Magnesium borophosphate modified pure magnesium coating as well as preparation method and application thereof

By preparing a magnesium borophosphate modified coating on the surface of a magnesium matrix, the problems of rapid degradation and tissue inflammation of magnesium-based metals in the treatment of infectious bone defects were solved, and the corrosion resistance and antibacterial properties were improved, thus promoting osseointegration.

CN118976685APending Publication Date: 2024-11-19深圳市龙华区中心医院
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411050794.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Magnesium-based biomaterials rapidly degrade during the treatment of infected bone defects, leading to decreased corrosion resistance and osteogenic activity. Degradation products cause tissue inflammation and fail to effectively promote bone integration.

Method used

A magnesium borate phosphate modified coating was prepared on the surface of a pure magnesium matrix. A double-layer structure coating, consisting of an inner layer of magnesium hydroxide and an outer layer of magnesium borate phosphate, was generated by a hydrothermal method. The borate and phosphate ions were used to enhance osteogenic activity and form borate ester bonds with the bacterial cell wall to capture bacteria.

Benefits of technology

It improved the corrosion resistance and cell compatibility of the magnesium matrix, significantly enhanced antibacterial properties, reduced the degradation rate, and promoted osseointegration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004974855970000011
    Figure HDA0004974855970000011
  • Figure HDA0004974855970000012
    Figure HDA0004974855970000012
  • Figure HDA0004974855970000013
    Figure HDA0004974855970000013
Patent Text Reader

Abstract

The invention provides a magnesium borophosphate modified pure magnesium coating as well as a preparation method and application thereof, and belongs to the technical field of biomedical magnesium-based metal coatings. The preparation method of the magnesium borophosphate modified pure magnesium coating comprises the following steps: preparing a hydrothermal solution, namely preparing potassium phosphate, boric acid and water into the hydrothermal solution; and a hydrothermal reaction step: carrying out a hydrothermal reaction on the pure magnesium matrix and the hydrothermal solution at 150-180 DEG C for 1.5-6 hours to obtain the magnesium borophosphate modified pure magnesium coating. The preparation method has the beneficial effects that the coating with good corrosion resistance, cytocompatibility and antibacterial performance can be prepared, the cost is relatively low, and the process is simple.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biomedical magnesium-based metal coatings, and in particular to a method for preparing a magnesium borophosphate modified pure magnesium coating, and also to a magnesium borophosphate modified pure magnesium coating prepared by the method for preparing the magnesium borophosphate modified pure magnesium coating and applications thereof. Background Art

[0002] Infected bone defects have always been a key disease in clinical orthopedic treatment. This disease is different from general bone defects. Due to the presence and spread of infection, local inflammation destroys the osteogenic microenvironment, hinders bone tissue healing, and continuously expands the scope of bone defects. Therefore, it is difficult to treat, the lesions are difficult to completely remove, the treatment cycle is long, and the effect is not very ideal. At the same time, long-term systemic antibiotic treatment in clinical practice may produce antibiotic resistance and adverse reactions that affect organs. Designing new biomaterials that are compatible with antibacterial and personalized osteogenic properties is of great significance in solving the problem of infected bone defects.

[0003] Magnesium-based metal biomaterials are highly favored due to their good biocompatibility, biosafety, mechanical properties matching bone tissue, and degradable absorption in the human body. In addition, according to the reference: Han HS, Loffredo S, Jun I, et al. Current status and outlook on the clinical translation of biodegradable metals [J]. Materials Today, 2019, 23: 57-71., it can be seen that the role of magnesium ions in promoting bone regeneration and remodeling bone homeostasis has also been confirmed by clinical studies. However, the antibacterial properties of magnesium-based metal materials depend on high concentrations of degradation products OH - With Mg 2+ , rapid degradation will sacrifice its corrosion resistance and osteogenic activity, and cannot effectively promote bone integration of infected bone defects. Moreover, the degradation products will cause inflammation of surrounding tissues, resulting in adverse symptoms such as hemolysis and osteolysis. Paradoxically, the degradation products of magnesium-based metals may be quickly carried away by circulating physiological fluids and fail to produce antibacterial effects. Therefore, it is necessary to modify magnesium-based metal implants to make up for the deficiencies in matrix performance, achieve the goal of controlling degradation rate, improving antibacterial activity, and avoiding infectious inflammation to promote bone integration between implants and body bones, thereby improving the success rate of healing infected bone defects.

[0004] Surface modification is the simplest and most effective means to obtain functional coatings on magnesium-based metal surfaces. The surface-modified materials have the combined advantages of coatings and magnesium substrates, and their degradation, antibacterial, anti-tumor and osteogenesis properties are all improved. Nevertheless, most coatings targeting antibacterial targets choose highly efficient bactericidal components and anti-bioadhesion materials, and these coatings have problems such as complex preparation methods, drug-resistant bacteria and tissue inflammation, so new surface modification strategies need to be designed.

[0005] Boron is a trace element required by the human body. Low concentrations of boron can have beneficial effects on the physiological system. Studies have found that boron affects the strength, shape and mineral composition of bones, and exhibits osteogenic activity. Introducing borates into the electrolyte used to prepare micro-arc oxidation films can effectively improve their protective properties. However, there are few reports on the antibacterial, anti-inflammatory and osteogenic properties of boron-containing coating materials. Summary of the invention

[0006] In order to solve the problem in the prior art that rapid degradation of magnesium-based metal biomaterials will sacrifice their corrosion resistance and osteogenic activity, and the degradation products will also cause inflammation of surrounding tissues and fail to effectively promote bone integration of infected bone defects, the present invention provides a method for preparing a magnesium borophosphate modified pure magnesium coating, and also provides a magnesium borophosphate modified pure magnesium coating prepared by the method for preparing the magnesium borophosphate modified pure magnesium coating, and the magnesium borophosphate modified pure magnesium coating is used in the preparation of bone infection and bone repair materials, thereby improving the corrosion resistance, antibacterial properties and cell compatibility of the substrate.

[0007] The method for preparing the pure magnesium coating modified by magnesium borophosphate of the present invention comprises the following steps:

[0008] The hydrothermal solution preparation step is as follows: potassium phosphate, boric acid and water are prepared into a hydrothermal solution, wherein the mass ratio of the potassium phosphate and boric acid to the volume of water is 0.005-0.015 mol: 0.0002-0.001 mol: 10-50 mL;

[0009] Hydrothermal reaction step: hydrothermally react the pure magnesium substrate with the hydrothermal solution at 150-180° C. for 1.5 h to 6 h to obtain a borophosphate magnesium salt-modified pure magnesium coating.

[0010] Furthermore, before the hydrothermal reaction, a purification step is also included: for purifying the pure magnesium matrix, the purification step includes: removing the surface oxide layer, washing and drying sub-steps.

[0011] Furthermore, the purity of the pure magnesium matrix is ​​greater than 99.9%.

[0012] Furthermore, the potassium phosphate salt includes one or more of potassium phosphate, dipotassium hydrogen phosphate and potassium dihydrogen phosphate.

[0013] Furthermore, the ratio of the mass of the potassium phosphate salt and boric acid to the volume of water is 0.005-0.01 mol: 0.0002-0.0005 mol: 10-30 mL.

[0014] The present invention also provides a magnesium borophosphate modified pure magnesium coating, wherein the magnesium borophosphate modified pure magnesium coating is prepared by the preparation method of the magnesium borophosphate modified pure magnesium coating, and the magnesium borophosphate modified pure magnesium coating comprises a flaky magnesium hydroxide layer and a magnesium borophosphate layer, wherein the magnesium hydroxide layer is distributed on the surface of a pure magnesium substrate, and the magnesium borophosphate layer is distributed on the surface of the magnesium hydroxide layer.

[0015] Furthermore, the thickness of the magnesium borophosphate modified pure magnesium coating is 15-40 μm.

[0016] Furthermore, the magnesium borophosphate layer includes uniformly distributed needle-shaped magnesium borophosphate clusters, and the total thickness of the magnesium borophosphate layer is 5-10 μm.

[0017] The present invention also provides an application of a pure magnesium coating modified by magnesium borophosphate in the preparation of bone infection and bone repair materials.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1. Through the preparation method of the present invention, a double-layer structure coating with an inner layer of magnesium hydroxide and an outer layer of borophosphate magnesium stone is generated by reaction on the surface of pure magnesium. Boric acid in the hydrothermal solution receives hydroxide ions dissociated from water, releases hydrogen ions, can activate the metal / solution interface reaction, and promote the growth of the sediment film layer. Phosphate chemical conversion film is a deposition-type film layer, which is deposited when the concentration of film-forming ions reaches the critical supersaturation, and its deposition process is controlled by the metal / solution interface reaction. The phosphate ions and borate ions released by the pure magnesium coating modified by borophosphate magnesium salt can improve the activity of osteoblasts; at the same time, the boron oxide anions on the surface of the coating can form borate ester bonds with lipopolysaccharide or peptidoglycan on the bacterial cell wall to capture bacteria, change the functional activity of phospholipids, lipopolysaccharides and glycoproteins in the cell membrane, so that the cell membrane structure changes and ruptures, and finally causes bacterial death. Therefore, the pure magnesium coating modified by borophosphate magnesium salt reacts with the lipopolysaccharide layer to form more borate ester bonds than the peptidoglycan layer, and is more likely to destroy the bacterial structure of Gram-negative bacteria such as Escherichia coli and cause their death, so that the present invention has excellent antibacterial properties. In addition, the present invention has a slow degradation rate, improves the corrosion resistance and biocompatibility of the pure magnesium matrix, and has excellent bone-promoting performance.

[0020] 2. Compared with the methods of the prior art, the present invention utilizes a simple one-step hydrothermal synthesis method to produce a coating with good corrosion resistance, cell compatibility and antibacterial properties. It does not require a template and is not restricted by the shape of the substrate. It has low cost and simple process, and has strong clinical application significance. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the present invention or the solutions in the prior art, a brief introduction is given below to the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0022] Figure 1 A schematic diagram of the surface microstructure of a pure magnesium coating provided in Example 1 of the present invention and a partial enlarged schematic diagram;

[0023] Figure 2 A schematic diagram of the surface microstructure of a pure magnesium coating provided in Example 2 of the present invention and a partially enlarged schematic diagram;

[0024] Figure 3 A schematic diagram of the surface microstructure of a pure magnesium coating provided in Example 3 of the present invention and a partial enlarged schematic diagram;

[0025] Figure 4 It is a schematic diagram of the surface microstructure of a pure magnesium substrate and a partial enlarged schematic diagram of Comparative Example 1 of the present invention;

[0026] Figure 5 A schematic diagram of the cross-sectional microscopic morphology of a pure magnesium coating provided in Example 1 of the present invention;

[0027] Figure 6 A cross-sectional element distribution surface scan of a pure magnesium coating provided in Example 1 of the present invention;

[0028] Figure 7 The X-ray diffraction pattern of the pure magnesium coating provided in Example 1 of the present invention;

[0029] Figure 8 A potentiodynamic polarization curve diagram of the pure magnesium coating provided in Example 1 of the present invention in a phosphate buffer solution;

[0030] Fig. 9 Schematic diagram of optical density values ​​after indirect culture of cells with Example 1 and Comparative Example 1 for 1 day and 3 days;

[0031] Fig.10 This is a schematic diagram of the structure of the plate prepared in Example 1 of the present invention and Comparative Example 1 after being reacted with Gram-positive bacteria Staphylococcus aureus for 1 day;

[0032] Fig.11 This is a schematic diagram of the structure of the plate prepared in Example 1 of the present invention and Comparative Example 1 after being reacted with Gram-negative bacteria Escherichia coli for 1 day. DETAILED DESCRIPTION

[0033] Unless otherwise defined, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs; the terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention; the terms "including" and "having" and any variations thereof in the specification and claims of the present invention and the above-mentioned drawings are intended to cover non-exclusive inclusions. The terms "first", "second", etc. in the specification and claims of the present invention or the above-mentioned drawings are used to distinguish different objects, not to describe a specific order.

[0034] Reference to "embodiments" in the present invention means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present invention. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it mutually exclusive, independent, or alternative to other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in the present invention may be combined with other embodiments.

[0035] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings.

[0036] Boron has an empty p orbital in its outermost electron structure, which can act as a Lewis acid and accept external lone pairs of electrons. This determines that boric acid and its derivatives can bind to active oxygen species and play an antioxidant role. The boron atom consists of sp 2 Hybridization to sp 3 Hybridization causes changes in spatial structure that affect the properties of carbohydrates, proteins, and polypeptides. Boric acid and its derivatives esterify with 1,2- or 1,3-dihydroxy compounds to form dynamic borate ester bonds, which can be used as a driving force to induce interfacial self-assembly; based on this, the present invention explores the biological mechanism of boron-containing composite coatings modified pure magnesium implants regulating the pathological microenvironment of infected bone defects from the composition and structure of boric acid compound materials.

[0037] 1. Preparation method

[0038] The preparation method of the magnesium borophosphate modified pure magnesium coating of the present invention comprises the following steps:

[0039] The hydrothermal solution preparation step is as follows: potassium phosphate, boric acid and water are prepared into a hydrothermal solution, wherein the ratio of the mass of the potassium phosphate and boric acid to the volume of water is 0.005-0.015 mol: 0.0002-0.001 mol: 10-50 mL; the present invention has no special requirements for the preparation order of the potassium phosphate and boric acid solutions, which can be carried out simultaneously or separately.

[0040] Hydrothermal reaction step: The pure magnesium substrate and the hydrothermal solution are hydrothermally reacted at 150-180°C for 1.5h-6h to obtain a magnesium borophosphate modified pure magnesium coating. The hydrothermal reaction under these conditions is a high temperature, closed environment, and the thermal stress of the coating is small, so the density and corrosion resistance of the coating can be significantly improved.

[0041] Preferably, before the hydrothermal reaction, a purification step of purifying the pure magnesium substrate is also included: the purification step includes: removing the surface oxide layer, washing and drying sub-steps.

[0042] The present invention preferably adopts the method of sanding with water-abrasive paper to remove the oxide layer. The present invention has no special requirements for the parameters of the sanding, and the conventional sanding method in the art can be adopted; in the present invention, the water-abrasive paper preferably includes 800#, 1000# and 2000# water-abrasive paper in sequence.

[0043] Specifically, in this example, the sample surface was first polished to 2000# using metallographic sandpaper on a metallographic polishing machine to remove the surface oxide layer, and then ultrasonically cleaned in acetone for 30 minutes and then blown dry, and stored in a drying oven for later use.

[0044] The purification step and the hydrothermal solution preparation step of this example have no order of precedence and can be performed in parallel. The source and preparation of the pure magnesium substrate are not particularly limited, and conventional alloy preparation methods in the art can be used. In this example, a pure magnesium substrate plate with a purity greater than 99.9% is selected.

[0045] The potassium phosphate salt in this example includes one or more of potassium phosphate, dipotassium hydrogen phosphate and potassium dihydrogen phosphate. The ratio of the mass of the potassium phosphate salt and boric acid to the volume of water is more preferably 0.005-0.01 mol: 0.0002-0.0005 mol: 10-30 mL. The present invention has no special requirements for the preparation method of the hydrothermal reaction solution, and the solution preparation method familiar to those skilled in the art can be used. In the present invention, the purity of the potassium phosphate salt and boric acid is preferably analytically pure; in a specific embodiment of the present invention, the potassium phosphate salt is preferably dipotassium hydrogen phosphate, and the water is preferably double distilled water, which is a kind of double distilled water, and is the water obtained by distilling water again after distilling it once.

[0046] 2. Magnesium borophosphate modified pure magnesium coating

[0047] The present invention also provides a magnesium borophosphate modified pure magnesium coating, which is prepared by the preparation method of the magnesium borophosphate modified pure magnesium coating. In this example, the magnesium borophosphate modified pure magnesium coating has a double-layer structure, including a flaky magnesium hydroxide layer and a magnesium borophosphate layer, wherein the magnesium hydroxide layer is distributed on the surface of the pure magnesium substrate, and the magnesium borophosphate layer is distributed on the surface of the magnesium hydroxide layer.

[0048] The thickness of the magnesium borophosphate modified pure magnesium coating is 15-40 μm, preferably 20-30 μm. The magnesium borophosphate layer in this example includes uniformly distributed needle-shaped magnesium borophosphate clusters, and the total thickness of the magnesium borophosphate layer is 5-10 μm.

[0049] 3. Basic principles

[0050] The formation mechanism of the borophosphate magnesium salt modified pure magnesium coating prepared in this example is as follows:

[0051] The basic principle of hydrothermal reaction is:

[0052] The pure magnesium matrix undergoes a chemical reaction in the hydrothermal solution. The pure magnesium matrix dissolves to increase the ion concentration and pH value at the metal / solution interface, producing a layer of insoluble compounds deposited on the surface of the matrix. The phosphate conversion process has the advantages of being environmentally friendly and non-toxic, and has been widely studied. Phosphate chemical conversion film is a deposition-type film layer that is deposited when the film-forming ion concentration reaches the critical supersaturation, and its deposition process is controlled by the metal / solution interface reaction.

[0053] Boric acid is a small molecule Lewis acid with a pKa value between 8.92 and 9.24. The direct dissociation of boric acid in aqueous solution can be ignored. The reason why boric acid aqueous solution is acidic is that the lone pair of electrons of the oxygen atom in the water molecule enters the empty orbital of the boron atom, releasing a proton (H + ) produces sp 3 Hybridized tetrahedral boron species ([B(OH)4] - ), so the boric acid aqueous solution is acidic.

[0054] The formation principle of pure magnesium coating modified by magnesium borophosphate is:

[0055] Due to the potential difference between the impurity phase and the substrate, the pure magnesium substrate has the following electrochemical corrosion with magnesium acting as the anode and the impurity phase acting as the cathode:

[0056] Anode reaction: Mg→Mg 2+ +2e -

[0057] Cathode reaction: 2H2O+2e - →2OH - +H 2 ↑

[0058] The overall reaction is: Mg+2H2O→Mg(OH)2+H2↑

[0059] Boric acid dissolves in water and undergoes the following hydrolysis reaction:

[0060] H3BO3+H2O→[B(OH)4] - +H +

[0061] The nascent Mg(OH)2 undergoes dissociation and diffusion reactions, and immediately undergoes a neutralization reaction:

[0062] Mg(OH)2→Mg 2+ +2OH -

[0063] H + +OH - →H2O

[0064] In the environment of tetrahydroxyborate ions and hydrogen phosphate ions, magnesium ions react with them to form stable and insoluble boraxite:

[0065]

[0066] IV. Application

[0067] The borophosphate magnesium salt modified pure magnesium coating of the present invention can be used in the preparation of bone infection and bone repair biomaterials. The present invention has no special restrictions on the specific application of the coating, and it can be implanted in any combination or form for bone repair. The specific preparation method can refer to the conventional technology in the field, which will not be described here.

[0068] V. Implementation

[0069] The present invention is further illustrated by specific examples.

[0070] Embodiment 1:

[0071] A method for preparing a borophosphate-modified pure magnesium coating, comprising:

[0072] (1) Set the surface area to 1 cm 2 The pure magnesium was polished with water-abrasive paper, and the surface of the sample was polished on a metallographic polishing machine with 800#, 1000#, and 2000# water-abrasive paper in turn to remove the oxide layer, and then ultrasonically cleaned in acetone for 30 minutes, and then dried and stored in a drying oven for later use;

[0073] (2) Weigh 0.005 mol of dipotassium hydrogen phosphate and 0.001 mol of boric acid and dissolve them in 50 mL of double distilled water to prepare a hydrothermal reaction solution;

[0074] (3) placing the purified pure magnesium substrate and the above hydrothermal reaction solution in a hydrothermal reaction kettle, and performing a hydrothermal reaction at 150° C. for 3 h;

[0075] (4) After the hydrothermal reaction is completed, the reactor is cooled to room temperature, the sample is taken out, rinsed with deionized water three times, and dried in a blast drying oven for 10 minutes to obtain the desired borophosphate magnesium salt modified pure magnesium coating sample. Figure 1 shown.

[0076] Embodiment 2:

[0077] A method for preparing a borophosphate-modified pure magnesium coating, comprising:

[0078] (1) Set the surface area to 1 cm 2 The pure magnesium substrate was polished with water-abrasive paper, and the surface of the sample was polished on a metallographic polishing machine with 800#, 1000#, and 2000# water-abrasive paper to remove the oxide layer, and then ultrasonically cleaned in acetone for 30 minutes, and then dried and stored in a drying oven for later use;

[0079] (2) Weigh 0.005 mol of dipotassium hydrogen phosphate and 0.0002 mol of boric acid and dissolve them in 50 mL of double distilled water to prepare a hydrothermal reaction solution;

[0080] (3) placing the purified pure magnesium substrate and the above hydrothermal reaction solution in a hydrothermal reaction kettle, and performing a hydrothermal reaction at 150° C. for 3 h;

[0081] (4) After the hydrothermal reaction is completed, the reactor is cooled to room temperature, the sample is taken out, rinsed with deionized water three times, and dried in a blast drying oven for 10 minutes to obtain the desired borophosphate magnesium salt modified pure magnesium coating sample. Figure 2 shown.

[0082] Embodiment 3:

[0083] (1) Set the surface area to 1 cm 2 The pure magnesium substrate was polished with water-abrasive paper, and the surface of the sample was polished on a metallographic polishing machine with 800#, 1000#, and 2000# water-abrasive paper to remove the oxide layer, and then ultrasonically cleaned in acetone for 30 minutes, and then dried and stored in a drying oven for later use;

[0084] (2) Weigh 0.015 mol of dipotassium hydrogen phosphate and 0.001 mol of boric acid and dissolve them in 50 mL of double distilled water to prepare a hydrothermal reaction solution;

[0085] (3) placing the purified pure magnesium substrate and the above hydrothermal reaction solution in a hydrothermal reaction kettle, and performing a hydrothermal reaction at 150° C. for 3 h;

[0086] (4) After the hydrothermal reaction is completed, the reactor is cooled to room temperature, the sample is taken out, rinsed with deionized water three times, and dried in a blast drying oven for 10 minutes to obtain the desired borophosphate magnesium salt modified pure magnesium coating sample. Figure 3 shown.

[0087] Comparative Example 1:

[0088] A pure magnesium without any coating, the preparation process of which is the same as the pure magnesium purification method in step (1) of implementation 1, and the obtained pure magnesium substrate is as follows Figure 4 shown.

[0089] pass Figure 1-Figure 3 It can be seen that the borophosphate magnesium clusters on the borophosphate magnesium salt modified pure magnesium coating sample generated in Example 1 are evenly distributed on the surface of the magnesium hydroxide layer, and the surface layer presents a uniform needle-like shape, which is a more preferred embodiment. The number of borophosphate magnesium clusters generated in Example 2 is slightly less, and they are dispersed on the magnesium hydroxide layer. In the hydrothermal reaction process of Example 3, the contents of dipotassium hydrogen phosphate and boric acid are both high, so more borophosphate magnesium clusters are generated. After a uniform borophosphate magnesium layer is generated on the surface of the magnesium hydroxide layer, several borophosphate magnesium clusters are deposited on the surface of the borophosphate magnesium layer.

[0090] VI. Experimental Verification

[0091] In this example, the pure magnesium coating sample modified by magnesium borophosphate prepared in Example 1 was selected for testing to verify the characterization and performance of the pure magnesium coating sample modified by magnesium borophosphate of the present invention.

[0092] In this example, the sample with the coating was subjected to scanning electron microscopy (SEM), energy dispersive spectrum analysis (EDS), X-ray diffraction analysis (XRD), potentiodynamic polarization curve (PDP), cytotoxicity and proliferation (CCK8) and plate coating analysis, and the analysis results are as follows:

[0093] like Figure 1-Figure 4 The SEM image of the sample with the coating is shown, wherein the left side is a low magnification image and the right side is a high magnification image. It can be found that the surface of the uncoated pure magnesium substrate shows a large number of scratches formed by sandpaper polishing, while the surface of the coating sample of the present invention shows no scratches, and a large number of needle-like flakes are deposited, uniformly and completely covering the substrate surface.

[0094] like Figure 5 As shown, the cross-sectional SEM image of the sample with the coating of the present invention shows that the interface between the coating and the substrate is continuous, and there is no gap or film separation between the interfaces, indicating that the interface between the coating and the substrate is well bonded. The coating is a double-layer structure with a coating thickness of about 28 μm. Figure 6 As shown in the figure, the EDS scanning image of the cross section of the coating sample shows that the outer layer of the coating is enriched with Mg, P, and O. The chemical composition of the inner layer is mainly composed of Mg and O. Since B is a light element, it cannot be detected by EDS.

[0095] Figure 7The figure shows the X-ray diffraction pattern (XRD) of the sample with the coating, wherein the horizontal axis 2Theta (degree, angle) is the diffraction angle, and the vertical axis Intensity is the relative intensity of the diffraction peak. Figure 7 It can be seen that the characteristic diffraction peak of pure magnesium without coating in comparative example 1 is Mg peak. In comparison, in addition to the diffraction peak of Mg, characteristic diffraction peaks of Mg(OH)2 and Mg3B2(OH)6(PO4)2(H2O)6 can also be detected in the coating sample of embodiment 1 of the present invention, indicating that the main phases of the coating are Mg(OH)2 and Mg3B2(OH)6(PO4)2(H2O)6. XRD phase analysis results are similar to Figure 6 The cross-sectional EDS elemental composition analysis results were consistent, further confirming that the elemental composition of the coating was Mg(OH)2 and Mg3B2(OH)6(PO4)2(H2O)6.

[0096] Figure 8 The figure shows the obtained potentiodynamic polarization curve (PDP) of the sample with the coating, wherein the horizontal axis Current density is the current density and the vertical axis Potential is the electrode potential. In the electrochemical research of metal corrosion, it is generally believed that the potentiodynamic polarization curve is an effective and rapid method to evaluate the corrosion resistance of metal materials or metal materials with coatings. In theory, the self-corrosion potential (E corr ) is more positive, indicating that the material has a lower tendency to corrode thermodynamically and a higher corrosion resistance. corr ) is smaller, indicating that the corrosion rate of the material in the environment is lower. Figure 8 It can be seen that, compared with the uncoated pure magnesium in comparative example 1, the polarization curve of the coated sample in embodiment 1 of the present invention shifts to the left, and the corrosion current density decreases, indicating that the coating can significantly improve the corrosion resistance of pure magnesium. The polarization curves of the untreated pure magnesium and the coated sample are fitted by Tafel, and the corresponding E corr and i corr . Untreated pure magnesium E corr and i corr -1.32V and 2.50×10 -5 A.cm 2 . E of the coating sample corr and i corr -1.25 and 5.56×10 -6 A.cm 2 Compared with untreated pure magnesium, the coated samples showed lower i corr and the corrected E corr , revealing that the coating effectively improves the corrosion resistance of pure magnesium.

[0097] like Fig. 9 As shown in the figure, the CCK8 experimental results were obtained by indirect co-culturing the cells with the coating sample of Example 1 of the present invention and the pure magnesium substrate extract of Comparative Example 1 for 1 day and 3 days respectively. Figure 8 It can be seen that after 1d and 3d of co-culture, the OD (optical density) value of the coating sample group of Example 1 of the present invention is significantly higher than that of the uncoated pure magnesium, and as the culture time increases, the OD values ​​of the coating sample and the uncoated pure magnesium group both increase, indicating cell proliferation. This shows that the coating of Example 1 of the present invention effectively improves the cell compatibility of pure magnesium.

[0098] Fig.10 The following are photos of colonies on a plate after the coating sample of Example 1 (right figure) and the pure magnesium substrate of Comparative Example 1 (left figure) were treated with Gram-positive bacteria Staphylococcus aureus for 1 day. Fig.11 The following are photos of colonies on the plate after the coating sample of Example 1 (the figure on the right) and the pure magnesium substrate of Comparative Example 1 (the figure on the left) were treated with Gram-negative bacteria Escherichia coli for 1 day.

[0099] from Fig.10 and Fig.11 It can be seen that for the Staphylococcus aureus group, the samples in the coated sample group and the uncoated pure magnesium group were surrounded by colonies, and no obvious inhibition zone was formed; for the Escherichia coli group, the samples in the coated sample group formed an obvious inhibition zone around the sample, while the samples in the uncoated pure magnesium group were still surrounded by colonies, and no obvious inhibition zone was formed. The formation of the inhibition zone is due to the dissolution of the boron oxide anions in the coating and diffusion into the nutrient agar around the sample to kill Escherichia coli, so that a colony-free inhibition zone is formed around the sample.

[0100] Since the boron oxide anions on the coating surface can form borate ester bonds with the lipopolysaccharide or peptidoglycan on the bacterial cell wall, the bacteria are captured, the functional activity of the phospholipids, lipopolysaccharides and glycoproteins in the cell membrane is changed, the cell membrane structure is changed and ruptured, and finally the bacteria die. Because the lipopolysaccharide layer of Gram-negative bacteria has more 1,2-diol or 1,3-diol structures than the peptidoglycan layer of Gram-positive bacteria, the borophosphate magnesium modified pure magnesium coating reacts with the lipopolysaccharide layer to form more borate ester bonds than the peptidoglycan layer, which is easier to destroy the structure of Gram-negative bacteria and cause their death. Therefore, this example has a good antibacterial effect on Gram-negative bacteria. This example uses Escherichia coli among Gram-negative bacteria for testing. In addition, this example can also be used for antibacterial treatment of bacteria such as Staphylococcus epidermidis and Acinetobacter baumannii.

[0101] Through the above test verification, it can be seen that the borophosphate magnesium salt modified pure magnesium coating provided by the present invention has a slow degradation rate, good cell compatibility and antibacterial properties, improves the corrosion resistance and cell compatibility of the pure magnesium substrate, and improves the antibacterial properties of the pure magnesium substrate. In addition, the boric acid and potassium phosphate salt modified pure magnesium coating has an antibacterial effect on Gram-negative bacteria Escherichia coli, but has no antibacterial effect on Gram-positive bacteria Staphylococcus aureus.

[0102] In addition, compared with the methods of the prior art, the present invention utilizes a simple one-step hydrothermal synthesis method to produce a coating with good corrosion resistance, cell compatibility and antibacterial properties. It does not require a template and is not restricted by the shape of the substrate. It has a low cost and a simple process, and has strong clinical application significance.

[0103] The specific implementation modes described above are preferred implementation modes of the present invention, and are not intended to limit the specific implementation scope of the present invention. The scope of the present invention includes but is not limited to the specific implementation modes, and all equivalent changes made according to the present invention are within the protection scope of the present invention.

Claims

1. A method for preparing a pure magnesium coating modified by magnesium borophosphate, characterized in that: The steps include: The hydrothermal solution preparation step is as follows: potassium phosphate, boric acid and water are prepared into a hydrothermal solution, wherein the mass ratio of the potassium phosphate and boric acid to the volume of water is 0.005-0.015 mol: 0.0002-0.001 mol: 10-50 mL; Hydrothermal reaction step: hydrothermally react the pure magnesium substrate with the hydrothermal solution at 150-180° C. for 1.5 h to 6 h to obtain a borophosphate magnesium salt-modified pure magnesium coating.

2. The method for preparing a pure magnesium coating modified by magnesium borophosphate according to claim 1, characterized in that: Before the hydrothermal reaction, a purification step is also included: for purifying the pure magnesium matrix, the purification step includes: removing the surface oxide layer, washing and drying sub-steps.

3. The method for preparing a pure magnesium coating modified by magnesium borophosphate according to claim 1 or 2, characterized in that: The purity of the pure magnesium matrix is ​​greater than 99.9%.

4. The method for preparing a pure magnesium coating modified by magnesium borophosphate according to claim 1 or 2, characterized in that: The potassium phosphate salt includes one or more of potassium phosphate, dipotassium hydrogen phosphate and potassium dihydrogen phosphate.

5. The method for preparing a pure magnesium coating modified by magnesium borophosphate according to claim 1 or 2, characterized in that: The ratio of the mass of the potassium phosphate salt and boric acid to the volume of water is 0.005-0.01 mol: 0.0002-0.0005 mol: 10-30 mL.

6. A pure magnesium coating modified by magnesium borophosphate, characterized in that: The magnesium borophosphate modified pure magnesium coating is prepared by the preparation method of the magnesium borophosphate modified pure magnesium coating according to any one of claims 1 to 5.

7. The magnesium borophosphate modified pure magnesium coating according to claim 6, characterized in that: The magnesium borophosphate modified pure magnesium coating comprises a flaky magnesium hydroxide layer and a magnesium borophosphate layer. The magnesium hydroxide layer is distributed on the surface of the pure magnesium substrate, and the magnesium borophosphate layer is distributed on the surface of the magnesium hydroxide layer.

8. The magnesium borophosphate modified pure magnesium coating according to claim 7, characterized in that: The thickness of the magnesium borophosphate modified pure magnesium coating is 15-40 μm.

9. The magnesium borophosphate modified pure magnesium coating according to claim 7, characterized in that: The magnesium borophosphate layer includes uniformly distributed needle-shaped magnesium borophosphate clusters, and the total thickness of the magnesium borophosphate layer is 5-10 μm.

10. Use of the pure magnesium coating modified by magnesium borophosphate according to any one of claims 6 to 9 in the preparation of bone infection and bone repair materials.