Compound chromite catalyst as well as preparation method and application thereof
By preparing the composite chromite catalyst, the problem of low catalyst activity of the traditional Fenton oxidation method is solved, and efficient degradation of organic pollutants in dye wastewater and the cyclic stability of the catalyst is achieved, with significant environmental and economic benefits.
Patent Information
- Application Number
- CN202411071962.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
AI Technical Summary
After the COD reaches a certain removal rate, the traditional Fenton oxidation catalyst has low catalytic activity and cannot effectively degrade organic matter.
By using the preparation method of a compound chromite catalyst, calcining chromite ore with manganese dioxide and carbonate, reacting with an inorganic alkali solution, and then calcining with nickel salt to form a catalyst with a polymetallic active catalytic center. , activate reactants and regulate electronic structure to improve catalytic performance.
It achieves efficient degradation of organic pollutants in dye wastewater, improves the cycle stability and removal rate of the catalyst, reduces production costs, and has environmental and economic benefits.
Smart Images

Figure CN118976508A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of dye wastewater treatment, and specifically relates to a composite chromite catalyst and a preparation method and application thereof. Background Art
[0002] The Fenton oxidation method was first discovered by French scientist Fenton in 1894. 2+ It can catalyze H2O2 to produce strong oxidizing OH to oxidize tartaric acid. In the 1960s, after Canadian scholar Eisenhaner first successfully used Fenton reaction to degrade phenol wastewater and alkylbenzene wastewater, Fenton oxidation method began to attract widespread attention from scholars in the field of environmental catalysis. Compared with other treatment technologies, Fenton oxidation method has the advantages of mild reaction conditions, low equipment requirements, convenient operation, low cost, fast oxidation rate, and no selectivity for oxidation objects. It can oxidize almost all organic matter and has great application potential.
[0003] Fenton reaction is one of the main methods for treating organic wastewater. It mainly uses hydrogen peroxide as an oxidant to catalyze decomposition in the presence of metal ions to produce hydroxyl radicals. Hydroxyl radicals have strong oxidizing properties, with a standard electrode potential of 2.80V, and can deeply oxidize and degrade most organic pollutants in wastewater. As an advanced oxidation process, Fenton method has many advantages in treating dye wastewater, such as non-selective reaction, mild reaction conditions, and simple operation.
[0004] After COD reaches a certain removal rate, traditional Fenton reaction catalysts can no longer remove organic matter and have low catalytic activity. Summary of the invention
[0005] The invention provides a composite chromite catalyst and a preparation method and application thereof, which solves the problem that the traditional Fenton reaction catalyst can no longer remove organic matter and has low catalytic activity after the COD removal rate reaches a certain level.
[0006] A method for preparing a composite chromite catalyst comprises the following steps:
[0007] Calcine chromite ore, manganese dioxide and carbonate at 800°C to 1000°C for 5h to 9h to obtain a calcined product; the mass ratio of the chromite ore, manganese dioxide and carbonate is 5 to 15: 2 to 3: 10 to 20;
[0008] The calcined product is reacted with an inorganic alkali solution for 8 hours to 10 hours, and the solid after filtration is an alkalized product; the mass ratio of the calcined product to the inorganic alkali solution is 1 to 5:20 to 30;
[0009] The alkali compound and the nickel salt are calcined at 500°C to 800°C for 4h to 6h, water is added after cooling, and the mixture is vigorously stirred for 2h to 4h. The solid after filtration is the composite chromite catalyst; wherein the mass ratio of the alkali compound, the nickel salt and the water is 5-8:10-14:20-30.
[0010] The prepared composite chromite catalyst has multiple metal active catalytic centers, which can activate reactants at the same time and effectively reduce the activation energy barrier of the reaction; at the same time, the regulation of the electronic structure between the metal active centers promotes the reconstruction of the catalyst surface during the reaction, and the electron transfer during the reconstruction process leads to the exposure of more reaction active sites, thus giving it excellent catalytic performance.
[0011] The addition of carbonate can activate chromite ore, combine with impurities in chromite ore to form slag and separate from metal, change the structure of chromite ore and make it easier to decompose. At the same time, the carbonate decomposition reaction can also produce gases such as carbon dioxide to prevent heat loss. These gases can form a heat-proof layer to reduce heat loss during roasting.
[0012] The purpose of adding the inorganic alkali solution is to convert some effective components in the calcined material, such as chromium, iron, and manganese, into solid precipitation as much as possible, and to remove some soluble impurities.
[0013] Preferably, the carbonate is one or more of sodium carbonate, potassium carbonate, lithium carbonate, calcium carbonate, barium carbonate, and magnesium carbonate.
[0014] Preferably, the inorganic alkali solution is one or more of sodium hydroxide solution, potassium hydroxide solution, ammonia solution, and lithium hydroxide solution; the mass concentration of the inorganic alkali solution is 20% to 30%.
[0015] Preferably, the chromite is one or more of high-chromium chromite, high-iron chromite and high-aluminum chromite.
[0016] Preferably, the nickel salt is one or more of nickel nitrate, nickel nitrite, nickel chloride, nickel bromide and nickel sulfate.
[0017] The second object of the present invention is to protect the composite chromite catalyst prepared by any one of the preparation methods.
[0018] The third object of the present invention is to protect the application of the composite chromite catalyst in the Fenton reaction.
[0019] Preferably, the specific application method is: at 10-50° C., the composite chromite catalyst and hydrogen peroxide are added to the solution of the dye to be degraded, reacted for 50 min-60 min, and the concentration of the dye to be degraded is measured; the amount of the composite chromite catalyst added is 0.1wt%-0.3wt% of the dye to be degraded, and the amount of hydrogen peroxide added is 0.5vt%-1.5vt% of the dye to be degraded.
[0020] Preferably, the initial concentration of the dye to be degraded is 400 mg / L to 800 mg / L.
[0021] Preferably, the dye to be degraded is one or more of methyl orange, rhodamine B, azobenzene, and methylene blue.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The present invention provides a method for preparing a composite chromite catalyst. The prepared catalyst has a good degradation effect on organic pollutants in wastewater, and solves the problem of low catalytic activity and poor stability of traditional Fenton reaction catalysts. It not only realizes the high-value utilization of chromite ore, but also reduces the production cost of Fenton reaction catalysts, which has significant environmental benefits and economic value.
[0024] 2. After the composite chromite catalyst prepared by the present invention was recycled for 3 times, the removal rate of dye pollutants decreased from 96% to 92%, indicating that the composite chromite catalyst has good cyclic stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The graphs of degradation of dye pollutants by the composite chromite catalyst prepared in Example 3, no catalyst and traditional Fenton catalyst are shown;
[0026] Figure 2 This is a cycle stability test diagram of the composite chromite catalyst prepared in Example 3;
[0027] Figure 3 This is the SEM image of the composite chromite catalyst prepared in Example 3. DETAILED DESCRIPTION
[0028] The technical solutions in the present invention will be described clearly and completely below in conjunction with the specific implementation of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] The methods described in the embodiments of the present invention are conventional methods unless otherwise specified. The materials, reagents, etc. used can be obtained from commercial sources unless otherwise specified.
[0030] Example 1
[0031] A method for preparing a composite chromite catalyst for Fenton reaction comprises the following steps.
[0032] (1) Grind the natural chromite ore into powder and pass it through a 200-mesh sieve. Then add manganese dioxide and sodium carbonate, stir evenly with a mixer, calcine at 800°C for 5 hours to obtain a calcined product, grind the calcined product and pass it through a 100-mesh sieve for later use. The mass ratio of natural chromite ore, manganese dioxide and sodium carbonate is 5:2:10.
[0033] (2) Adding a 20% sodium hydroxide solution to the ground calcined product of (1), wherein the mass ratio of the ground calcined product to the sodium hydroxide solution is 1:20. Stirring at a speed of 1200 rpm for 8 hours, filtering and washing the solid with distilled water to obtain an alkalized product, drying the alkalized product and grinding it into powder, passing it through a 100-mesh sieve for later use;
[0034] (3) Add nickel nitrate to the ground alkalized product in (2), stir evenly, and then place in a muffle furnace for calcination at 500° C. for 4 hours. After cooling, add distilled water, wherein the mass ratio of the alkalized product, nickel nitrate and distilled water is 1:2:4. Stir and react for 2 hours, filter and dry, and the composite chromite catalyst is obtained.
[0035] The application of the composite chromite catalyst in the Fenton reaction is specifically as follows:
[0036] At 50° C., the composite chromite catalyst and hydrogen peroxide were added to the solution of the dye to be degraded, reacted for 50 minutes, and then the concentration of the dye to be degraded was measured. The dye to be degraded was methyl orange, and the initial concentration was 400 mg / L.
[0037] The added amount of the composite chromite catalyst is 0.1wt% of the dye to be degraded, and the added amount of hydrogen peroxide is 0.5vt% of the dye to be degraded.
[0038] Example 2
[0039] A method for preparing a composite chromite catalyst for Fenton reaction comprises the following steps.
[0040] (1) Grind the natural chromite ore into powder, pass through a 200-mesh sieve, then add manganese dioxide and potassium carbonate, stir evenly with a stirrer, calcine at 850°C for 6 hours to obtain a calcined product, grind the calcined product and pass through a 100-mesh sieve for later use. The mass ratio of the natural chromite ore, manganese dioxide and potassium carbonate is 5:2:10.
[0041] (2) Adding a 20% potassium hydroxide solution to the ground calcined product in (1), wherein the mass ratio of the ground calcined product to the potassium hydroxide solution is 1:20. Stirring at a speed of 1200 rpm for 8 hours, filtering and washing the solid with distilled water to obtain an alkalized product, drying the alkalized product and grinding it into powder, passing it through a 100-mesh sieve for later use.
[0042] (3) Add nickel nitrite to the ground alkalized product in (2), stir evenly, and then place in a muffle furnace for calcination at 600° C. for 4 hours. After cooling, add distilled water, wherein the mass ratio of the alkalized product, nickel nitrite and distilled water is 6:11:23. Stir and react for 2 hours, filter and dry, and the composite chromite catalyst is obtained.
[0043] The application of the composite chromite catalyst in the Fenton reaction is specifically as follows:
[0044] At 50° C., the composite chromite catalyst and hydrogen peroxide were added to the solution of the dye to be degraded, reacted for 50 minutes, and then the concentration of the dye to be degraded was measured. The dye to be degraded was methyl orange, and the initial concentration was 500 mg / L.
[0045] The added amount of the composite chromite catalyst is 0.1wt% of the dye to be degraded, and the added amount of hydrogen peroxide is 0.5vt% of the dye to be degraded.
[0046] Example 3
[0047] A method for preparing a composite chromite catalyst for Fenton reaction comprises the following steps.
[0048] (1) Grind the natural chromite ore into powder and pass it through a 200-mesh sieve. Add manganese dioxide and lithium carbonate, stir evenly with a stirrer, calcine at 900°C for 7 hours to obtain a calcined product, grind the calcined product and pass it through a 200-mesh sieve for later use. The mass ratio of natural chromite ore, manganese dioxide and lithium carbonate is 4:1:6.
[0049] (2) Adding a 25% aqueous ammonia solution to the ground calcined product in (1), wherein the mass ratio of the ground calcined product to the aqueous ammonia solution is 3:25. Stirring at a speed of 1200 rpm for 9 hours, filtering and washing the solid with distilled water to obtain an alkalized product, drying the alkalized product and grinding it into powder, passing it through a 200-mesh sieve for later use;
[0050] (3) Add nickel chloride to the ground alkalized product in (2), stir evenly, and then place in a muffle furnace for calcination at 700° C. for 5 h. After cooling, add distilled water, wherein the mass ratio of the alkalized product, nickel chloride and distilled water is 7:12:26. Stir and react for 3 h, filter and dry, and the composite chromite catalyst is obtained.
[0051] The application of the composite chromite catalyst in the Fenton reaction is specifically as follows:
[0052] At 50° C., the composite chromite catalyst and hydrogen peroxide were added to the solution of the dye to be degraded, reacted for 55 minutes, and then the concentration of the dye to be degraded was measured. The dye to be degraded was methyl orange, and the initial concentration was 600 mg / L.
[0053] The added amount of the composite chromite catalyst is 0.2wt% of the dye to be degraded, and the added amount of hydrogen peroxide is 1.0vt% of the dye to be degraded.
[0054] Example 4
[0055] A method for preparing a composite chromite catalyst for Fenton reaction comprises the following steps.
[0056] (1) Grind the natural chromite ore into powder and pass it through a 200-mesh sieve. Add manganese dioxide and calcium carbonate, stir evenly with a mixer, calcine at 950°C for 8 hours to obtain a calcined product, grind the calcined product and pass it through a 300-mesh sieve for later use. The mass ratio of natural chromite ore, manganese dioxide and calcium carbonate is 15:3:20.
[0057] (2) Adding a 30% lithium hydroxide solution to the ground calcined product in (1), wherein the mass ratio of the ground calcined product to the lithium hydroxide solution is 1:6. Stirring at a speed of 2000 rpm for 10 hours, filtering and washing the solid with distilled water to obtain an alkalized product, drying the alkalized product and grinding it into powder, passing it through a 300-mesh sieve for later use;
[0058] (3) Add nickel bromide to the ground alkalized product in (2), stir evenly, and then place in a muffle furnace for calcination at 800° C. for 6 hours. After cooling, add distilled water, wherein the mass ratio of the alkalized product, nickel bromide and distilled water is 8:13:29. Stir the reaction for 4 hours, filter and dry, and the composite chromite catalyst is obtained.
[0059] The application of the composite chromite catalyst in the Fenton reaction is specifically as follows:
[0060] At 50° C., the composite chromite catalyst and hydrogen peroxide were added to the solution of the dye to be degraded, reacted for 60 minutes, and then the concentration of the dye to be degraded was measured. The dye to be degraded was methyl orange, and the initial concentration was 700 mg / L.
[0061] The added amount of the composite chromite catalyst is 0.3wt% of the dye to be degraded, and the added amount of hydrogen peroxide is 1.5vt% of the dye to be degraded.
[0062] Example 5
[0063] A method for preparing a composite chromite catalyst for Fenton reaction comprises the following steps.
[0064] (1) Grind the natural chromite ore into powder and pass it through a 200-mesh sieve. Add manganese dioxide and barium carbonate, stir evenly with a mixer, calcine at 1000°C for 9 hours to obtain a calcined product, grind the calcined product and pass it through a 300-mesh sieve for later use. The mass ratio of natural chromite ore, manganese dioxide and barium carbonate is 15:3:20.
[0065] (2) Adding a 30% sodium hydroxide solution to the ground calcined product in (1), wherein the mass ratio of the ground calcined product to the sodium hydroxide solution is 1:6. Stirring at a speed of 2000 rpm for 10 hours, filtering and washing the solid with distilled water to obtain an alkalized product, drying the alkalized product and grinding it into powder, passing it through a 300-mesh sieve for later use;
[0066] (3) Add nickel sulfate to the ground alkalized product in (2), stir evenly, and then place in a muffle furnace for calcination at 800° C. for 6 hours. After cooling, add distilled water, wherein the mass ratio of the alkalized product, nickel sulfate and distilled water is 4:7:15. Stir the reaction for 4 hours, filter and dry, and obtain the composite chromite catalyst.
[0067] The application of the composite chromite catalyst in the Fenton reaction is specifically as follows:
[0068] At 50° C., the composite chromite catalyst and hydrogen peroxide were added to the solution of the dye to be degraded, reacted for 60 minutes, and then the concentration of the dye to be degraded was measured. The dye to be degraded was methyl orange, and the initial concentration was 800 mg / L.
[0069] The added amount of the composite chromite catalyst is 0.3wt% of the dye to be degraded, and the added amount of hydrogen peroxide is 1.5vt% of the dye to be degraded.
[0070] Comparative Example 1
[0071] Take methyl orange, a dye to be degraded, with an initial concentration of 600 mg / L for later use.
[0072] Comparative Example 2
[0073] The traditional Fenton catalyst uses analytically pure FeSO4 and a H2O2 system with a mass concentration of 30%. During the experiment, a calculated amount of FeSO4 and hydrogen peroxide are added according to the preset concentration and the reaction is continued for the set time.
[0074] Since the removal rates of methyl orange pollutants by the composite chromite catalysts prepared in Examples 1, 2, 4 and 5 are all between 94% and 97%, the composite chromite catalyst prepared in Example 3 is used as an example for comparison with Comparative Examples 1 and 2.
[0075] The application of the composite chromite catalyst in the Fenton reaction is specifically as follows: Figure 1 The graph is a graph of the degradation of methyl orange pollutants by the composite chromite catalyst prepared in Example 3 and the traditional Fenton catalyst, and the methyl orange pollutants without catalyst. The experimental conditions are: 50°C, 0.2wt% catalyst, 1vt% hydrogen peroxide, the catalysts are used to degrade dye pollutant wastewater, and the removal rate curve is recorded. The initial concentration of methyl orange is 600mg / L. As can be seen from the figure, in the absence of a catalyst, that is, in Comparative Example 1, the pollutant concentration hardly changes. Under the traditional Fenton catalytic conditions, that is, in Comparative Example 2, the pollutant removal rate reaches 88%, and the pollutant removal rate reaches 96% in the presence of the composite chromite catalyst prepared in Example 3.
[0076] Figure 2 The cyclic stability test of the composite chromite catalyst prepared in Example 3 showed that the removal rate of dye pollutants decreased from 96% to 92% after the catalyst was recycled three times at 50°C and 0.2wt% of the catalyst, indicating that the composite chromite catalyst had good cyclic stability.
[0077] Figure 3 This is a SEM image of the composite chromite catalyst prepared in Example 3. From a) in the figure, it can be seen that the composite chromite catalyst prepared is spherical, with a particle size of 50 nm and good uniformity. b) in the figure is an enlarged view of a).
[0078] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0079] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A method for preparing a composite chromite catalyst, characterized in that: The specific steps include: Calcine chromite ore, manganese dioxide and carbonate at 800°C to 1000°C for 5h to 9h to obtain a calcined product; the mass ratio of the chromite ore, manganese dioxide and carbonate is 5 to 15: 2 to 3: 10 to 20; The calcined product is reacted with an inorganic alkali solution for 8 hours to 10 hours, and the solid after filtration is an alkalized product; the mass ratio of the calcined product to the inorganic alkali solution is 1 to 5:20 to 30; The alkali compound and the nickel salt are calcined at 500°C to 800°C for 4h to 6h, water is added after cooling, and the reaction is carried out for 2h to 4h. The solid after filtration is the composite chromite catalyst; wherein the mass ratio of the alkali compound, the nickel salt and the water is 5-8:10-14:20-30.
2. The method for preparing a composite chromite catalyst according to claim 1, characterized in that: The carbonate is one or more of sodium carbonate, potassium carbonate, lithium carbonate, calcium carbonate, barium carbonate and magnesium carbonate.
3. The method for preparing a composite chromite catalyst according to claim 2, characterized in that: The inorganic alkali solution is one or more of sodium hydroxide solution, potassium hydroxide solution, ammonia solution and lithium hydroxide solution; the mass concentration of the inorganic alkali solution is 20% to 30%.
4. The method for preparing a composite chromite catalyst according to claim 3, characterized in that: The chromite is one or more of high-chromium chromite, high-iron chromite and high-aluminum chromite.
5. The method for preparing a composite chromite catalyst according to claim 4, characterized in that: The nickel salt is one or more of nickel nitrate, nickel nitrite, nickel chloride, nickel bromide and nickel sulfate.
6. The composite chromite catalyst prepared according to any one of the preparation methods of claims 1 to 5.
7. Use of the composite chromite catalyst according to claim 6 in degrading dyes.
8. The use according to claim 7, characterized in that: The specific application method is: at 10°C to 50°C, the composite chromite catalyst and hydrogen peroxide are added to the dye solution to be degraded, reacted for 50min to 60min, and the concentration of the dye solution to be degraded is measured; the amount of the composite chromite catalyst added is 0.1wt% to 0.3wt% of the dye to be degraded, and the amount of hydrogen peroxide added is 0.5vt% to 1.5vt% of the dye to be degraded.
9. The use according to claim 8, characterized in that: The initial concentration of the dye to be degraded is 400 mg / L to 800 mg / L.
10. The use according to claim 9, characterized in that: The dye to be degraded is one or more of methyl orange, rhodamine B, azobenzene and methylene blue.
Citation Information
Patent Citations
Chromium-doped magnetite hetero-phase Fenton catalyst and preparation method for same
CN106944076A
Method for oxidizing roasting conversion of chrome mineral
CN110171849A
Calcium-free roasting chromium slag, resource application and preparation method
CN117263357A
Macroporous pseudo-boehmite and preparation method thereof
CN118255375A