Preparation process of high-performance aluminum-based composite material based on laser additive
Patent Information
- Application Number
- CN202411070025.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
但现有技术中采用原位自生方式还存在着反应过程难以控制,易形成粗大有害相,成形的材料致密度低等问题
[0030] 1. The present invention first uses the sol-gel method to prepare titanium dioxide-coated boron-enhanced powder. The titanium dioxide coating layer generated by the sol-gel method has fine grains, which can achieve uniform titanium dioxide coating on the surface of the boron powder and effectively prevent Defects and unevenness in cladding. During the laser melting process, aluminum can reduce titanium dioxide to form aluminum oxide (Al 2 O 3 ) and titanium (T i), titanium (T i) reacts with boron powder to form titanium diboride (T iB 2 ), the remaining titanium (T i) reacts with aluminum to form titanium aluminum alloy (TiAl 3 ). Boron powder is wrapped with titanium dioxide to avoid direct reaction between boron powder and aluminum to form aluminum boride (AlB 2 ), and in the presence of titanium dioxide, aluminum preferentially reacts with titanium dioxide, and its reaction thermodynamics and kinetic conditions take precedence, again avoiding aluminum borides (Al B 2 ) production; aluminum boride (Al B 2 ) can increase hardness, but it also increases the brittleness of the material.
Smart Images

Figure CN118976907A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal additive manufacturing, and in particular to a preparation process of a high-performance aluminum-based composite material based on laser additive manufacturing. Background Art
[0002] Laser additive manufacturing (3D printing) is a new type of material manufacturing technology. It uses external 3D modeling software such as UG and ProE to build a model of the part, converts the model into G code through slicing software, and finally uses G code to control the 3D printing equipment to manufacture solid parts from bottom to top. Compared with traditional material removal manufacturing, this method does not require a mold. The existing technology can prepare high-performance metal parts with complex shapes by controlling the laser scanning path to melt metal powder layer by layer. At the same time, for additive manufacturing, the utilization rate of its raw materials is nearly 100%, and parts can be formed in one go without multiple processing steps.
[0003] Laser additive manufacturing mainly covers two core technologies: one is selective laser melting (SLM) technology, and the other is laser melting deposition (LMD) technology. Selective laser melting uses a high-energy laser beam to completely melt metal powder, and then quickly cools and forms it to obtain high-density, high-precision metal parts. SLM technology can directly manufacture highly complex components with mechanical properties better than castings. The molded parts have high precision, and the surface can meet the use accuracy requirements with a little surface treatment. It is suitable for manufacturing complex workpieces with complex internal structures that are difficult to process with traditional methods.
[0004] SLM forming technology is widely used in materials, and has currently achieved the forming of metal-based composite materials such as aluminum-based, nickel-based, titanium-based, and iron-based. Aluminum-based composite materials are composite materials formed by adding reinforcing phases (such as ceramic particles, intermetallic compounds, etc.) with aluminum and its alloys as the matrix. Aluminum-based composite materials have the advantages of low density, high strength, high modulus, good wear resistance, fatigue resistance, and high temperature resistance, and are widely used in aerospace, automotive, electronics, and sporting goods.
[0005] The introduction of reinforcing phase can be divided into two ways: direct addition and in-situ self-generation. Direct addition refers to adding reinforcing phase directly to the aluminum matrix from the outside. Generally, the reinforcing phase particles are coarse, there are defects inside, and the interface bonding with the matrix is weak, which cannot meet the use requirements of certain environments. Compared with the direct addition method, when the reinforcing phase is generated by the in-situ self-generation method, since the reinforcing phase directly nucleates and grows in the matrix, the interface contamination between the reinforcing phase and the matrix is avoided, the reinforcing phase is evenly distributed and the interface bonding is good, thereby more effectively improving the performance of the material. However, the in-situ self-generation method in the prior art still has problems such as the reaction process is difficult to control, coarse and harmful phases are easily formed, and the density of the formed material is low. Summary of the invention
[0006] Based on the problems existing in the background technology, the present invention provides a preparation process of a high-performance aluminum-based composite material based on laser additive manufacturing, which significantly improves the comprehensive performance of the aluminum-based composite material.
[0007] The present invention is implemented by the following technical solutions:
[0008] A preparation process of a high-performance aluminum-based composite material based on laser additive manufacturing comprises the following steps:
[0009] S1. A boron-enhanced powder of titanium dioxide was prepared by a sol-gel method;
[0010] S2. The boron-enhanced titanium dioxide-coated powder obtained in step S1 is mixed evenly with the AlS i 10Mg powder under an inert gas protection to obtain a mixed powder;
[0011] S3. Process the mixed powder through laser additive manufacturing method to obtain high-performance aluminum-based composite materials.
[0012] Furthermore, the specific operation of the sol-gel method in step S1 is: dissolving butyl titanate in anhydrous ethanol, adding deionized water, adjusting the solution pH to 5-6 with hydrochloric acid, and stirring to obtain a sol; adding boron powder to the sol, stirring to make it evenly dispersed, aging at room temperature for 12-24 hours to form a gelled sample; placing the gelled sample in an oven to remove the sol and moisture; and finally placing it in a muffle furnace for high-temperature calcination to finally obtain a reinforced powder of titanium dioxide encapsulated boron.
[0013] Furthermore, the concentration of the butyl titanate ethanol solution is 0.85-1.58 mol / L; and the molar ratio of deionized water to butyl titanate is 2:1.
[0014] Furthermore, the mass ratio of boron powder to sol is 1:(6-12); and the particle size of the boron powder is 1-10 μm.
[0015] Furthermore, the high temperature calcination temperature is 500-600°C, and the calcination time is 2-4h.
[0016] Furthermore, in step S2, the mass ratio of the boron-encapsulated titanium dioxide reinforcing powder to the AlS10Mg powder is (1-5): (95-99); the particle size range of the AlS10Mg is 15 μm to 53 μm.
[0017] Furthermore, in step S2, the boron-encapsulated titanium dioxide reinforced powder and the AlS10Mg powder are uniformly mixed under the protection of inert gas, specifically by using a ball mill for mixing, with a ball-to-material ratio of (1-2):1, a ball milling speed of 80-120 rpm, indirect ball milling for 8-12 hours, and air cooling for 10 minutes for every 30 minutes of ball milling.
[0018] Furthermore, the laser additive manufacturing method in step S3 includes the following steps:
[0019] S31. Establishing a three-dimensional model of the workpiece, performing layered slicing on the model, and setting processing parameters of the workpiece;
[0020] S32. The mixed powder is placed in the powder cavity. The powder spreading device spreads the mixed powder on the forming workbench according to the set parameters. According to the slice model data, laser selective melting and consolidation are performed layer by layer to obtain a high-performance aluminum-based composite material.
[0021] Furthermore, in step S32, after the mixed powder is placed in the powder chamber, argon gas is introduced to ensure that the oxygen content in the equipment is less than 50 ppm.
[0022] Furthermore, the laser selection process parameters of step S32 are: laser peak power of 200-350W, laser efficiency of 35%, spot diameter of 0.08-0.1mm, scanning speed of 1000-2000mm / s, scanning spacing of 50-80μm, powder thickness of 30-50μm, and scraper time of 10s.
[0023] Furthermore, in step S2, after the boron-encapsulated titanium oxide reinforced powder and the Al Si 10Mg powder are mixed for 8 hours using a ball mill under inert gas protection, a ball mill mixing degree detection system can be used to detect the uniformity of the mixed powder to ensure that the boron-encapsulated titanium oxide reinforced powder and the Al Si 10Mg powder are evenly mixed.
[0024] Furthermore, the ball milling mixing degree detection system includes:
[0025] Automatic sampling module for extracting ball-milled powder during cooling intervals;
[0026] An image acquisition module is used to acquire images of the sampled mixed ball-milled powder, including an industrial CCD camera and system, and an LED light source;
[0027] An image processing module performs grayscale processing on the collected mixed ball-milled powder image;
[0028] The calculation and analysis module calculates and processes the image of the mixed ball-milled powder, compares it with the preset threshold, and transmits the corresponding control instructions to the ball milling equipment according to the results.
[0029] Beneficial effects of the present invention:
[0030] 1. The present invention first adopts the sol-gel method to prepare the titanium dioxide-encapsulated boron reinforced powder. The titanium dioxide coating layer generated by the sol-gel method has fine grains, which can achieve uniform titanium dioxide coating on the surface of the boron powder, effectively preventing defects and unevenness of the coating layer. During the laser melting process, aluminum can reduce titanium dioxide to generate aluminum oxide (Al2O3) and titanium (Ti), and titanium (Ti) reacts with boron powder to generate titanium diboride (T iB2). The remaining titanium (T i) reacts with aluminum to generate titanium aluminum alloy (TiAl3). The use of titanium dioxide to encapsulate boron powder avoids the direct reaction of boron powder and aluminum to generate aluminum boride (AlB2), and in the presence of titanium dioxide, aluminum is more inclined to react with titanium dioxide first, and its reaction thermodynamics and kinetic conditions are prioritized, which again avoids the generation of aluminum boride (Al B2); although aluminum boride (Al B2) can increase hardness, it will also increase the brittleness of the material.
[0031] 2. Under the action of high-energy laser, through in-situ reaction, the interface defects caused by physical mixing in traditional methods are reduced, and the mechanical properties of the composite material are improved. The generation of aluminum oxide (Al2O3) can fill the micropores and defects in the material, improve the overall size and density of the material, and at the same time, the good interface bonding between aluminum oxide (Al2O3) and the matrix material can improve the overall strength of the material. Strong interface bonding helps to reduce the expansion of cracks and improve the fracture toughness of the material. In the SLM process, titanium diboride (TiB2) can form a stable phase with the matrix aluminum alloy. Titanium diboride (TiB2) can effectively prevent the expansion and transmission of cracks, and can significantly enhance the impact resistance and crack propagation resistance of the composite material. Titanium aluminum alloy (TiAl3), as an intermetallic compound, has high hardness and good high-temperature stability. Titanium aluminum alloy (TiAl3) can form a hard phase in the material, which helps to improve the hardness and wear resistance of the material. Since the present invention adopts the reinforcing powder of titanium dioxide coated with boron, the in-situ generation of aluminum oxide (Al2O3), titanium diboride (T iB2) and titanium aluminum alloy (T iAl3) in Al Si 10Mg is not isolated, and they will interact with each other to jointly improve the comprehensive performance of the alloy. The precipitation of titanium diboride (TiB2) and titanium aluminum alloy (T iAl3) further promotes the generation of aluminum oxide (Al2O3), and the high hardness of aluminum oxide (Al2O3) can provide support for other strengthening phases to form a more compact strengthening network. These in-situ generated phases are usually dispersed in the α-Al matrix, playing a role of dispersion strengthening, and the in-situ generated phases can optimize the distribution of the precipitated phases, reduce the agglomeration of the precipitated phases, thereby improving the uniformity and stability of the alloy; at the same time, since SLM laser additive manufacturing has the characteristics of fast cooling rate, it has the effect of inhibiting grain growth, thereby playing a role of refining grains, and grain refinement helps to improve the strength and toughness of the alloy. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The accompanying drawings are used to provide further explanation of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0033] Figure 1 This is an optical microscope image of the high-performance aluminum-based composite material sample prepared in Example 1. DETAILED DESCRIPTION
[0034] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments, but the protection scope of the present invention is not limited to the following embodiments.
[0035] Example 1
[0036] A preparation process of a high-performance aluminum-based composite material based on laser additive manufacturing comprises the following steps:
[0037] S1. A boron-enhanced powder of titanium dioxide was prepared by a sol-gel method;
[0038] Butyl titanate is dissolved in anhydrous ethanol, and the concentration of the butyl titanate ethanol solution is 1.1 mol / L; deionized water is added, and the molar ratio of deionized water to butyl titanate is 2:1, and the pH value of the solution is adjusted to 6 with hydrochloric acid, and stirred to obtain a sol; boron powder is added to the sol, and the mass ratio of boron powder to sol is 1:10, and stirred to make it evenly dispersed, and aged at room temperature for 12 hours to form a gelled sample; the gelled sample is placed in an oven to remove the sol and moisture; finally, it is placed in a muffle furnace for high-temperature calcination, the high-temperature calcination temperature is 550°C, and the calcination time is 3 hours, and finally a reinforced powder of titanium dioxide encapsulated boron is obtained.
[0039] S2. The titanium dioxide-coated boron reinforced powder obtained in step S1 is mixed with AlSi10Mg powder in a mass ratio of 5:95 in a ball mill under inert gas protection, with a ball-to-material ratio of 2:1, a ball milling speed of 100 rpm, indirect ball milling for 10 hours, and air cooling for 10 minutes after every 30 minutes of ball milling; mix well to obtain a mixed powder.
[0040] S3. Processing of mixed powder by laser additive manufacturing:
[0041] S31. Establish a three-dimensional model of the workpiece, perform layered slicing on the model, and set processing parameters for the workpiece;
[0042] S32. Place the mixed powder into the powder chamber and introduce argon gas to ensure that the oxygen content in the equipment is less than 50ppm. The powder spreading device spreads the mixed powder on the molding workbench according to the set parameters. According to the slicing model data, laser selection is performed layer by layer for melting and forming. The laser selection process parameters are: laser peak power of 250W, laser efficiency of 35%, spot diameter of 0.1mm, scanning speed of 1000mm / s, scanning spacing of 60μm, and powder spreading thickness of 30μm, so as to obtain high-performance aluminum-based composite materials.
[0043] The optical microscope image of the high performance aluminum-based composite material prepared in this embodiment is as follows: Figure 1 As shown, the reinforcement phase is evenly dispersed in the aluminum matrix composite material, and there are no obvious defects between the reinforcement phase and the matrix interface, which has good interface bonding performance.
[0044] Example 2
[0045] A preparation process of a high-performance aluminum-based composite material based on laser additive manufacturing comprises the following steps:
[0046] S1. A boron-enhanced powder of titanium dioxide was prepared by a sol-gel method;
[0047] Butyl titanate is dissolved in anhydrous ethanol, and the concentration of the butyl titanate ethanol solution is 1.4 mol / L; deionized water is added, and the molar ratio of deionized water to butyl titanate is 2:1, and the pH value of the solution is adjusted to 6 with hydrochloric acid, and stirred to obtain a sol; boron powder is added to the sol, and the mass ratio of boron powder to sol is 1:10, and stirred to make it evenly dispersed, and aged at room temperature for 12 hours to form a gelled sample; the gelled sample is placed in an oven to remove the sol and moisture; finally, it is placed in a muffle furnace for high-temperature calcination, the high-temperature calcination temperature is 550°C, and the calcination time is 3 hours, and finally a reinforced powder of titanium dioxide encapsulated boron is obtained.
[0048] The remaining steps are the same as in Example 1.
[0049] Example 3
[0050] A preparation process of a high-performance aluminum-based composite material based on laser additive manufacturing comprises the following steps:
[0051] S1. A titanium dioxide-encapsulated boron reinforced powder was prepared using a sol-gel method (same as in Example 1).
[0052] S2. The titanium dioxide-coated boron reinforced powder obtained in step S1 is mixed with AlS10Mg powder in a mass ratio of 3:97 in a ball mill under inert gas protection, with a ball-to-material ratio of 2:1, a ball mill speed of 100 rpm, indirect ball milling for 10 hours, and air cooling for 10 minutes every 30 minutes of ball milling; mix well to obtain a mixed powder.
[0053] S3. Processing the mixed powder by laser additive manufacturing method (same as Example 1).
[0054] Comparative Example 1
[0055] A preparation process of an aluminum-based composite material based on laser additive manufacturing comprises the following steps:
[0056] S1. Mix aluminum oxide (Al2O3), titanium diboride (TiB2) and AlSi10Mg powders in a mass ratio of 2:3:95 in a ball mill under inert gas protection, with a ball-to-material ratio of 2:1, a ball mill speed of 100 rpm, indirect ball milling for 10 hours, and air cooling for 10 minutes every 30 minutes of ball milling; mix well to obtain a mixed powder.
[0057] S2. Processing the mixed powder by laser additive manufacturing method (same as Example 1).
[0058] Comparative Example 2
[0059] A preparation process of an aluminum-based composite material based on laser additive manufacturing comprises the following steps:
[0060] S1. Mix titanium dioxide, boron powder and Al Si 10Mg powder in a mass ratio of 3:2:95 in a ball mill under inert gas protection, with a ball-to-material ratio of (1-2):1, a ball mill speed of 80-120 rpm, indirect ball milling for 8-12 hours, and air cooling for 10 minutes after every 30 minutes of ball milling; mix well to obtain a mixed powder.
[0061] S2. Processing the mixed powder by laser additive manufacturing method (same as Example 1).
[0062] Test example
[0063] The performance of the aluminum-based composite materials prepared in Examples 1-3 and Comparative Examples 1-2 was tested, and the results are shown in Table 1.
[0064] Table 1
[0065] Group Density(%) Tensile strength(MPa) Elongation(%) Example 1 99.74 510.5 5.82 Example 2 99.68 508.6 5.76 Example 3 99.83 509.1 5.64 Comparative Example 1 97.97 453.4 4.48 Comparative Example 2 97.59 415.8 3.80
[0066] As can be seen from the results in Table 1, the aluminum-based composite material sample prepared in the embodiment of the present invention has a high density and relatively good mechanical properties. In Comparative Example 1, aluminum oxide (Al2O3) and titanium diboride (TiB2) are directly added as reinforcing phases. The interface bonding between the directly added reinforcing phase and the matrix material is often poor, and there may be many defects in the interface area, which may produce microcracks, leading to stress concentration, affecting the overall density and mechanical properties. The composite material with directly added reinforcing phases is prone to brittle fracture at the interface defects, which may reduce the toughness of the material. The reinforcing phases generated in situ in the present invention usually have better interface bonding, because these phases are generated in the matrix material by chemical reaction, forming a metallurgical bond. Good interface bonding helps to reduce defects and voids in the interface area and improve the density and mechanical properties of the material. The aluminum oxide (Al2O3) and titanium diboride (TiB2) generated in situ can fill microscopic defects and pores during the formation process, further improving the density of the material. In comparative example 2, titanium dioxide and boron powder are directly added. Titanium dioxide and aluminum react with aluminotherm under laser melting. Aluminum reduces titanium dioxide to generate aluminum oxide (Al2O3) and titanium (Ti). Since the distribution of titanium dioxide and boron powder is discontinuous, the titanium (Ti) generated by reduction may react less with boron powder. Boron powder easily reacts with aluminum to generate aluminum boride (Al B2). Although aluminum boride (Al B2) can improve hardness, it will also increase the brittleness of the material, resulting in a decrease in the tensile strength and elongation of the composite material. The uniform titanium dioxide coating layer in the present invention can ensure that a consistent titanium diboride (TiB2) reinforcement phase is generated in a local area. Titanium diboride (T iB2) has high hardness and high modulus, and can significantly improve the mechanical properties of the material. The uniform titanium dioxide coating layer makes the generation of the reinforcement phase more controllable during the SLM process, reducing the fluctuation of material properties.
[0067] Example 4
[0068] In step S2, after the titanium oxide-encapsulated boron reinforcing powder and the Al Si 10Mg powder are mixed for 8 hours using a ball mill under inert gas protection, the uniformity of the mixed powder can be detected using a ball mill mixing degree detection system to ensure that the titanium oxide-encapsulated boron reinforcing powder and the Al Si 10Mg powder are evenly mixed.
[0069] Among them, the ball mill mixing degree detection system includes:
[0070] Automatic sampling module for extracting ball-milled powder during cooling intervals;
[0071] An image acquisition module is used to acquire images of the sampled mixed ball-milled powder, including an industrial CCD camera and system, and an LED light source;
[0072] An image processing module performs grayscale processing on the collected mixed ball-milled powder image;
[0073] The calculation and analysis module calculates and processes the image of the mixed ball-milled powder, compares it with the preset threshold, and transmits the corresponding control instructions to the ball milling equipment according to the results.
[0074] The operation process of the ball milling mixing degree detection system is as follows:
[0075] S1, the automatic sampling module extracts the mixed ball-milled powder during the cooling time of the ball mill and sends it to the CCD camera detection position;
[0076] S2, the image acquisition module uses a CCD camera to extract images of the mixed ball-milled powder;
[0077] S3, the image processing module removes noise and performs gray value statistics on the collected mixed ball mill powder image;
[0078] S4. Calculate the uniformity index V of the collected mixed ball mill powder:
[0079]
[0080] v i is the gray value of the i-th pixel of the collected image, is the grayscale mean of the collected image, and a is the number of pixels in the collected image.
[0081] S5. The threshold is set by test data, and the calculation and analysis module compares the calculated uniformity index V with the threshold. If its value is greater than the threshold, it is determined that the mixing is uneven and the ball mill continues to work. If its value is less than the set threshold, it is determined that the mixing is uniform and meets the requirements. The calculation and analysis module sends a command to the ball mill to stop working.
[0082] Finally, it should be noted that the above-mentioned embodiments only express several implementation methods of the present invention and are not intended to limit the invention. For those skilled in the art, any modification, equivalent replacement, improvement, etc. made without departing from the concept of the present invention should be included in the protection scope of the invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A process for preparing a high-performance aluminum-based composite material based on laser additive, characterized in that: The following steps are involved: S1. A boron-enhanced powder of titanium dioxide was prepared by a sol-gel method; S2. The boron-enhanced titanium dioxide-coated powder obtained in step S1 is mixed with AlSi 10Mg powder under an inert gas protection to obtain a mixed powder; S3. Process the mixed powder through laser additive manufacturing method to obtain high-performance aluminum-based composite materials.
2. The preparation process according to claim 1, characterized in that: The specific operation of the sol-gel method in step S1 is as follows: dissolve butyl titanate in anhydrous ethanol, add deionized water, adjust the solution pH to 5-6 with hydrochloric acid, and stir to obtain a sol; add boron powder to the sol, stir to make it evenly dispersed, and age at room temperature for 12-24 hours to form a gelled sample; put the gelled sample into an oven to remove the sol and moisture; finally, put it into a muffle furnace for high-temperature calcination to finally obtain a reinforced powder of titanium dioxide encapsulated boron.
3. The preparation process according to claim 2, characterized in that: The concentration of the butyl titanate ethanol solution is 0.85-1.58 mol / L; the molar ratio of deionized water to butyl titanate is 2:
1.
4. The preparation process according to claim 2, characterized in that: The mass ratio of boron powder to sol is 1:(6-12); the particle size of the boron powder is 1-10 μm.
5. The preparation process according to claim 2, characterized in that: The high temperature calcination temperature is 500-600°C and the calcination time is 2-4h.
6. The preparation process according to claim 1, characterized in that: In step S2, the mass ratio of the boron-encapsulated titanium dioxide reinforcing powder to the AlSi 10Mg powder is (1-5): (95-99); the particle size range of the AlSi 10Mg is 15 μm to 53 μm.
7. The preparation process according to claim 1, characterized in that: In step S2, the titanium dioxide-encapsulated boron reinforced powder and the AlSi 10Mg powder are mixed uniformly under the protection of inert gas, specifically: a ball mill is used for mixing, the ball-to-material ratio is (1-2): 1, the ball milling speed is 80-120 rpm, the indirect ball milling is 8-12 hours, and air cooling is performed for 10 minutes every 30 minutes of ball milling.
8. The preparation process according to claim 1, characterized in that: The laser additive manufacturing method in step S3 includes the following steps: S31. Establish a three-dimensional model of the workpiece, perform layered slicing on the model, and set processing parameters for the workpiece; S32. The mixed powder is placed in the powder cavity. The powder spreading device spreads the mixed powder on the forming workbench according to the set parameters. According to the slice model data, laser selective melting and consolidation are performed layer by layer to obtain a high-performance aluminum-based composite material.
9. The preparation process according to claim 8, characterized in that: Step S32: After the mixed powder is placed in the powder chamber, argon gas is introduced to ensure that the oxygen content in the equipment is less than 50 ppm.
10. The preparation process according to claim 8, characterized in that: The laser selection process parameters of step S32 are: laser peak power of 200-350W, laser efficiency of 35%, spot diameter of 0.08-0.1mm, scanning speed of 1000-2000mm / s, scanning spacing of 50-80μm, powder thickness of 30-50μm, and scraper time of 10s.
Citation Information
Patent Citations
Method for preparing composite powder for laser 3D printing through sol coating method
CN112024872A
Laser additive manufacturing method of in-situ synthesized nano Al2O3 reinforced aluminum-based composite material
CN112176213A
Preparation method of interface strengthening in-situ reinforced aluminum-based composite material based on laser additive manufacturing