Preparation method and application of catalyst for preparing acetaldehyde through direct dehydrogenation of ethanol
By using nitrogen-doped carbon support and copper source to prepare Cu/Si@NC catalysts in the direct dehydrogenation method of ethanol, the problems of catalyst stability and high production costs in the prior art are solved, and efficient ethanol conversion and acetaldehyde are achieved Selectivity reduces the occurrence of side reactions.
Patent Information
- Application Number
- CN202411061139.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The existing catalysts with direct ethanol dehydrogenation method have high energy consumption, many by-products, high production costs and poor catalyst stability. Especially in the preparation of copper-based catalysts, the ammonia distillation method leads to a decrease in copper load and poor activity. .
Different organic amines are used as nitrogen sources, and nitrogen-doped carbon support is prepared by hydroxymethylation reaction with formaldehyde, combined with silicon sol and copper sources, and Cu is supported by ammonia distillation method to form Cu/Si@NC catalyst to improve the catalyst Activity, selectivity and stability.
A catalyst with high activity, high selectivity and high stability is achieved, which reduces production costs, improves ethanol conversion and acetaldehyde selectivity, reduces the occurrence of side reactions, and maintains stability during long-term use.
Smart Images

Figure CN118976527A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalyst preparation, and particularly relates to a method for preparing a Cu / Si@NC catalyst for direct dehydrogenation of ethanol. Background Art
[0002] As an important organic chemical, acetaldehyde is an important intermediate for the synthesis of medicines and food additives. It has extremely high industrial application value. The downstream products of acetaldehyde include acetate, sorbic acid, pyridine compounds, crotonaldehyde, etc., which are widely used in the chemical industry. With the development of the chemical industry, my country is currently the world's largest consumer of acetaldehyde. The traditional methods for the synthesis of acetaldehyde mainly include ethylene oxidation, acetylene hydration, acetic acid reduction and ethane oxidation. The traditional methods for the synthesis of acetaldehyde have the disadvantages of high energy consumption and many by-products. With the development of science and technology, ethanol dehydrogenation has received more and more attention. Ethanol dehydrogenation methods include oxidative dehydrogenation and direct dehydrogenation. Ethanol oxidative dehydrogenation is an exothermic reaction. Therefore, direct oxidative dehydrogenation in industry needs to be carried out under high temperature conditions, which consumes a lot of energy. At the same time, water will be produced during the reaction, which makes it difficult to separate and purify acetaldehyde and increases production costs. The by-products of the reaction, such as formic acid and acetic acid, will cause serious corrosion problems during the condensation and recovery of the products. The direct dehydrogenation of ethanol to synthesize acetaldehyde can effectively reduce energy consumption in the production process, and the product H2 is a clean renewable energy. Therefore, ethanol can not only be used to synthesize widely used acetaldehyde but also can be used as an effective carrier for hydrogen storage.
[0003] At present, direct dehydrogenation of ethanol can be divided into homogeneous catalysis and heterogeneous catalysis. Although homogeneous catalysis has been proven to have excellent catalytic performance, its dependence on precious metals and the high cost of ligands limit its large-scale practical application. Compared with homogeneous catalysis, heterogeneous catalysts are easier to recycle and can exhibit better catalytic performance. Non-precious metal-supported Cu-based catalysts show excellent catalytic activity in heterogeneous catalysis, with high ethanol conversion rate and high acetaldehyde selectivity.
[0004] Designing and developing highly active, highly selective and highly stable non-precious metal catalysts has become a problem for this reaction. However, copper-based catalysts have been widely studied in ethanol dehydrogenation reactions and have been proven to be the catalysts with the greatest commercial potential. CN116060098A discloses a Cu-based MFI molecular sieve single-atom catalyst prepared by an ammonia evaporation method and an acid treatment strategy. The ammonia evaporation method can change the pore structure of the molecular sieve, improve the anchoring effect of copper and the molecular sieve, and help to improve the stability of the catalyst. However, the acid treatment will significantly reduce the copper loading. Although the single-atom dispersion of copper is achieved, the overall activity of the catalyst is greatly reduced. CN117225423A discloses a catalyst for ethanol dehydrogenation to acetaldehyde, using silicon dioxide as a carrier, copper as an active component, nickel and zinc as additives, and realizing the loading of three metals by an ammonia evaporation method and a post-impregnation method. The catalyst preparation process is cumbersome, which greatly increases the production cost of the catalyst. Through research, this patent found that carbon carriers play an important role in enriching ethanol. At the same time, using nitrogen-doped carbon materials as carriers is beneficial to promoting the desorption of acetaldehyde, thereby reducing the side reactions of acetaldehyde and improving acetaldehyde selectivity. Summary of the invention
[0005] The object of the present invention is to provide a preparation method and application of a catalyst for ethanol dehydrogenation to acetaldehyde in view of the limitations of the current technology. The method uses different organic amines as nitrogen sources, and then achieves nitrogen doping by reacting with formaldehyde (formalin) for hydroxymethylation. The catalyst obtained by the present invention has the characteristics of uniform dispersion of active centers, high catalyst activity, not easy to deactivate, high mechanical strength, high thermal stability, etc. In the direct dehydrogenation of ethanol to acetaldehyde reaction, the catalyst has the advantages of high activity, high selectivity and high stability.
[0006] To achieve the above object, the technical solution of the present invention is as follows:
[0007] A method for preparing a catalyst for direct dehydrogenation of ethanol to produce acetaldehyde, the method comprising the following steps:
[0008] (1) weighing anhydrous sodium carbonate, resorcinol and formalin, placing them in deionized water, and dissolving them by ultrasonication to obtain solution A, wherein the mass ratio of anhydrous sodium carbonate, resorcinol, formalin and water is 0.1 to 1:10 to 100:10 to 50:30;
[0009] (2) Weighing organic amine and formalin, putting them into deionized water, and dissolving them by ultrasonication to obtain solution B.
[0010] Wherein, the mass ratio of organic amine to formalin is 1:2-5;
[0011] The organic amine is one or more of aniline, diphenylamine, phenylenediamine, melamine, ethylenediamine and urea;
[0012] The mass concentration range of formaldehyde in the formalin in steps (1) and (2) is 35-40%.
[0013] (3) adding solution A and solution B to the silica sol within 3-30 minutes under stirring to obtain a mixture C;
[0014] Wherein, 10 to 50 mL of solution A and 10 to 50 mL of solution B are added to every 50 to 150 mL of silica sol;
[0015] The concentration of the silica sol is 30wt%; the particle size of the silicon dioxide is 8-15nm.
[0016] (4) Heat the mixture C in a sealed water bath at 35-55° C. for 3-8 h to solidify the mixture, thereby obtaining a solid D;
[0017] (5) Drying and grinding solid D, and then calcining in an inert atmosphere at 600-1000° C. for 1-8 h to obtain solid E;
[0018] (6) placing solid E in a sodium hydroxide solution, heating in a water bath at 40 to 70° C. with stirring for 1 to 5 hours, and filtering, washing, and vacuum drying to obtain carrier F;
[0019] Wherein, the mass ratio of solid E to sodium hydroxide is 1-10:5-20;
[0020] The concentration of sodium hydroxide solution is 0.1-4 mol / L.
[0021] (7) Weigh a copper source, water, and aqueous ammonia into a container, seal it, and stir at room temperature to dissolve all the solids to obtain a solution G;
[0022] The mass ratio of the copper element, water and ammonia contained in the copper source is 0.01-0.5:100:50;
[0023] The concentration of the ammonia water is 20-30wt%;
[0024] (8) Add carrier F to solution G, stir for 4 to 10 hours, then heat to 60 to 80° C., evaporate ammonia while the liquid level remains essentially constant until the pH of the solution is 7-9, and then filter, wash, vacuum dry, and calcine to obtain the desired catalyst;
[0025] Wherein, 0.5-4 g of carrier F is added to every 200 mL of solution G;
[0026] In step (5), the drying temperature is 80-12° C. and the drying time is 42-96 hours.
[0027] In step (5), the inert atmosphere is one of nitrogen, argon, and a nitrogen-argon mixture.
[0028] In step (6), the vacuum drying temperature is 60 to 90° C., and the vacuum drying time is 4 to 12 hours.
[0029] In step (7), the copper source is one or more of copper nitrate trihydrate, copper sulfate and copper chloride.
[0030] In step (8), the vacuum drying temperature is 60 to 90° C., and the vacuum drying time is 4 to 12 hours.
[0031] In step (8), the calcination atmosphere is argon, the calcination temperature is 250-500° C., and the calcination time is 1-5 hours.
[0032] The catalyst of the preparation method is used for direct dehydrogenation reaction of ethanol.
[0033] The specific steps include:
[0034] (1) introducing the reaction gas into a fixed bed reactor filled with a catalyst after the N2 gas is evacuated, reacting at normal pressure and 240-350° C. to obtain the catalytic performance of direct dehydrogenation of ethanol to acetaldehyde;
[0035] The reaction gas is a mixture of ethanol and nitrogen, with ethanol accounting for 2-20% by volume of the reaction gas; the air velocity is 0.5-3h -1 .
[0036] The essential features of the present invention are:
[0037] The core innovation of the present invention lies in the research discovery that the nitrogen-doped carbon carrier prepared by using different nitrogen sources has the function of enriching ethanol and promoting the desorption of acetaldehyde, thereby improving the activity of the catalyst, reducing the side reactions of acetaldehyde, and improving the acetaldehyde selectivity and catalyst stability.
[0038] In the current technology, copper is loaded on a silicon-carbon composite material as a catalyst by using an ammonia evaporation method, and active metal copper is introduced by the ammonia evaporation method to obtain a catalyst with fatty acid ester hydrogenation performance;
[0039] The present invention utilizes the principle of hydroxymethylation reaction, adopts different organic amines as nitrogen sources, reacts with formaldehyde to achieve nitrogen doping, and the obtained nitrogen-doped carbon carrier has the function of enriching ethanol and promoting the desorption of acetaldehyde, which is beneficial to reduce the side reaction of acetaldehyde, improve acetaldehyde selectivity and catalyst stability, and then applies for a patent for the preparation method of the catalyst for direct dehydrogenation of ethanol to acetaldehyde.
[0040] The beneficial effects of the present invention are:
[0041] (1) Using the hard template method, SiO2 is used as the hard template agent, phenolic resin is used as the carbon precursor, and organic amine is used as the nitrogen source. After carbonization and removal of part of the template agent, a mesoporous silicon-coated nitrogen-carbon composite material can be obtained. The preparation method is simple and low-cost. The pore size of the obtained catalyst is controllable and mainly distributed in the mesoporous range, which can fully realize the internal and external diffusion and adsorption and desorption of each reactant and product in the ethanol dehydrogenation reaction. -1 At an air velocity of 300°C, an ethanol conversion rate of 90.5% and an acetaldehyde selectivity of 92% were achieved, which remained basically stable after 600 hours of reaction.
[0042] (2) The phenolic resin with mature preparation technology is used as the carbon precursor, the organic amine is used as the nitrogen source, and the silica sol is used as the hard template. The synthesis method has the advantages of abundant raw materials, simple preparation process, adjustable material structure, high repeatability, and easy large-scale preparation, and has broad industrial application prospects.
[0043] (3) Mesoporous silicon-coated nitrogen-carbon composite materials have an enrichment effect on ethanol. At the same time, the low-temperature desorption barrier of acetaldehyde is low (300oC). After acetaldehyde is generated, it can quickly leave the catalyst surface, reducing the occurrence of side reactions and improving acetaldehyde selectivity. Compared with the undoped nitrogen catalyst, the nitrogen-doped catalyst has a higher ethanol concentration than the undoped nitrogen catalyst in 1.5h. -1 At 300℃, the ethanol conversion rate increased by nearly 30% and the acetaldehyde selectivity increased by nearly 20%.
[0044] (4) The ammonia evaporation method is used to load Cu on the silicon-coated nitrogen-carbon composite material. The copper dispersion is more uniform and the particle size is smaller. The active material has a stronger interaction with the carrier and is not easily deactivated due to aggregation of active centers during the catalytic reaction. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 The pore size distribution diagram of the catalysts prepared in Examples 1, 7, 10 and Comparative Example 1.
[0046] Figure 2 This is a graph showing the changes in conversion rate and selectivity of ethanol dehydrogenation reaction in a fixed bed reactor using the catalyst prepared in Example 1.
[0047] Figure 3 This is the SEM image of the catalyst prepared in Example 1. DETAILED DESCRIPTION
[0048] The present invention will be further explained below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the following specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.
[0049] Example 1
[0050] The preparation steps of mesoporous Cu / Si@NC catalyst for ethanol dehydrogenation are as follows:
[0051] (1) Weigh 0.15 g of anhydrous sodium carbonate, 10 g of resorcinol and 10 g of formalin (concentration: 37%), put them into 6 g of deionized water, and sonicate until they are completely dissolved to obtain solution A.
[0052] (2) Weigh 5 g of melamine and 10 g of formalin, put them into deionized water, and dissolve them by ultrasonication to obtain solution B.
[0053] (3) 90 mL of silica sol (SiO2 mass concentration of 30 wt%, silica particle size of 8-15 nm) was measured and placed in a beaker. Solution A and solution B were slowly added dropwise at a rate of 5 mL / min during stirring to obtain a mixture C.
[0054] (4) Seal the beaker with plastic wrap and solidify mixture C in a 38°C water bath for 4 h to obtain solid D.
[0055] (5) The solid D was crushed with a spatula and dried at 80°C for 36 h. The solid was ground to a particle size of ≤200 mesh and carbonized at 800°C for 2 h under an argon atmosphere to obtain a solid E.
[0056] (6) Weigh 600 mL of water, 6.74 g of sodium hydroxide (0.17 mol) and 5.73 g of solid carrier E into a beaker, heat in a 50°C water bath with stirring for 2 h, filter out the solid, wash with deionized water until the filtrate is neutral, and dry in a vacuum at 80°C for 8 h to obtain carrier F.
[0057] (7) Weigh 0.81 g of copper nitrate trihydrate (containing 0.22 g of copper element), 100 mL of deionized water, and 50 mL of aqueous ammonia (concentration 25-28 wt%) into a flask, seal and stir in a 38°C water bath for 30 min to obtain solution G.
[0058] (8) Add 1 g of carrier F to solution G, stir for 6 h, then heat to 80 °C and start to evaporate ammonia. Use a pen to mark the liquid level on the outside of the three-necked flask, and keep the liquid level in the flask unchanged while evaporating ammonia until the pH of the solution is 7. Filter to obtain a solid, wash with deionized water until the pH of the filtrate is 7, vacuum dry the filter cake at 80 °C for 8 h, and calcine at 350 °C for 2 h under argon atmosphere to obtain the desired catalyst, which is denoted as Cu / Si@NC-1.
[0059] The evaluation process and conditions of the catalyst are:
[0060] (1) The catalysts Cu / Si@NC-1~15 and Cu / Si@C-16 prepared by the above method were respectively loaded into a fixed bed reactor with an inner diameter of 8 mm, and N2 gas was continuously introduced for 4 h to exhaust the impurity gas in the system.
[0061] (2) 10v% ethanol gas was introduced at an air velocity of 1.5h -1 , the carrier gas is nitrogen, the total flow rate of the mixed gas is 98 mL / min, the reaction temperature is 300°C, and the reaction is carried out under normal pressure.
[0062] (3) After the reaction is stable, the reaction raw materials and products are analyzed using online chromatography.
[0063] Product analysis method:
[0064] The product composition is mainly ethanol, acetaldehyde, ether, acetic acid, ethylene, ethyl formate, and ethyl acetate. The product was analyzed online using Anhui GC5190E chromatographic system, with FID and TCD detectors configured. The product analysis was performed using the internal standard method, with ethanol as the internal standard, and the relative molar correction factor of each component relative to ethanol was calculated according to formula 1.
[0065] Formula 1: f2 / f1 = (A1m2M1) / (A2m1M2); where f1 is the molar correction factor of ethanol, set to 1; f2 is the molar correction factor of the substance to be determined; A1 is the peak area of ethanol; A2 is the peak area of the substance to be determined; m1 is the mass of ethanol; m2 is the mass of the substance to be determined; M1 is the molecular weight of ethanol; M2 is the molecular weight of the substance to be determined. Thus, the corresponding conversion rate and selectivity can be calculated.
[0066] The evaluation effect of the catalyst prepared in Example 1 in the ethanol dehydrogenation reaction is as follows Figure 1 As shown, the products of the catalytic reaction fluctuate in the early stage of catalysis, but they quickly stabilize. During the 600-hour activity and stability evaluation process, the conversion rate of ethanol stabilized at more than 90%, and the selectivity of the main product acetaldehyde could reach more than 92.5%, and it could be stable for a long time; the by-products of the catalytic reaction mainly included ethylene, ether, ethyl formate, ethyl acetate and acetic acid, and the selectivity of the by-products was basically below 3%. After 600 hours of activity evaluation, there was no obvious deactivation of the catalyst, and the stability and activity of the catalytic reaction could be stable for a long time. The catalyst has a high industrial application value.
[0067] Example 2
[0068] The preparation steps of mesoporous Cu / Si@NC catalyst for ethanol dehydrogenation are as follows:
[0069] The other conditions were the same as those in Example 1, except that the amount of anhydrous sodium carbonate added in step (1) was changed to 0.24 g. The obtained catalyst was recorded as Cu / Si@NC-2.
[0070] Example 3
[0071] The preparation steps of mesoporous Cu / Si@NC catalyst for ethanol dehydrogenation are as follows:
[0072] The other conditions were the same as those in Example 1, except that the type of organic amine in step (2) was changed: melamine was replaced by aniline, and the obtained catalyst was recorded as Cu / Si@NC-3.
[0073] Example 4
[0074] The preparation steps of mesoporous Cu / Si@NC catalyst for ethanol dehydrogenation are as follows:
[0075] The other conditions were the same as those in Example 1, except that the dropping speeds of solution A and solution B in step (3) were changed to 20 mL / min. The obtained catalyst was recorded as Cu / Si@NC-4.
[0076] Example 5
[0077] The preparation steps of mesoporous Cu / Si@NC catalyst for ethanol dehydrogenation are as follows:
[0078] The other conditions were the same as those in Example 1, except that the water bath temperature in step (4) was changed to 55° C. The obtained catalyst was denoted as Cu / Si@NC-5.
[0079] Example 6
[0080] The preparation steps of mesoporous Cu / Si@NC catalyst for ethanol dehydrogenation are as follows:
[0081] The other conditions were the same as those in Example 1, except that the calcination procedure in step (5) was changed: calcination at 600° C. for 4 h under a nitrogen atmosphere. The obtained catalyst was denoted as Cu / Si@NC-6.
[0082] Example 7
[0083] The preparation steps of mesoporous Cu / Si@NC catalyst for ethanol dehydrogenation are as follows:
[0084] The other conditions were the same as those in Example 1, except that the amount of sodium hydroxide added in step (6) was changed to 8.26 g. The obtained catalyst was recorded as Cu / Si@NC-7.
[0085] Example 8
[0086] The preparation steps of mesoporous Cu / Si@NC catalyst for ethanol dehydrogenation are as follows:
[0087] The other conditions were the same as those in Example 1, except that the water bath conditions in step (6) were changed: heating in a water bath at 70° C. with stirring for 5 h. The obtained catalyst was recorded as Cu / Si@NC-8.
[0088] Example 9
[0089] The preparation steps of mesoporous Cu / Si@NC catalyst for ethanol dehydrogenation are as follows:
[0090] The other conditions were the same as those in Example 1, except that the copper source in step (7) was changed from copper nitrate trihydrate to copper sulfate. The obtained catalyst was denoted as Cu / Si@NC-9.
[0091] Example 10
[0092] The preparation steps of mesoporous Cu / Si@NC catalyst for ethanol dehydrogenation are as follows:
[0093] The other conditions were the same as those in Example 1, except that the amount of copper nitrate trihydrate added in step (7) was changed to 3.26 g of copper nitrate trihydrate ammonia water. The resulting catalyst was recorded as Cu / Si@NC-10.
[0094] Embodiment 11
[0095] The preparation steps of mesoporous Cu / Si@NC catalyst for ethanol dehydrogenation are as follows:
[0096] The other conditions were the same as those in Example 1, except that the amount of the carrier added in step (8) was changed: 1.5 g of the carrier was added, and the obtained catalyst was recorded as Cu / Si@NC-11.
[0097] Example 12
[0098] The preparation steps of mesoporous Cu / Si@NC catalyst for ethanol dehydrogenation are as follows:
[0099] The other conditions were the same as those in Example 1, except that the temperature of the water bath for evaporating ammonia in step (8) was changed to 60° C. The obtained catalyst was denoted as Cu / Si@NC-12.
[0100] Embodiment 13
[0101] The preparation steps of mesoporous Cu / Si@NC catalyst for ethanol dehydrogenation are as follows:
[0102] The other conditions were the same as those in Example 1, except that the calcination procedure in step (8) was changed to calcine at 500° C. for 3 h. The obtained catalyst was denoted as Cu / Si@NC-13.
[0103] Comparative Example 1
[0104] The Cu / Si@NC catalyst was prepared by the equal volume impregnation method. The specific preparation steps are as follows:
[0105] (1) The preparation steps of Si@NC carrier are the same as steps (1) to (7) in Example 1.
[0106] (2) Dissolve 1.63 g of copper nitrate trihydrate in deionized water and stir for 30 minutes to obtain an impregnation solution.
[0107] (3) The impregnation solution was added dropwise onto the carrier Si@NC, dried at room temperature for 4 h, and then vacuum dried at 80 °C for 8 h. The catalyst was calcined at 350 °C for 2 h under an argon atmosphere to obtain the desired catalyst, which was designated as Cu / Si@NC-14.
[0108] Comparative Example 2
[0109] The purpose is to compare with Example 1 to illustrate the effect of the sodium hydroxide silicon dissolution step on the catalytic activity.
[0110] The preparation steps of mesoporous Cu / Si@NC catalyst are as follows:
[0111] (1) Weigh 0.12 g of anhydrous sodium carbonate, 9 g of resorcinol, and 13.27 g of formalin, put them into 3.68 g of deionized water, and sonicate until they are completely dissolved to obtain solution A.
[0112] (2) Weigh 5 g of melamine and 10 g of formalin, put them into deionized water, and dissolve them by ultrasonication to obtain solution B.
[0113] (3) 90 ml of silica sol was measured and placed in a beaker. Solution A and solution B were slowly added dropwise at a rate of 5 mL / min during stirring to obtain a mixture C.
[0114] (3) Seal the mouth of the beaker with plastic wrap, and solidify the mixture C in a 38°C water bath for 4 h to obtain solid D.
[0115] (4) The solid D was crushed with a spatula and dried at 80°C for 36 h. The solid was ground to a particle size of ≤200 mesh and carbonized at 800°C for 2 h under an argon atmosphere to obtain a solid E.
[0116] (5) Weigh 1.63 g of copper nitrate trihydrate, 100 mL of deionized water, and 50 mL of aqueous ammonia into a flask, seal and stir in a 38°C water bath for 30 min to obtain solution F.
[0117] (6) Add 1 g of carrier E to solution F, stir for 6 h, then heat to 80 °C and start to evaporate ammonia. Use a pen to mark the liquid level on the outside of the three-necked flask, and keep the liquid level in the flask unchanged while evaporating ammonia until the pH of the solution is 7. Filter to obtain a solid, wash with deionized water until the pH of the filtrate is 7, vacuum dry the filter cake at 80 °C for 8 h, and calcine at 350 °C for 2 h under argon atmosphere to obtain the desired catalyst, which is recorded as Cu / Si@NC-15.
[0118] Comparative Example 3
[0119] The purpose is to compare with Example 1 to illustrate the effect of N doping on catalytic activity.
[0120] (1) Weigh 0.15 g of anhydrous sodium carbonate, 10 g of resorcinol, and 15.38 g of formalin, put them into 5.87 g of deionized water, and sonicate until they are completely dissolved to obtain solution A.
[0121] (2) 90 ml of silica sol was measured and placed in a beaker. Solution A was slowly added dropwise at a rate of 5 mL / min during stirring to obtain a mixture B.
[0122] (3) Seal the beaker with plastic wrap and solidify mixture B in a 38°C water bath for 4 h to obtain solid C.
[0123] (4) The solid C was crushed with a spatula and dried at 80°C for 36 h. The solid was ground to a particle size of ≤200 mesh and carbonized at 800°C for 2 h under an argon atmosphere to obtain a solid D.
[0124] (5) Weigh 600 mL of water, 6.74 g of sodium hydroxide and 5.73 g of solid carrier D into a beaker, heat in a 50°C water bath with stirring for 2 h, filter out the solid, wash with deionized water until the filtrate is neutral, and dry in a vacuum at 80°C for 8 h to obtain carrier E.
[0125] (6) Weigh 0.81 g of copper nitrate trihydrate, 100 mL of deionized water, and 50 mL of aqueous ammonia into a flask, seal and stir in a 38°C water bath for 30 min to obtain solution F.
[0126] (7) Add 1 g of carrier E to solution F, stir for 6 h, then heat to 80 °C and start to evaporate ammonia. Use a pen to mark the liquid level on the outside of the three-necked flask. Keep the liquid level in the flask unchanged and evaporate ammonia until the pH of the solution is 7. Filter to obtain a solid, wash with deionized water until the pH of the filtrate is 7, vacuum dry the filter cake at 80 °C for 8 h, and calcine at 350 °C for 2 h in an argon atmosphere to obtain the desired catalyst, which is denoted as Cu / Si@C-16.
[0127] The reaction performances of the catalysts prepared in Examples 1 to 13 and Comparative Examples 1 to 3 are shown in Table 1, and the data results are all stable results after 50 hours of reaction.
[0128] Table 1
[0129] catalyst X(ethanol) / % S(acetaldehyde) / % catalyst X(ethanol) / % S(acetaldehyde) / % Cu / Si@NC-1 90.5 92.2 Cu / Si@NC-9 63.4 73.2 Cu / Si@NC-2 87.6 89.4 Cu / Si@NC-10 88.4 90.5 Cu / Si@NC-3 84.3 94.6 Cu / Si@NC-11 76.8 91.5 Cu / Si@NC-4 85.4 90.4 Cu / Si@NC-12 65.2 88.3 Cu / Si@NC-5 78.6 91.5 Cu / Si@NC-13 56.4 76.8 Cu / Si@NC-6 75.2 82.4 Cu / Si@NC-14 25.8 85.6 Cu / Si@NC-7 75.3 87.2 Cu / Si@NC-15 68.4 87.6 Cu / Si@NC-8 86.5 90.3 Cu / Si@C-16 61.2 72.3
[0130] The pore size distribution diagrams of the catalysts prepared in Examples 1, 7, 10 and Comparative Example 1 are as follows: Figure 1As shown, the catalytic pore size prepared in Example 1 is mainly distributed in the mesoporous range of 11 to 30 nm; in Example 7, due to the increase in the amount of sodium hydroxide added, the amount of dissolved silicon increased, causing some pores in the catalyst to become macropores, and the pore size is mainly distributed in 12 to 70 nm; in Example 10, due to the increase in the amount of Cu added, some pores were blocked by Cu, causing the pores of the catalyst to become smaller, but the pore size of the catalyst was still in the mesoporous range, and the pore size was mainly distributed in 6 to 15 nm; in Comparative Example 1, Cu was loaded by impregnation method, and Cu was more likely to form large particles, so the pore size of the catalyst was reduced more, and the pore size was mainly distributed in 2 to 9 nm. Comparative Example 2 is mainly because the template agent is not removed for loading, and the catalyst cannot produce suitable pores, thereby affecting the reaction activity and selectivity; Comparative Example 3 is mainly because the catalyst carrier is not doped with nitrogen for preparation, thereby reducing the amount of ethanol adsorption and the amount of acetaldehyde desorption at low temperature (less than 300°C), thereby reducing the catalyst activity and selectivity.
[0131] It should be noted that the above content only illustrates the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications all fall within the protection scope of the claims of the present invention.
[0132] Matters not covered by the present invention are known technologies.
Claims
1. A method for preparing a catalyst for direct dehydrogenation of ethanol to acetaldehyde, characterized in that the method comprises the following steps: (1) Weigh anhydrous sodium carbonate, resorcinol and formalin, put them into deionized water, and dissolve them by ultrasonication to obtain solution A. in, The mass ratio of anhydrous sodium carbonate, resorcinol, formalin and water is 0.1-1:10-100:10-50:30; (2) Weighing organic amine and formalin, putting them into deionized water, and dissolving them by ultrasonication to obtain solution B. Wherein, the mass ratio of organic amine to formalin is 1:2-5; The organic amine is one or more of aniline, diphenylamine, phenylenediamine, melamine, ethylenediamine and urea; (3) adding solution A and solution B to the silica sol within 3-30 minutes under stirring to obtain a mixture C; Wherein, 10 to 50 mL of solution A and 10 to 50 mL of solution B are added to every 50 to 150 mL of silica sol; (4) Heat the mixture C in a sealed water bath at 35-55° C. for 3-8 h to solidify the mixture, thereby obtaining a solid D; (5) Drying and grinding solid D, and then calcining in an inert atmosphere at 600-1000° C. for 1-8 h to obtain solid E; (6) placing solid E in a sodium hydroxide solution, heating in a water bath at 40 to 70° C. with stirring for 1 to 5 hours, and filtering, washing, and vacuum drying to obtain carrier F; Wherein, the mass ratio of solid E to sodium hydroxide is 1-10:5-20; (7) Weigh a copper source, water, and aqueous ammonia into a container, seal it, and stir at room temperature to dissolve all the solids to obtain a solution G; The mass ratio of the copper element, water and ammonia contained in the copper source is 0.01-0.5:100:50; (8) Add carrier F to solution G, stir for 4 to 10 hours, then heat to 60 to 80° C., evaporate ammonia while the liquid level remains essentially constant until the pH of the solution is 7-9, and then filter, wash, vacuum dry, and calcine to obtain the desired catalyst; Wherein, 0.5 to 4 g of carrier F is added to every 200 mL of solution G.
2. The method for preparing a catalyst for direct dehydrogenation of ethanol to acetaldehyde as claimed in claim 1, characterized in that The mass concentration range of formaldehyde in the formalin in steps (1) and (2) is 35-40%, the concentration of the silica sol described in step (3) is 30wt%, and the particle size of the silicon dioxide is 8-15nm.
3. The method for preparing a catalyst for direct dehydrogenation of ethanol to acetaldehyde as claimed in claim 1, wherein the step (5), the drying temperature is 80-12°C, and the drying time is 42-96h.
4. The method for preparing a catalyst for direct dehydrogenation of ethanol to acetaldehyde as claimed in claim 1, wherein the step In (5), the inert atmosphere is one of nitrogen, argon, and a nitrogen-argon mixed gas.
5. The method for preparing a catalyst for direct dehydrogenation of ethanol to acetaldehyde as claimed in claim 1, wherein the step (6), the vacuum drying temperature is 60-90° C., the vacuum drying time is 4-12 h, and the concentration of the sodium hydroxide solution is 0.1-4 mol / L.
6. The method for preparing a catalyst for direct dehydrogenation of ethanol to acetaldehyde as claimed in claim 1, wherein the step (7), the copper source is one or more of copper nitrate trihydrate, copper sulfate and copper chloride; the concentration of the ammonia water is 20-30wt%.
7. The method for preparing a catalyst for direct dehydrogenation of ethanol to acetaldehyde as claimed in claim 1, wherein in step (8), the vacuum drying temperature is 60-90° C., and the vacuum drying time is 4-12 hours; the calcination atmosphere is argon, the calcination temperature is 250-500° C., and the calcination time is 1-5 hours.
8. The use of the catalyst prepared by the preparation method as claimed in claim 1, characterized in that it is used for direct dehydrogenation of ethanol.
9. The use according to claim 8, comprising the following steps: (1) introducing the reaction gas into a fixed bed reactor filled with a catalyst after the N2 gas is evacuated, reacting at normal pressure and 240-350° C. to obtain the catalytic performance of direct dehydrogenation of ethanol to acetaldehyde; The reaction gas is a mixture of ethanol and nitrogen, with ethanol accounting for 2-20% by volume of the reaction gas; the air velocity is 0.5-3h -1 .
Citation Information
Patent Citations
Catalyst for preparing acetaldehyde through direct dehydrogenation of ethyl alcohol as well as preparation method and application thereof
CN106673977A
Meso-porous nitrogen-doped carbon material, and preparation method and use thereof
CN109879265A
Preparation method and application of catalyst for preparing acetaldehyde through ethanol dehydrogenation
CN114054079A
Cu-based organic hybrid material, preparation method thereof and application of Cu-based organic hybrid material in catalytic preparation of acetaldehyde
CN117380275A
Nitrogen-doped carbon carrier platinum-carbon catalyst material, preparation method thereof and application of nitrogen-doped carbon carrier platinum-carbon catalyst material in hydrogen fuel cell
CN118136868A
Cited By
Monatomic catalyst as well as preparation method and application thereof
CN119588430A