Manufacturing method of sulfuric acid corrosion resistant seamless steel tube

The preparation of chemically specific sulfuric acid dew point corrosion-resistant steel through smelting and continuous rolling processes, solving the problem of failure of traditional steel in low temperature environments, and achieving efficient and economical seamless steel pipe production, with excellent corrosion resistance and high production efficiency , suitable for high sulfur-containing flue gas environments.

CN118976797APending Publication Date: 2024-11-19HENGYANG VALIN STEEL TUBE CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411071353.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Traditional sulfuric acid-resistant dew point corrosion-resistant steel fails in the low-temperature flue gas emission environment. The market demands new seamless steel pipes that are resistant to sulfuric acid-resistant dew point corrosion. The existing materials such as enamel pipes and borosilicate glass pipes have a long construction cycle and low heat recovery efficiency.

Method used

Prepare the chemical composition specific sulfuric acid-resistant dew point corrosion steel of the blank through smelting, continuous casting and continuous rolling processes, and control the content of elements such as C, Si, Mn, P, S, Cu, Cr, Ni, Sb, Ti, Mo, Nb, Al, etc. , the hot continuous rolling process is used to produce seamless steel pipes to ensure their high corrosion resistance in low temperature environments.

Benefits of technology

The obtained seamless steel pipe showed excellent comprehensive mechanical properties in the 24-hour corrosion resistance experiment, with a corrosion rate lower than that of traditional steel, good surface quality, fast production speed and high economicality, suitable for boilers, economizers and air pre-pre- Components such as heaters extend service life and reduce energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976797A_ABST
    Figure CN118976797A_ABST
Patent Text Reader

Abstract

The invention discloses a manufacturing method of a sulfuric acid corrosion resistant seamless steel tube, and belongs to the technical field of seamless steel tube manufacturing. The blank comprises the following chemical components in percentage by weight: 0.06 to 0.12 percent of C, 0.15 to 0.50 percent of Si, 0.30 to 1.10 percent of Mn, less than or equal to 0.020 percent of P, 0.01 to 0.02 percent of S, 0.20 to 0.60 percent of Cu, 0.70 to 1.25 percent of Cr, 0.10 to 0.65 percent of Ni, 0.10 to 0.40 percent of Sb, 0.015 to 0.025 percent of Ti, 0.25 to 0.65 percent of Mo, 0.015 to 0.030 percent of Nb, 0.02 to 0.05 percent of Als and the balance of Fe and inevitable impurities; the technology comprises the steps of continuous casting, rolled steel heating and rolling, the rolling process is conducted in a continuous rolling pipe unit, and the obtained sulfuric acid dew point corrosion resistant steel has the following good comprehensive mechanical properties that ReL is larger than or equal to 315 MPa, Rm is larger than or equal to 440 MPa, A is larger than or equal to 25.0%; the corrosion resistance is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of seamless steel pipe manufacturing, and relates to a method for manufacturing a seamless steel pipe resistant to sulfuric acid corrosion. Background Art

[0002] In the power, petroleum, chemical, and flue-cured tobacco industries, high sulfur-containing fuels are usually used. After combustion, sulfur first forms SO2, which is further oxidized into SO3 gas under certain conditions. SO3 gas dissolves in water vapor and combines with it to form sulfuric acid vapor. When the flue gas temperature drops below the sulfuric acid dew point or contacts the metal pipe wall with a lower temperature, sulfuric acid will condense on the metal surface, causing severe corrosion to the metal pipe wall. This corrosion is called sulfuric acid dew point corrosion.

[0003] Steel resistant to sulfuric acid dew point corrosion is widely used in the manufacture of economizers and air preheaters that serve in high-sulfur flue gas to resist dew point corrosion of sulfur-containing flue gas. At present, seamless steel pipes used in economizers and air heat exchangers of boilers in petroleum refining enterprises and power stations can all be made of sulfuric acid dew point corrosion steel, and the market prospects are broad. Environmental significance Since the flue gas generated by the combustion of coal, fuel oil, and domestic garbage produces acid corrosion on the metal surface, with the increase in boiler capacity and parameters in the power generation industry such as coal, gas, and fuel oil, as well as the key use of fuels with high sulfur content, the rise of industries such as biomass power generation, the sulfuric acid dew point corrosion problem faced by steel is becoming more and more serious. Due to the national policy of energy conservation and emission reduction, power generation, petroleum refining, and other industries require low flue gas temperature (below 130°C), which makes the sulfuric acid dew point corrosion in the low temperature section of flue gas more serious. The service temperature of traditional ND (09CrCuSb) steel is higher than 130°C, which can no longer meet the flue gas emission requirements after low temperature. The market urgently needs the development of new seamless steel pipes for sulfuric acid dew point corrosion resistance.

[0004] At present, enamel tubes, borosilicate glass tubes, non-metallic coatings, etc. are mostly used to avoid sulfuric acid dew point corrosion. Such materials not only have a long construction period, but also reduce the heat recovery efficiency. Therefore, the development and use of a new type of acid-resistant steel that can be used for a long time in sulfuric acid and hydrochloric acid dew point corrosion environments is of great significance for improving the service life of components such as boilers, economizers, air preheaters, chimneys, reducing energy consumption and protecting the environment. Summary of the invention

[0005] The present invention aims to provide a method for preparing a seamless steel pipe resistant to sulfuric acid dew point corrosion, and produces sulfuric acid dew point corrosion resistant steel with ReL≥315MPa, RmMPa≥440, A≥25.0%; and has the advantages of fast production speed, good economy, high product precision, good surface quality, etc.

[0006] The present invention is achieved through the following technical solutions:

[0007] A method for manufacturing a seamless steel pipe resistant to sulfuric acid corrosion, wherein the chemical composition of the blank is C=0.06-0.12% by weight, Si=0.15-0.50%, Mn=0.30-1.10%, P≤0.020%, S=0.01-0.02%, Cu=0.20-0.60%, Cr=0.70-1.25%, Ni=0.10-0.65%, Sb=0.10-0.40%, Ti=0.015-0.025%, Mo=0.25-0.65%, Nb=0.015-0.030%, Als=0.02-0.05, and the rest is Fe and unavoidable impurities; the key process steps include:

[0008] 1) Smelting: Using molten iron and scrap steel as raw materials, the billet is smelted through electric furnace smelting, refining furnace refining, and vacuum treatment in a vacuum degassing furnace. The chemical composition of the billet is strictly controlled during the smelting process;

[0009] 2) Continuous casting: The smelted molten steel is continuously casted by a round billet arc continuous casting machine, and the temperature of the molten steel in the refining furnace ladle is controlled to be liquidus temperature + (90-110) ± 10°C; the billet drawing speed is controlled at 1.00-3.50m / min, and the superheat is controlled at 20-35°C; the LF refining time is ≥45min, the VD holding time is ≥10min, and the soft argon blowing time after breaking and feeding wire is 15-25min; after cutting the HGNS continuous casting billet to a certain length, the billet is stacked and slowly cooled;

[0010] 3) Continuous rolling: The round tube billet obtained after sawing and cutting to length is heated by an annular furnace, pierced by a conical piercing machine, rolled by a continuous rolling mill, sized by a sizing mill, and then cooled on a large cooling bed. It is sawed to the ordered length by a tube row saw; the sulfuric acid dew point corrosion resistant steel ReL≥315MPa, RmMPa≥440, A≥25.0% is obtained.

[0011] Furthermore, the outer diameter of the blank is φ150-280 mm.

[0012] Furthermore, after the conical perforator perforates in step 3), a perforated rough tube is obtained, and the wall thickness of the perforated rough tube is 12 to 35 mm.

[0013] Furthermore, in the step 3) continuous rolling, the mandrel diameter of the continuous tube rolling mill is 119-278 mm, and the starting rolling temperature is 1000-1050°C.

[0014] Furthermore, in the step 3) continuous rolling, the hot rolled steel pipe has an outer diameter of 47.6 to 273 mm and a wall thickness of 3.6 to 7.0 mm.

[0015] The working principle of each chemical element in steel:

[0016] The amount of C element is controlled at 0.06% to 0.12%, which can significantly improve the quality of steel grade A.r1 Temperature promotes the nucleation of proeutectoid ferrite, which is beneficial to corrosion resistance. At the same time, this content range can not only ensure the strength and weldability of the steel, but also ensure the precipitation of the second phase particles.

[0017] Si is the main deoxidizer in steel, which can improve the purity of molten steel, and when Si and Cu work together, it can improve the corrosion resistance of steel. However, when Si is added in too high an amount, it will deteriorate the welding performance of steel, reduce the low-temperature toughness of the welding heat-affected zone, and deteriorate the processing performance of steel. Therefore, it should be controlled within a reasonable range to ensure its processing performance while improving corrosion resistance and intergranular corrosion resistance. Therefore, the Si content used in the present invention is 0.15% to 0.50%.

[0018] Mn is one of the most economical alloying elements. Mn atoms have a very large solid solubility in steel, which can significantly improve the strength of steel without losing the plasticity of steel. However, Mn also has an adverse effect on the welding performance and corrosion resistance of steel, so it should be controlled within a reasonable range. The Mn content range used in the present invention is Mn = 0.30% to 1.10%.

[0019] S is a harmful element in ordinary steel, and the lower its content, the better. However, for the acid-resistant steel involved in the present invention, the presence of a certain amount of S element can, on the one hand, promote the formation of a Cu2S film on the surface of the steel when it comes into contact with an acidic solution. The film can play a passivation role, preventing the acidic solution from further reacting with the steel and protecting the steel from being corroded by sulfuric acid. On the other hand, it can also inhibit the galvanic cell effect and reduce the self-corrosion effect. However, if the S content is low and is not enough to form a Cu2S passivation film, Cu + If it is simply dissolved and accumulated on the surface of the steel pipe, it will not only fail to achieve anti-corrosion effect, but will also increase the anode area and accelerate the galvanic cell reaction. Therefore, the sulfur content in the steel should be controlled between 0.01% and 0.02%.

[0020] P is a harmful element in steel. P will be segregated at the grain boundary, making the steel brittle and detrimental to the toughness of the steel. The P content range used in the present invention is P≤0.020%.

[0021] Cr in steel can improve strength and hardness through solid solution strengthening and grain refinement without reducing impact toughness.

[0022] The formation of Cu compounds (such as CuO and Cu2S) on the surface of Cu metal can prevent the metal from suffering local corrosion. The enrichment of Cu on the metal surface inhibits the active dissolution of the matrix, thereby improving the corrosion resistance of the metal. However, too high a Cu content is not conducive to the formation of a passivation film, so the Cu content range used in the present invention is: 0.20% to 0.60%.

[0023] Sb oxide Sb2O5 is relatively stable in acidic solution, especially can promote the formation of Cu-containing compounds, can further inhibit the anodic reaction of metals, and the addition of Sb can prevent the corrosion of H2SO4 on steel, but the antimony content should be controlled within a suitable range, aiming to improve the corrosion resistance of sulfuric acid while reducing the adverse effects on the strength, toughness, plasticity and weldability of steel. Therefore, the Sb content range used in the present invention is: 0.10% to 0.40%.

[0024] Mo, as a strong carbide-forming element, expands the ferrite phase region and promotes the formation of ferrite. The Mo element not only hinders the growth of austenite grains, but also helps to refine ferrite grains and improve the strength and toughness of steel. MoO3 also has high stability in strong acidic solutions, and can reduce the dissolution of the corrosion product layer in acid solutions and improve the stability of the corrosion product film. Therefore, the Mo content range used in the present invention is: 0.25% to 0.65%.

[0025] Ti can make the internal structure of steel dense, reduce aging sensitivity and cold brittleness, and improve welding performance, but its content in steel should be reasonably controlled to resist sulfuric acid corrosion in high temperature and high concentration environment and have good intergranular corrosion resistance. At the same time, Ti has a strong affinity with N and C in steel, and can form carbides, nitrides, and carbonitrides to improve the strength and plasticity of steel. Therefore, the Ti content range used in the present invention is: 0.015% to 0.025%.

[0026] Nb is distributed in the form of small-sized carbonitride particles in low alloy steel, and has a significant effect on refining grain size, increasing strength, hardness, and improving toughness. The Nb content range used in the present invention is: 0.015% to 0.030%.

[0027] The Ni element can greatly improve the strength and low temperature toughness of steel by refining grains and strengthening solid solution. At the same time, under appropriate proportions, Ni can also reduce surface cracks caused by Cu element. The Ni content range used in the present invention is: 0.10% to 0.65%.

[0028] The addition of Al element can effectively improve the stability of austenite. At the same time, Al element can significantly increase the stacking fault energy and pin dislocations to achieve the effect of strengthening the steel. Too much Al element will reduce the toughness of the steel. Therefore, the Als content range used in the present invention is: 0.02% to 0.05%.

[0029] The present invention has the following advantages and positive effects: The present invention adopts hot rolling process to produce sulfuric acid dew point corrosion resistant seamless steel pipe, which has the advantages of fast production speed, good economy, high product precision, good surface quality, etc. The obtained sulfuric acid dew point corrosion resistant steel has the following good comprehensive mechanical properties: ReL≥315MPa, Rm≥440MPa, A≥25.0%. Among them, in the 24h corrosion resistance test, the average corrosion rate is 32g / m 2 ×h, according to GB 150.2-2011A.3.5d), the corrosion-resistant steel pipe is immersed in a 50% H2SO4 solution at a constant temperature of 70℃±2℃ for 24h, and the average corrosion rate of the two samples is not more than 140g / m 2 ×h, which is sufficient to show that the present invention has better sulfuric acid corrosion resistance than 20 steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is the microstructure diagram of the HGNS seamless steel pipe of Example 1.

[0031] Figure 2 This is the microstructure diagram of the HGNS seamless steel pipe of Example 2. DETAILED DESCRIPTION

[0032] The technical solutions in the embodiments of the present invention will be described in detail below with reference to the accompanying drawings in the embodiments of the present invention.

[0033] Example 1: Production of φ48×4mm HGNS seamless steel pipe

[0034] The chemical composition of the steel is shown in Table 1. The key process steps include:

[0035] 1) Smelting: Use high-quality molten iron and high-quality scrap steel as raw materials, and smelt the billet through 45-ton electric furnace smelting, 45-ton refining furnace refining, 45-ton vacuum degassing furnace and round billet arc continuous casting machine continuous casting process. During the smelting process, the chemical composition of HGNS steel is strictly controlled to meet the requirements of chemical composition. Round billet arc continuous casting machine continuous casting, control the temperature of the molten steel in the refining furnace ladle = liquidus temperature + (90-110) ± 10 ℃; the billet drawing speed is controlled at 2.00-3.50m / min, and the superheat is controlled at 20-35 ℃; LF refining time ≥ 45min, VD holding time ≥ 10min, and the soft argon blowing time after breaking and feeding wire is 15-25min. Crystallizer electric stirring: 175A / 3HZ. End electric stirring: 480A / 7HZ. After cutting the HGNS continuous casting billet to a certain size, stack and slow cooling.

[0036] 2) Continuous rolling: The HGNS billet is heated in a ring furnace according to the heating system in Table 2. When preparing a seamless steel pipe of φ48*4mmHGNS, the piercing temperature is 1180℃, the size after piercing is φ159*13mm, the size after rolling is φ122*4mm, the diameter reduction in the continuous rolling process is 37mm, and the wall reduction is 9mm. The CTP two-roller oblique rolling piercing machine has a head diameter of 118mm, a roll pitch of 129mm, and a roll speed of 450rpm.

[0037] The pass profile of the continuous rolling tube is φ128mm, the speeds of the 6 stands are 680, 920, 910, 890, 910, 990rpm respectively, and the starting rolling temperature is 1000℃~1050℃.

[0038] The mechanical properties and corrosion resistance of the HGNS seamless steel pipe of this example were measured, wherein the tensile properties are shown in Table 4, and the weight loss per unit area of ​​the corrosion test is shown in Table 5.

[0039] It can be seen from the data in Table 4 and Table 5 that HGNS exhibits better mechanical properties and corrosion resistance than Comparative Example 1.

[0040] like Figure 1 As shown, the microstructure of the seamless steel pipe of this embodiment is determined to be polygonal ferrite and pearlite, and the grain size is level 10. The non-metallic inclusions of the φ48x 4mm HGNS seamless steel pipe of this embodiment are: A 0, B 0.5, C0, D 0.5, Ds0.5, and the flattening test is qualified.

[0041] Example 2: Production of φ273×7mm HGNS seamless steel pipe

[0042] The chemical composition of the steel is shown in Table 1. The key process steps include:

[0043] 1) Smelting: Use high-quality molten iron and high-quality scrap steel as raw materials, and then smelt the billet through 90-ton electric furnace smelting, 100-ton refining furnace refining, double-station vacuum degassing furnace and round billet arc continuous casting machine continuous casting process. During the smelting process, the chemical composition of HGNS steel is strictly controlled to meet the requirements of chemical composition. The round billet arc continuous casting machine is used for continuous casting. The temperature of the molten steel in the refining furnace ladle is controlled to be liquidus temperature + (90-110) ± 10 °C; the billet drawing speed is controlled at 1.00-1.90 m / min, and the superheat is controlled at 20-

[0044] 35℃; LF refining time ≥45min, VD holding time ≥10min, soft argon blowing time after air breaking and wire feeding 15-25min. Crystallizer electric stirring: 175A / 3HZ. End electric stirring: 480A / 7HZ. After cutting the HGNS continuous casting billet to a certain length, stack and slow cool.

[0045] 2) Continuous rolling: The HGNS billet is heated in a ring furnace according to the heating system in Table 3. When preparing a seamless steel pipe of φ273*7mmHGNS, the piercing temperature is 1180℃, the size after piercing is φ336*19.8mm, the size after rolling is φ293*7mm, the diameter reduction of the continuous rolling process is 43mm, and the wall reduction is 13mm. The CTP two-roller oblique rolling piercing machine has a head diameter of 272mm, a mandrel diameter of 259mm, a roll pitch of 241.8mm, and a roll speed of 350rpm.

[0046] The continuous rolling tube pass is φ293mm, the mandrel diameter is 278.4mm, and the starting rolling temperature is 1000℃~1050℃.

[0047] The mechanical properties and corrosion resistance of the HGNS seamless steel pipe of this example were measured, wherein the tensile properties are shown in Table 4, and the weight loss per unit area of ​​the corrosion test is shown in Table 5.

[0048] It can be seen from the data in Tables 4 and 5 that HGNS exhibits good mechanical properties and corrosion resistance.

[0049] like Figure 2 As shown, after testing the microstructure of the seamless steel pipe of this embodiment, it is determined that the structure is polygonal ferrite and pearlite, and the grain size is 9.5. The non-metallic inclusions of the φ273x 7mm HGNS seamless steel pipe of this embodiment are: A 0, B0.5, C0.5, D 0.5, Ds 0, and the flattening test is qualified.

[0050] Comparative Example 1: 20 steel is rolled into 48*4mm seamless steel pipe

[0051] The sulfuric acid corrosion resistance of the seamless steel pipes of Example 1, Example 2 and Comparative Example 1 is compared, and the results are shown in Table 5.

[0052] Test method: The average corrosion weight loss rate of steel in 70℃ hydrochloric acid solution refers to immersing a certain thickness of steel in a 50% sulfuric acid solution at 70℃ for 24 hours, then taking it out and drying it, and calculating the weight difference Δm before and after immersion. The average corrosion weight loss rate of steel = Δm (weight difference before and after immersion) / (S (surface area of ​​steel) × 24 (h)). For comparison, the corrosion weight loss data in sulfuric acid solutions with mass concentrations of 15% and 50% at room temperature were also tested.

[0053] Table 1 Chemical composition of examples and comparative examples (wt)

[0054] element C Si Mn P S Cu Cr Ni Sb Ti Mo Als Nb Example 1 0.08 0.20 0.35 0.015 0.010 0.42 0.95 0.25 0.18 0.02 0.45 0.03 0.018 Example 2 0.08 0.19 0.34 0.010 0.008 0.45 1.02 0.26 0.22 0.08 0.19 0.34 0.010 Comparative Example 1 0.19 0.19 0.37 0.020 0.019 / / / / / / / /

[0055] Table 2 Heating system of HGNS billet in ring furnace (unit 89)

[0056]

[0057] Table 3 Heating system of HGNS billet in ring furnace (340 units)

[0058]

[0059] Table 4 Mechanical properties test results of examples and comparative examples

[0060] Rp0.2(MPa) Rm(MPa) A(%) Example 1 415 600 31 Example 1 420 586 31.5 Example 2 406 589 32 Example 2 412 603 31.3

[0061] Table 5 Corrosion resistance test results of examples and comparative examples

[0062]

[0063]

Claims

1. A method for manufacturing a seamless steel pipe resistant to sulfuric acid corrosion, characterized in that: The chemical composition of the blank by weight percentage is C=0.06-0.12%, Si=0.15-0.50%, Mn=0.30-1.10%, P≤0.020%, S=0.01-0.02%, Cu=0.20-0.60%, Cr=0.70-1.25%, Ni=0.10-0.65%, Sb=0.10-0.40%, Ti=0.015-0.025%, Mo=0.25-0.65%, Nb=0.015-0.030%, Als=0.02-0.05, and the rest is Fe and unavoidable impurities; The key process steps include: 1) Smelting: Using molten iron and scrap steel as raw materials, the billet is smelted through electric furnace smelting, refining furnace refining, and vacuum treatment in a vacuum degassing furnace. The chemical composition of the billet is strictly controlled during the smelting process; 2) Continuous casting: The smelted molten steel is continuously casted by a round billet arc continuous casting machine, and the temperature of the molten steel in the refining furnace ladle is controlled to be liquidus temperature + (90-110) ± 10°C; the billet drawing speed is controlled at 1.00-3.50m / min, and the superheat is controlled at 20-35°C; the LF refining time is ≥45min, the VD holding time is ≥10min, and the soft argon blowing time after breaking and feeding wire is 15-25min; after cutting the HGNS continuous casting billet to a certain length, the billet is stacked and slowly cooled; 3) Continuous rolling: The round tube billet obtained after sawing and cutting to length is heated by an annular furnace, pierced by a conical piercing machine, rolled by a continuous rolling mill, sized by a sizing mill, and then cooled on a large cooling bed. It is sawed to the ordered length by a tube row saw; the sulfuric acid dew point corrosion resistant steel ReL≥315MPa, RmMPa≥440, A≥25.0% is obtained.

2. The method for manufacturing a seamless steel pipe resistant to sulfuric acid corrosion according to claim 1, characterized in that: The outer diameter of the blank is φ150-280 mm.

3. The method for manufacturing a seamless steel pipe according to claim 1, characterized in that: After the conical perforator perforates in step 3), a perforated rough tube is obtained, and the wall thickness of the perforated rough tube is 12 to 35 mm.

4. The method for manufacturing a seamless steel pipe resistant to sulfuric acid corrosion according to claim 1, characterized in that The step 3) continuous rolling: the mandrel diameter of the continuous tube rolling unit is 119-278 mm, and the starting rolling temperature is 1000-1050°C.

5. The method according to claim 1, characterized in that: Step 3) Continuous rolling: The hot rolled steel pipe has an outer diameter of 47.6 to 273 mm and a wall thickness of 3.6 to 7.0 mm.

Citation Information

Patent Citations

  • Zr-containing sulphuric acid dew point corrosion resistant steel plate and manufacturing method thereof

    CN103160753A

  • Improved 09CrCuSb steel resistant to sulfuric acid dew point corrosion and manufacturing method thereof

    CN105937010A

  • Thick-specification Q420-level high-temperature and high-pressure resisting sulfuric acid dew point corrosion steel plate and production method thereof

    CN108286017A

  • Tungsten-containing sulfuric acid dew point corrosion resistant steel and production method thereof

    CN114807760A