reintroduced into the reaction container to further convert HCFO-1233xf into HFO-1234yf. In this process, the presence of HFC-245cb in the gas can inhibit the side reaction of HFO-1234yf→HFC-245cb.
[0030] Compared with the prior art, the present invention has the following advantages: (1) In the fluorine-chlorine exchange reaction catalyst of the present invention, by providing a hollow layer between the core layer and the shell layer, and providing a channel in the shell layer connecting the hollow layer with the outside, the catalyst can achieve a faster reaction rate and better anti-carbon deposition effect when used in the fluorine-chlorine exchange reaction.
[0031] (2) In the process of preparing the fluorine-chlorine exchange reaction catalyst, the bacterial cellulose is introduced when coating the SiO2 layer, so that the structure of the hollow layer and the shell layer can be better maintained, thereby further improving the reaction rate and the anti-carbon deposition effect.
[0032] (3) The fluorine-chlorine exchange reaction catalyst of the present invention can exert a good catalytic effect in the reactions of HCC-240db→HCFO-1233xf and HCFO-1233xf→HFO-1234yf, so the two-step reactions can be combined in the same reaction vessel. DETAILED DESCRIPTION
[0033] The present invention will be further described below in conjunction with embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. Without departing from the spirit and scope of the inventive concept, changes and advantages that can be imagined by those skilled in the art are included in the present invention, and the attached claims and any equivalents thereof are the protection scope of the present invention.
[0034] Overall embodiment A fluorine-chlorine exchange reaction catalyst comprises a core layer, a hollow layer and a shell layer from the inside to the outside; the core layer and the shell layer are both loaded with chromium fluoride oxide; the shell layer is provided with pores connecting the hollow layer with the outside; and the hollow layer is provided with a carbon fiber network.
[0035] As a specific implementation, the diameter of the core layer carrier is 5 to 15 μm, the thickness of the hollow layer is 0.5 to 1 μm, and the thickness of the catalytic shell layer is 0.5 to 10 μm.
[0036] As a specific implementation, the core layer and the shell layer both include a porous carrier, and a fluorinated chromium oxide and a promoter supported on the porous carrier; the promoter contains one or more elements of Ni, Zn, Co, Cu, Mn and Mg; the porous carrier in the core layer and the shell layer can be fluorinated aluminum oxide.
[0037] A method for preparing the fluorine-chlorine exchange reaction catalyst comprises the following steps: (1) After the inorganic porous microspheres are coated with a bacterial cellulose / SiO2 composite layer, the bacterial cellulose is calcined to carbonize the bacterial cellulose to obtain double-layer structure particles; (2) coating the double-layer structure particles with a shell carrier to obtain a three-layer structure particle; (3) reacting the three-layer structure particles with HF to remove SiO2 and obtain hollow particles; (4) Chromium oxide is loaded on the hollow particles by impregnation and calcination, and then activated with HF to prepare a fluorine-chlorine exchange reaction catalyst.
[0038] As a specific implementation method, step (1) specifically includes the following steps: mixing inorganic porous microspheres, bacterial cellulose and solvent I, adding a silicon source dropwise thereto, performing a hydrolysis condensation reaction, separating the product, and then heating to 250-350°C at a rate of 1-3°C / min in an oxygen-free atmosphere and keeping the temperature for 1-2h, then heating to 400-500°C at a rate of 2-5°C / min and keeping the temperature for 1-2h, and then heating to 700-800°C at a rate of 5-10°C / min and keeping the temperature for 2-3h; the mass ratio of the silicon source in terms of Si to the bacterial cellulose is 1:0.2-0.6.
[0039] As a specific implementation, in step (1), the inorganic porous microspheres are spherical γ-Al2O3.
[0040] As a specific implementation, in step (2), the shell carrier is alumina; step (2) specifically includes the following steps: after mixing the aluminum source, double-layer structure particles and solvent II, adding alkaline solution, carrying out coating reaction, separating the product, repeating the above process, and then calcining.
[0041] As a specific implementation, step (3) specifically includes the following steps: placing the three-layer structure particles in a 15-20wt% HF solution and reacting at 70-80°C for 2-3h.
[0042] As a specific implementation, step (4) specifically includes the following steps: placing the hollow particles in Cr 3+ After being fully immersed in the solution, the product is taken out and calcined at 400-450°C in an oxygen-free atmosphere for 5-8 hours, and then placed in an HF gas flow and activated at 350-400°C for 8-10 hours.
[0043] The fluorine-chlorine exchange reaction catalyst is used in the preparation of 2,3,3,3-tetrafluoropropene, wherein the fluorine-chlorine exchange reaction catalyst is used to catalyze the reaction of 1,1,1,2,3-pentachloropropane and HF to generate 2,3,3,3-tetrafluoropropene.
[0044] As a specific implementation, the application includes the following steps: placing the fluorine-chlorine exchange reaction catalyst in a reaction container, introducing 1,1,1,2,3-pentachloropropane and HF into the reaction container to carry out a fluorine-chlorine exchange reaction, separating 2,3,3,3-tetrafluoropropene from the product and returning it to the reaction container, and introducing 1,1,1,2,3-pentachloropropane and HF to carry out a fluorine-chlorine exchange reaction to generate 2,3,3,3-tetrafluoropropene. Specific embodiments Unless otherwise defined, all technical terms and scientific terms used in the present invention have the same meanings as those commonly understood by ordinary technicians in the field to which the present disclosure belongs. Unless otherwise specified, the raw materials and equipment used in the present invention are conventional raw materials and equipment in the field and can be obtained from conventional commercial channels; unless otherwise specified, the methods used in the present invention are conventional methods in the field.
[0046] In the following examples and comparative examples, the meanings of the abbreviations are as follows: CTAB: hexadecyltrimethylammonium bromide; HCC-240db: 1,1,1,2,3-pentachloropropane; HCFO-1233xf: 2-chloro-3,3,3-trifluoropropene; HFO-1234yf: 2,3,3,3-tetrafluoropropene; HFC-245cb: 1,1,1,2,2-pentafluoropropane.
[0047] Example 1: Preparation of fluorine-chlorine exchange reaction catalyst A fluorine-chlorine exchange reaction catalyst is prepared by the following steps: (1) Making the middle layer: Disperse 10g CTAB and 11.5g bacterial cellulose in 200mL water to prepare a dispersion. Disperse 50g spherical γ-Al2O3 with a particle size of 5-10μm in 500mL anhydrous ethanol, add the dispersion, ultrasonicate for 30min, adjust the pH to 9.5, heat to 70℃, add 180mL tetraethyl silicate dropwise at a rate of 0.5mL / min under stirring, continue stirring at 70℃ for 5.5h, separate by suction filtration, wash with water and dry, and transfer to a tube furnace. Nitrogen was filled into the tubular furnace to replace the air in the furnace, and then the temperature was increased to 300°C at a rate of 2°C / min and maintained for 1.5 h, then increased to 450°C at a rate of 3°C / min and maintained for 1.5 h, and then increased to 750°C at a rate of 6°C / min and maintained for 2.5 h. The mixture was naturally cooled to room temperature to obtain double-layer structure particles, in which the thickness of the outer layer was 0.5 to 1 μm.
[0048] (2) Shell layer: The double-layer structure particles prepared in step (1) are dispersed in 500 mL of ethanol / water (v / v=3:2) mixed solution, and 150 mL of 15 wt% AlCl3 aqueous solution is added dropwise thereto under stirring. After the addition is completed, the temperature is raised to 65°C, and the pH is adjusted to 7.5 with a 5M sodium hydroxide solution. Stirring is continued at 65°C for 24 hours, and the first coating is completed after separation by suction filtration and drying. The first coating step is repeated for a total of 4 times, and then transferred to a tube furnace, heated to 600°C at a rate of 15°C / min and maintained for 2 hours to obtain three-layer structure particles, wherein the thickness of the outermost layer is 1 to 5 μm.
[0049] (3) Making the hollow layer: The three-layer structure particles prepared in step (2) were dispersed in 500 mL of 15 wt % HF solution and stirred at 70° C. for 3 h to obtain hollow particles.
[0050] (4) Loading chromium oxide and promoter: The hollow particles prepared in step (3) are dispersed in 750 mL of an aqueous solution containing Cr(NO3)3, Co(NO3)2 and Zn(NO3)2, wherein the amounts of Cr(NO3)3, Co(NO3)2 and Zn(NO3)2 are 5 wt%, 0.25 wt% and 0.25 wt% respectively based on the loading amounts of Cr, Co and Zn. After immersion for 12 h, the mixture is filtered and dried, and then transferred to a tubular furnace. After nitrogen is introduced to replace the air in the furnace, the mixture is heated to 450°C at a rate of 15°C / min and maintained for 5 h, and then cooled to 350°C. HF gas is introduced into the furnace and maintained at 350°C for 10 h to obtain a fluorine-chlorine exchange reaction catalyst.
[0051] Example 2: Preparation of fluorine-chlorine exchange reaction catalyst A fluorine-chlorine exchange reaction catalyst is prepared by the following steps: (1) Making the middle layer: 10g CTAB and 2g bacterial cellulose were dispersed in 200mL water to prepare a dispersion. 50g spherical γ-Al2O3 with a particle size of 10-15μm was dispersed in 500mL anhydrous ethanol, and the dispersion was added thereto. After ultrasonication for 30min, the pH was adjusted to 9.5, the temperature was raised to 70℃, and 160mL tetraethyl silicate was added dropwise at a rate of 0.5mL / min under stirring. After the addition, stirring was continued at 70℃ for 6h. After separation by suction filtration, washing and drying, it was transferred to a tubular furnace. Nitrogen was filled into the tubular furnace to replace the air in the furnace, and then the temperature was raised to 250℃ at a rate of 1℃ / min and maintained for 2h, then raised to 500℃ at a rate of 2℃ / min and maintained for 1h, and then raised to 800℃ at a rate of 5℃ / min and maintained for 2h, and naturally cooled to room temperature to obtain double-layer structure particles, in which the thickness of the outer layer was 0.5-1μm.
[0052] (2) Shell layer: The double-layer structure particles prepared in step (1) are dispersed in 500 mL of ethanol / water (v / v=3:2) mixed solution, and 45 mL of 15 wt% AlCl3 aqueous solution is added dropwise thereto under stirring. After the addition is completed, the temperature is raised to 60°C, and the pH is adjusted to 8 with a 5M sodium hydroxide solution. Stirring is continued at 60°C for 24 hours, and the first coating is completed after separation by suction filtration and drying. The first coating step is repeated for a total of 3 times, and then transferred to a tube furnace, heated to 600°C at a rate of 15°C / min and maintained for 2 hours to obtain three-layer structure particles, wherein the thickness of the outermost layer is 0.5 to 1.5 μm.
[0053] (3) Making the hollow layer: The three-layer structure particles prepared in step (2) were dispersed in 500 mL of 15 wt % HF solution and stirred at 70° C. for 3 h to obtain hollow particles.
[0054] (4) Loading chromium oxide and promoter: The hollow particles prepared in step (3) are dispersed in 750 mL of an aqueous solution containing Cr(NO3)3, Co(NO3)2 and Zn(NO3)2, wherein the amounts of Cr(NO3)3, Co(NO3)2 and Zn(NO3)2 are 5 wt%, 0.25 wt% and 0.25 wt% respectively based on the loading amounts of Cr, Co and Zn. After immersion for 12 h, the mixture is filtered and dried, and then transferred to a tubular furnace. After nitrogen is introduced to replace the air in the furnace, the temperature is increased to 400°C at a rate of 20°C / min and maintained for 8 h, and then cooled to 400°C. HF gas is introduced into the furnace and maintained at 400°C for 8 h to obtain a fluorine-chlorine exchange reaction catalyst.
[0055] Example 3: Preparation of fluorine-chlorine exchange reaction catalyst A fluorine-chlorine exchange reaction catalyst is prepared by the following steps: (1) Making the middle layer: 10g CTAB and 13.3g bacterial cellulose were dispersed in 200mL water to prepare a dispersion. 50g spherical γ-Al2O3 with a particle size of 5-10μm was dispersed in 500mL anhydrous ethanol, and the dispersion was added thereto. After ultrasonication for 30min, the pH was adjusted to 9.5, the temperature was raised to 70℃, and 175mL tetraethyl silicate was added dropwise at a rate of 0.5mL / min under stirring. After the addition, stirring was continued at 70℃ for 5h. After separation by suction filtration, washing and drying, it was transferred to a tube furnace. Nitrogen was filled into the tube furnace to replace the air in the furnace, and then the temperature was raised to 350℃ at a rate of 3℃ / min and maintained for 1h, then raised to 400℃ at a rate of 5℃ / min and maintained for 1h, and then raised to 700℃ at a rate of 10℃ / min and maintained for 3h, and then naturally cooled to room temperature to obtain double-layer structure particles, in which the thickness of the outer layer was 0.5-1μm.
[0056] (2) Shell layer: The double-layer structure particles prepared in step (1) are dispersed in 500 mL of ethanol / water (v / v=3:2) mixed solution, and 500 mL of 15 wt% AlCl3 aqueous solution is added dropwise thereto under stirring. After the addition is completed, the temperature is raised to 70°C, and the pH is adjusted to 7 with a 5M sodium hydroxide solution. Stirring is continued at 70°C for 24 hours, and the first coating is completed after separation by suction filtration and drying. The first coating step is repeated for a total of 6 times, and then transferred to a tube furnace, heated to 600°C at a rate of 15°C / min and maintained for 2 hours to obtain three-layer structure particles, wherein the thickness of the outermost layer is 5 to 10 μm.
[0057] (3) Making the hollow layer: The three-layer structure particles prepared in step (2) were dispersed in 500 mL of 20 wt % HF solution and stirred at 80° C. for 2 h to obtain hollow particles.
[0058] (4) Loading chromium oxide and promoter: The hollow particles prepared in step (3) are dispersed in 750 mL of an aqueous solution containing Cr(NO3)3, Co(NO3)2 and Zn(NO3)2, wherein the amounts of Cr(NO3)3, Co(NO3)2 and Zn(NO3)2 are 5 wt%, 0.25 wt% and 0.25 wt% respectively based on the loading amounts of Cr, Co and Zn. After immersion for 12 h, the mixture is filtered and dried, and then transferred to a tubular furnace. After nitrogen is introduced to replace the air in the furnace, the mixture is heated to 450°C at a rate of 15°C / min and maintained for 5 h, and then cooled to 350°C. HF gas is introduced into the furnace and maintained at 350°C for 10 h to obtain a fluorine-chlorine exchange reaction catalyst.
[0059] Example 4: Preparation of fluorine-chlorine exchange reaction catalyst A fluorine-chlorine exchange reaction catalyst is prepared by the following steps: (1) Making the middle layer: 10g CTAB and 11.5g bacterial cellulose were dispersed in 200mL water to prepare a dispersion. 50g spherical γ-Al2O3 with a particle size of 5-10μm was dispersed in 500mL anhydrous ethanol, and the dispersion was added thereto. After ultrasonication for 30min, the pH was adjusted to 9.5, the temperature was raised to 70℃, and 30mL tetraethyl silicate was added dropwise at a rate of 0.5mL / min under stirring. After the addition, stirring was continued at 70℃ for 5.5h. After separation by suction filtration, washing and drying, it was transferred to a tubular furnace. Nitrogen was filled into the tubular furnace to replace the air in the furnace, and then the temperature was raised to 300℃ at a rate of 2℃ / min and maintained for 1.5h, then raised to 450℃ at a rate of 3℃ / min and maintained for 1.5h, and then raised to 750℃ at a rate of 6℃ / min and maintained for 2.5h, and naturally cooled to room temperature to obtain double-layer structure particles, in which the thickness of the outer layer was 50-200nm.
[0060] (2) Shell layer: The double-layer structure particles prepared in step (1) are dispersed in 500 mL of ethanol / water (v / v=3:2) mixed solution, and 150 mL of 15 wt% AlCl3 aqueous solution is added dropwise thereto under stirring. After the addition is completed, the temperature is raised to 65°C, and the pH is adjusted to 7.5 with a 5M sodium hydroxide solution. Stirring is continued at 65°C for 24 hours, and the first coating is completed after separation by suction filtration and drying. The first coating step is repeated for a total of 4 times, and then transferred to a tube furnace, heated to 600°C at a rate of 15°C / min and maintained for 2 hours to obtain three-layer structure particles, wherein the thickness of the outermost layer is 1 to 5 μm.
[0061] (3) Making the hollow layer: The three-layer structure particles prepared in step (2) were dispersed in 500 mL of 15 wt % HF solution and stirred at 70° C. for 3 h to obtain hollow particles.
[0062] (4) Loading chromium oxide and promoter: The hollow particles prepared in step (3) are dispersed in 750 mL of an aqueous solution containing Cr(NO3)3, Co(NO3)2 and Zn(NO3)2, wherein the amounts of Cr(NO3)3, Co(NO3)2 and Zn(NO3)2 are 5 wt%, 0.25 wt% and 0.25 wt% respectively based on the loading amounts of Cr, Co and Zn. After immersion for 12 h, the mixture is filtered and dried, and then transferred to a tubular furnace. After nitrogen is introduced to replace the air in the furnace, the mixture is heated to 450°C at a rate of 15°C / min and maintained for 5 h, and then cooled to 350°C. HF gas is introduced into the furnace and maintained at 350°C for 10 h to obtain a fluorine-chlorine exchange reaction catalyst.
[0063] Example 5: Preparation of fluorine-chlorine exchange reaction catalyst A fluorine-chlorine exchange reaction catalyst is prepared by the following steps: (1) Making the middle layer: Disperse 10g CTAB and 11.5g bacterial cellulose in 200mL water to make a dispersion. Disperse 50g spherical γ-Al2O3 with a particle size of 5-10μm in 500mL anhydrous ethanol, add the dispersion, ultrasonicate for 30min, adjust the pH to 9.5, heat to 70℃, add 180mL tetraethyl silicate dropwise at a rate of 0.5mL / min under stirring, continue stirring at 70℃ for 5.5h, filter, wash and dry to complete the first coating. Repeat the first coating step for a total of 4 times. Then transfer to a tube furnace. Nitrogen was filled into the tubular furnace to replace the air in the furnace, and then the temperature was increased to 300°C at a rate of 2°C / min and maintained for 1.5 h, then increased to 450°C at a rate of 3°C / min and maintained for 1.5 h, and then increased to 750°C at a rate of 6°C / min and maintained for 2.5 h. The mixture was naturally cooled to room temperature to obtain double-layer structure particles, in which the thickness of the outer layer was 1 to 3.5 μm.
[0064] (2) Shell layer: The double-layer structure particles prepared in step (1) are dispersed in 500 mL of ethanol / water (v / v=3:2) mixed solution, and 150 mL of 15 wt% AlCl3 aqueous solution is added dropwise thereto under stirring. After the addition is completed, the temperature is raised to 65°C, and the pH is adjusted to 7.5 with a 5M sodium hydroxide solution. Stirring is continued at 65°C for 24 hours, and the first coating is completed after separation by suction filtration and drying. The first coating step is repeated for a total of 4 times, and then transferred to a tube furnace, heated to 600°C at a rate of 15°C / min and maintained for 2 hours to obtain three-layer structure particles, wherein the thickness of the outermost layer is 1 to 5 μm.
[0065] (3) Making the hollow layer: The three-layer structure particles prepared in step (2) were dispersed in 500 mL of 15 wt % HF solution and stirred at 70° C. for 3 h to obtain hollow particles.
[0066] (4) Loading chromium oxide and promoter: The hollow particles prepared in step (3) are dispersed in 750 mL of an aqueous solution containing Cr(NO3)3, Co(NO3)2 and Zn(NO3)2, wherein the amounts of Cr(NO3)3, Co(NO3)2 and Zn(NO3)2 are 5 wt%, 0.25 wt% and 0.25 wt% respectively based on the loading amounts of Cr, Co and Zn. After immersion for 12 h, the mixture is filtered and dried, and then transferred to a tubular furnace. After nitrogen is introduced to replace the air in the furnace, the mixture is heated to 450°C at a rate of 15°C / min and maintained for 5 h, and then cooled to 350°C. HF gas is introduced into the furnace and maintained at 350°C for 10 h to obtain a fluorine-chlorine exchange reaction catalyst.
[0067] Example 6: Preparation of fluorine-chlorine exchange reaction catalyst A fluorine-chlorine exchange reaction catalyst is prepared by the following steps: (1) Making the middle layer: Dissolve 10g CTAB in 200mL water to prepare CTAB solution. Disperse 50g spherical γ-Al2O3 with a particle size of 5-10μm in 500mL anhydrous ethanol, add CTAB solution, ultrasonicate for 30min, adjust pH to 9.5, heat to 70℃, add 190mL tetraethyl silicate dropwise at a rate of 0.5mL / min under stirring, continue stirring at 70℃ for 5.5h after addition, filter, wash and dry, and transfer to a tube furnace. Fill the tube furnace with nitrogen to replace the air in the furnace, then heat to 300℃ at a rate of 2℃ / min and keep for 1.5h, then heat to 450℃ at a rate of 3℃ / min and keep for 1.5h, then heat to 750℃ at a rate of 6℃ / min and keep for 2.5h, cool naturally to room temperature, and obtain double-layer structure particles, in which the thickness of the outer layer is 0.5-1μm.
[0068] (2) Shell layer: The double-layer structure particles prepared in step (1) are dispersed in 500 mL of ethanol / water (v / v=3:2) mixed solution, and 150 mL of 15 wt% AlCl3 aqueous solution is added dropwise thereto under stirring. After the addition is completed, the temperature is raised to 65°C, and the pH is adjusted to 7.5 with a 5M sodium hydroxide solution. Stirring is continued at 65°C for 24 hours, and the first coating is completed after separation by suction filtration and drying. The first coating step is repeated for a total of 4 times, and then transferred to a tube furnace, heated to 600°C at a rate of 15°C / min and maintained for 2 hours to obtain three-layer structure particles, wherein the thickness of the outermost layer is 1 to 5 μm.
[0069] (3) Making the hollow layer: The three-layer structure particles prepared in step (2) were dispersed in 500 mL of 15 wt % HF solution and stirred at 70° C. for 3 h to obtain hollow particles.
[0070] (4) Loading chromium oxide and promoter: The hollow particles prepared in step (3) are dispersed in 750 mL of an aqueous solution containing Cr(NO3)3, Co(NO3)2 and Zn(NO3)2, wherein the amounts of Cr(NO3)3, Co(NO3)2 and Zn(NO3)2 are 5 wt%, 0.25 wt% and 0.25 wt% respectively based on the loading amounts of Cr, Co and Zn. After immersion for 12 h, the mixture is filtered and dried, and then transferred to a tubular furnace. After nitrogen is introduced to replace the air in the furnace, the mixture is heated to 450°C at a rate of 15°C / min and maintained for 5 h, and then cooled to 350°C. HF gas is introduced into the furnace and maintained at 350°C for 10 h to obtain a fluorine-chlorine exchange reaction catalyst.
[0071] Comparative Example 1: Preparation of Fluorine-Chlorine Exchange Reaction Catalyst A fluorine-chlorine exchange reaction catalyst is prepared by the following steps: 50g of spherical γ-Al2O3 with a particle size of 5 to 10μm was dispersed in 750mL of an aqueous solution containing Cr(NO3)3, Co(NO3)2 and Zn(NO3)2, wherein the amounts of Cr(NO3)3, Co(NO3)2 and Zn(NO3)2 were calculated based on the loading amounts of Cr, Co and Zn, respectively, and after immersion for 12h, the mixture was filtered, dried and transferred to a tubular furnace. After nitrogen was introduced to replace the air in the furnace, the temperature was increased to 450℃ at a rate of 15℃ / min and maintained for 5h, and then cooled to 350℃. HF gas was introduced into the furnace and maintained at 350℃ for 10h to obtain a fluorine-chlorine exchange reaction catalyst.
[0072] Application example: Application of fluorine-chlorine exchange reaction catalyst in the preparation of HFO-1234yf HFO-1234yf is prepared from HCC-240db by the following steps: S1: Take 10g of each catalyst prepared in Examples 1 to 6 and Comparative Example 1, respectively, and load them into a tubular reactor. After sealing, heat the reactor to 300°C, introduce 1,1,1,2,3-pentachloropropane and HF, with flow rates of 15g / min and 38g / min respectively (Comparative Example 1 also introduces O2, with a flow rate of 2g / min), collect the gas at the outlet, and maintain the temperature in the reactor at 300°C and the pressure at normal pressure. After continuous use for 20h, sample the gas collected from the outlet and use gas chromatography to detect the content (molar fraction) of HCFO-1233xf, HFO-1234yf and HFC-245cb therein, and the results are shown in Table 1. After continuous use for 150h, sample again to detect the content (molar fraction) of each component in the gas at the outlet, and the results are shown in Table 1.
[0073] S2: The gas collected at the outlet in step S1 is distilled to separate HFO-1234yf, and the remaining gas is re-introduced into the tubular reactor containing the catalyst in step S1 at a flow rate of 9 g / min, and 1,1,1,2,3-pentachloropropane and HF are introduced at flow rates of 15 g / min and 70 g / min respectively (comparative example 1 also introduces O2 at a flow rate of 4 g / min), and the gas at the outlet is collected, and the temperature in the reactor is maintained at 300°C and the pressure is normal pressure. After 20 hours (if the use time in step S1 is included, the total use time is 170 hours), a sample is taken from the gas collected at the outlet and the HFO-1234yf and HFC-245cb content (molar fraction) thereof is detected by gas chromatography, and the results are shown in Table 2. After 150 hours of continuous use (if the use time in step S1 is included, the total continuous use time is 300 hours), samples are taken again to detect the content (molar fraction) of each component in the gas at the outlet. The results are shown in Table 2.
[0074] Table 1 Table 2 According to the test results in Table 1 and Table 2, it can be seen that: (1) Compared with Comparative Example 1, when the material is first introduced into the reactor (step S1), Example 1 can achieve a higher yield of HCFO-1233xf and HFO-1234yf, and when the material is introduced into the reactor again (step S2), it can achieve a higher yield of HFO-1234yf, and can maintain a high yield of HFO-1234yf after long-term use. This is because: Example 1 sets a hollow layer and a shell layer in the catalyst, and uses the hollow layer to interconnect the pores in the shell layer. When used to catalyze the fluorine-chlorine exchange reaction, it helps to accelerate the adsorption of the substrate and the desorption process of the product, thereby increasing the reaction rate. At the same time, it can also shorten the residence time of olefins (substrate and product) in the catalyst, slow down the formation of carbon deposits, and enable the catalyst to maintain a high activity after long-term use. In addition, after the material was introduced into the reactor again, the HFC-245cb content in the outlet gas obtained in Example 1 was lower than that in Comparative Example 1. This may be because Example 1 shortened the residence time of the material in the product HFO-1234yf, thereby reducing its further reaction to generate HFC-245cb.
[0075] (2) Compared with Examples 4 and 5, Example 1 can maintain a higher HFO-1234yf yield after long-term use. This is because: the hollow layer thickness in Example 4 is relatively small, which is not conducive to accelerating the circulation of substrates and products in and out of the catalyst, so the anti-carbon deposition effect is relatively weak; the hollow layer thickness in Example 5 is relatively large, and the retention time of products and substrates in the hollow layer is prolonged, which will also have an adverse effect on the anti-carbon deposition effect of the catalyst.
[0076] (3) Compared with Example 6, Example 1 can achieve higher HCFO-1233xf and HFO-1234yf yields when the material is first introduced into the reactor (step S1), and can achieve higher HFO-1234yf yields when the material is introduced into the reactor again (step S2), and can maintain a higher HFO-1234yf yield after long-term use. This is because: during the catalyst preparation process, when HF is used to remove SiO2, the supporting effect of SiO2 on the shell layer disappears, and the released gas will impact the shell layer, so the problem of partial collapse of the shell layer is prone to occur; Example 1 introduces bacterial cellulose when coating the SiO2 layer, which can form a carbon fiber network after carbonization, and play a supporting role between the shell layer and the inorganic porous microspheres, thereby avoiding the collapse of the shell layer, so as to ensure that the shell layer and the hollow layer can better play their role in improving the reaction rate and preventing carbon deposition.
[0077] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A fluorine-chlorine exchange reaction catalyst, It is characterized in that From the inside to the outside, it includes a core layer, a hollow layer and a shell layer; the core layer and the shell layer are both loaded with chromium fluoride oxide; the shell layer is provided with channels connecting the hollow layer with the outside; and the hollow layer is provided with a carbon fiber network.
2. The fluorine-chlorine exchange reaction catalyst according to claim 1, It is characterized in that The diameter of the core layer carrier is 5-15 μm, the thickness of the hollow layer is 0.5-1 μm, and the thickness of the catalytic shell layer is 0.5-10 μm.
3. The fluorine-chlorine exchange reaction catalyst according to claim 1, It is characterized in that The core layer and the shell layer both include a porous support and chromium fluoride oxide supported on the porous support.
4. The fluorine-chlorine exchange reaction catalyst according to claim 3, It is characterized in that The core layer and the shell layer further include a promoter supported on a porous carrier; the promoter contains one or more elements selected from the group consisting of Ni, Zn, Co, Cu, Mn and Mg.
5. A method for preparing the fluorine-chlorine exchange reaction catalyst according to any one of claims 1 to 4, It is characterized in that The following steps are involved: (1) Coating the inorganic porous microspheres with bacterial cellulose / SiO 2 After the composite layer, calcination is performed to carbonize the bacterial cellulose to obtain double-layer structure particles; (2) coating the double-layer structure particles with a shell carrier to obtain a three-layer structure particle; (3) Removal of SiO by reacting the three-layer structure particles with HF 2 , to obtain hollow particles; (4) Chromium oxide is loaded on the hollow particles by impregnation and calcination, and then activated with HF to prepare a fluorine-chlorine exchange reaction catalyst.
6. The preparation method according to claim 5, It is characterized in that In step (1), the inorganic porous microspheres are coated with bacterial cellulose / SiO 2 The composite layer process specifically includes the following steps: mixing inorganic porous microspheres, bacterial cellulose and solvent I, adding silicon source dropwise thereto, performing hydrolysis condensation reaction, and separating the product; the mass ratio of the silicon source to the bacterial cellulose is 1:0.2-0.6 in terms of Si.
7. The preparation method according to claim 5, It is characterized in that In step (1), the calcination process specifically includes the following steps: in an oxygen-free atmosphere, heating to 250-350°C at a rate of 1-3°C / min and keeping warm for 1-2h, then heating to 400-500°C at a rate of 2-5°C / min and keeping warm for 1-2h, and then heating to 700-800°C at a rate of 5-10°C / min and keeping warm for 2-3h.
8. The preparation method according to claim 5, It is characterized in that In step (4), the activation temperature is 350-400° C. and the activation time is 8-10 hours.
9. Use of the fluorine-chlorine exchange reaction catalyst according to any one of claims 1 to 4 in the preparation of 2,3,3,3-tetrafluoropropene, It is characterized in that The fluorine-chlorine exchange reaction catalyst is used for catalyzing the reaction of 1,1,1,2,3-pentachloropropane with HF to generate 2,3,3,3-tetrafluoropropene.
10. The use according to claim 9, It is characterized in that The method comprises the following steps: placing the fluorine-chlorine exchange reaction catalyst in a reaction container, introducing 1,1,1,2,3-pentachloropropane and HF into the reaction container to carry out a fluorine-chlorine exchange reaction, separating 2,3,3,3-tetrafluoropropene from the product and returning the product to the reaction container, introducing 1,1,1,2,3-pentachloropropane and HF into the reaction container to carry out a fluorine-chlorine exchange reaction to generate 2,3,3,3-tetrafluoropropene.
Citation Information
Patent Citations
Process for the manufacture of 2,3,3,3- tetrafluoropropene by gas phase fluorination of pentachloropropane
CN103328422A
Process for preparing 2,3,3,3-tetrafluoropropene
CN103717560A
Process for the preparation of 2,3,3,3-tetrafluoropropene
CN103998405A
Method for coproduction of 1-chloro-3,3,3-trifluoropropene, 2,3,3,3-tetrafluoropropene and 1,3,3,3-tetrafluoropropene
CN106349005A
Co-production method of trans-1-chlorine-3,3,3-trifluoropropene and 2,3,3,3-tetrafluoropropene
CN108383679A
Cited By
Method for producing alkene halogens
JP7925445B1