Cu / SnAgCu / Cu brazing method based on Cu5Zn8 diffusion barrier layer preparation
By preparing the Cu5Zn8 diffusion barrier layer on the surface of the Cu substrate and brazing it with SnAgCu brazing, the problems of poor wetting of the SnAgCu brazing on the surface of the Cu substrate and excessive growth of intermetallic compounds on the interface are solved, and high wetting of the brazing joints is achieved The high-quality and low-cost process significantly inhibits the overgrowth of intermetallic compounds in the interface.
Patent Information
- Application Number
- CN202411326998.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-19
AI Technical Summary
The SnAgCu solder has poor wettability on the surface of Cu substrate, and the intermetallic compounds are overgrown in the aging stage, resulting in a decrease in joint performance. The existing modification methods are costly and complex in the process.
The Cu5Zn8 diffusion barrier layer was prepared on the surface of the Cu substrate, and the Cu5Zn8 diffusion barrier layer was prepared by the dip welding method and then soldered with SnAgCu brazing to form a Cu substrate/Cu5Zn8 diffusion barrier layer/SnAgCu brazing/Cu5Zn8 diffusion barrier layer/Cu substrate structure. Simplify the process and reduce costs.
It effectively inhibits the overgrowth of intermetallic compounds at the interface of the brazing joint, improves the wettability of the brazing system, and is simple in process and low in cost, avoiding the deterioration problem caused by brazing alloying.
Smart Images

Figure CN118976956A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electronic packaging soft soldering, and in particular provides a soldering method which is suitable for a Cu substrate / SnAgCu solder / Cu substrate soldering system and has high wettability and can inhibit excessive growth of joint interface compounds in an aging stage. Background Art
[0002] In recent years, the rapid development of smart phones and microcomputers towards high-density centralization and lightweight components has put forward higher requirements for advanced electronic packaging technology. Therefore, how to obtain Sn-based solder with good wettability and Sn / Cu interface intermetallic compound layer with moderate thickness is the goal that has been pursued in the current electronic packaging field. Since the promulgation of the lead restriction order, many scholars have been committed to the research and development of new lead-free solders, among which SnAgCu lead-free solder has shown obvious advantages due to its better comprehensive performance, but compared with Sn-Pb solder, SnAgCu solder still has many disadvantages.
[0003] For example, the wettability of SnAgCu solder on the surface of Cu substrate is poor. In addition, metallurgical reaction will occur when SnAgCu solder wets and spreads on the surface of Cu pad to form joint, generating interfacial Cu-Sn intermetallic compound layer. During the service life of the welded joint, excessive growth of interfacial intermetallic compound will seriously affect the joint performance and lead to more defects. More importantly, due to the different thermal expansion coefficients of SnAgCu solder, interfacial intermetallic compound layer and Cu substrate, when under the influence of thermal strain for a long time during the brazing process, thermal fatigue cracks will appear in the thicker intermetallic compound layer, and cracks will propagate as the welding time increases, further reducing the reliability of the joint.
[0004] At present, in response to this situation, many scholars at home and abroad have improved the wettability of the brazing system and inhibited the growth of interfacial compounds by adding foreign elements or nanoparticles to the SnAgCu solder. However, the alloying of the solder will lead to a certain degree of deterioration. For example, the addition of Ta, W, and Mo will increase the melting point of the solder, the Ni element may cause peeling at the solder joint interface, and the presence of various alloying elements and nanoparticles will reduce the conductivity of the solder joint. Therefore, the current research method has changed to the surface modification of the Cu substrate, usually introducing a diffusion barrier layer on the surface of the Cu substrate. The main preparation methods currently include magnetron sputtering, electroplating, and chemical plating, but the preparation cost is high and the process is complicated. Therefore, obtaining a surface coating with simple process, low preparation cost and good bonding with the Cu substrate is the main problem to be solved by current technology. Summary of the invention
[0005] In view of the current situation that the interface compounds of the joints of the Cu / SnAgCu / Cu brazing system are prone to excessive growth, the present invention proposes a Cu / SnAgCu / Cu brazing method based on the preparation of a Cu5Zn8 diffusion barrier layer, so that the Cu5Zn8 diffusion barrier layer with simple preparation process, low cost and good bonding with the Cu substrate is obtained, which can greatly inhibit the excessive growth of intermetallic compounds (IMC) at the interface of the brazing joint in the aging stage, and at the same time improve the wettability of the Cu / SnAgCu / Cu brazing system.
[0006] The technical solution for achieving the purpose of the present invention is as follows:
[0007] A Cu / SnAgCu / Cu brazing method based on the preparation of a Cu5Zn8 diffusion barrier layer, taking a Cu / SnAgCu / Cu brazing system composed of a SnAgCu solder and a Cu substrate as the object, preparing a Cu5Zn8 diffusion barrier layer on the surface of the Cu substrate, and then using a SnAgCu solder to braze the Cu substrate prepared with the Cu5Zn8 diffusion barrier layer to obtain a brazed joint of a Cu substrate / Cu5Zn8 diffusion barrier layer / SnAgCu solder / Cu5Zn8 diffusion barrier layer / Cu substrate structure. The specific process includes the following steps:
[0008] Step 1, placing the polished, cleaned and dried Sn-Zn solder in a crucible and placing it in a pit furnace, setting the temperature of the pit furnace to 245-265° C., and heating the solder in the furnace to a molten state;
[0009] Step 2, preparing a soldering flux according to the mass fraction of 90% ZnCl2:10% NH4Cl, and dissolving the soldering flux powder in anhydrous ethanol at a volume fraction of 1:1;
[0010] Step 3, evenly apply flux to the surface of the polished, cleaned and dried Cu substrate, and place it together with the fixture in a muffle furnace for preheating;
[0011] Step 4, use a fixture to clamp and fix the Cu substrate, immerse it vertically and uniformly in the molten Sn-Zn solder, take it out vertically and uniformly after dip soldering, and air cool it. The dip soldering time is 2 to 30 seconds;
[0012] Step 5, after cooling, the sample is placed in an etching solution and ultrasonicated at room temperature for 60 to 90 minutes to remove excess solder on the surface until the off-white Cu5Zn8 diffusion barrier layer is completely exposed on the surface;
[0013] Step 6, placing the polished, cleaned and dried SnAgCu solder between two cleaned and dried Cu substrates prepared with Cu5Zn8 diffusion barrier layers to form a sandwich structure of Cu substrate with Cu5Zn8 diffusion barrier layer / SnAgCu solder / Cu substrate with Cu5Zn8 diffusion barrier layer;
[0014] Step 7, placing the assembled pre-welded parts into a high vacuum brazing furnace for brazing connection to obtain a brazed joint of the structure of Cu substrate / Cu5Zn8 diffusion barrier layer / SnAgCu solder / Cu5Zn8 diffusion barrier layer / Cu substrate.
[0015] Furthermore, the composition of the Sn-Zn solder is 3-12 wt.% Zn, with the balance being Sn.
[0016] Furthermore, the composition of the SnAgCu solder is Sn3.0Ag0.5Cu.
[0017] Furthermore, the crucible in step 1 is an alumina crucible.
[0018] Furthermore, the grinding, cleaning and drying treatment described in step 1 is to grind the Sn-Zn solder, then ultrasonically clean it with acetone, alcohol and deionized water for 15 to 20 minutes, and put it into a drying oven at a constant temperature of 40 to 50°C for 20 to 30 minutes.
[0019] Furthermore, the preheating temperature of the muffle furnace described in step 3 is 245~265°C.
[0020] Furthermore, the polishing, cleaning and drying treatment described in step 3 is to polish the Cu substrate, then ultrasonically clean it with acetone, alcohol and deionized water for 15 to 20 minutes, and put it into a drying oven at a constant temperature of 40 to 50° C. for drying for 20 to 30 minutes.
[0021] Furthermore, the SnAgCu solder after the grinding, cleaning and drying treatment in step 6 is that the SnAgCu solder is ground, ultrasonically cleaned with acetone, alcohol and deionized water for 15 to 20 minutes in sequence, and placed in a drying oven at a constant temperature of 40 to 50° C. for 20 to 30 minutes.
[0022] Furthermore, the cleaning and drying of the Cu substrate prepared with the Cu5Zn8 diffusion barrier layer described in step 6 is to ultrasonically clean it with acetone, alcohol and deionized water for 15 to 20 minutes in sequence, and then put it in a drying oven at a constant temperature of 40 to 50°C for drying for 20 to 30 minutes.
[0023] Furthermore, the brazing connection in the high vacuum brazing furnace described in step 7 is carried out in a CMD-238 high vacuum brazing furnace. When the vacuum degree reaches 5×10 -3 Pa, start heating, heat to 180℃ at a heating rate of 8.5℃ / min and keep warm for 5min, then heat to 250℃ at a heating rate of 6℃ / min and keep warm for 1min, then cool with the furnace.
[0024] The present invention has the following advantages:
[0025] (1) By preparing a Cu5Zn8 diffusion barrier layer on the surface of the Cu substrate, the preparation process is simple, the cost is low, the surface is flat and dense, and the bonding with the Cu substrate is good. It has good electrical and thermal conductivity, avoiding the disadvantages of the conventional brazing system modification method, which is expensive and the alloying of the brazing material will lead to a certain degree of degradation.
[0026] (2) A Cu5Zn8 diffusion barrier layer is prepared on the surface of the Cu substrate. After brazing, a brazed joint with the structure of Cu substrate / Cu5Zn8 diffusion barrier layer / SnAgCu solder / Cu5Zn8 diffusion barrier layer / Cu substrate is formed. The Cu5Zn8 diffusion barrier layer can effectively hinder the diffusion of elements in the brazed joint and greatly inhibit the excessive growth of intermetallic compounds (IMC) at the interface of the brazed joint during the aging stage.
[0027] (3) During the brazing process, the Cu5Zn8 diffusion barrier layer prepared on the surface of the Cu substrate contacts the SnAgCu solder, which improves the wettability of the Cu / SnAgCu / Cu brazing system. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 In Example 1, a solder joint of a Cu substrate with a 0.496 μm thick Cu5Zn8 diffusion barrier layer was prepared by soldering with SnAgCu solder for 2 seconds at 160 o The interface microstructure after C aging for 240 hours. The black part at the bottom of the figure is the Cu substrate, the grayish white part at the top is the SnAgCu solder, and the grayish black part between the two is the interface metal compounds Cu6Sn5 and Cu3Sn. The average thickness of the interface metal compound layer is 9.287μm.
[0029] Figure 2 In Example 2, a solder joint of a Cu substrate with a 0.571 μm thick Cu5Zn8 diffusion barrier layer was prepared by soldering with SnAgCu solder for 5 seconds at 160 o The interface microstructure after C aging for 240 hours. The black part at the bottom of the figure is the Cu substrate, the gray-white part at the top is the SnAgCu solder, and the gray-black part between the two is the interface metal compounds Cu6Sn5 and Cu3Sn. The average thickness of the interface metal compound layer is 6.847μm.
[0030] Figure 3 For Example 3 at 250 o C conditions, the wetting angle morphology of SnAgCu solder on the Cu substrate prepared with Cu5Zn8 diffusion barrier layer (dip soldering 10s, Cu5Zn8 diffusion barrier layer thickness 0.674μm). The wetting angle of the SnAgCu / Cu brazing system is 21.161o .
[0031] Figure 4 In Example 3, a solder joint of a Cu substrate with a 0.674 μm thick Cu5Zn8 diffusion barrier layer was prepared by soldering with SnAgCu solder for 10 seconds at 160 o The interface microstructure after C aging for 240 hours. The black part at the bottom of the figure is the Cu substrate, the grayish white part at the top is the SnAgCu solder, and the grayish black part between the two is the interface intermetallic compounds Cu6Sn5 and Cu3Sn. The average thickness of the interface intermetallic compound layer is 7.754μm. DETAILED DESCRIPTION
[0032] Example 1
[0033] This embodiment is a Cu / SnAgCu / Cu brazing method based on the preparation of Cu5Zn8 diffusion barrier layer. In this embodiment, the excessive growth of intermetallic compounds (Cu6Sn5 and Cu3Sn) at the interface during the aging process is significantly suppressed in the Cu substrate prepared by the dip soldering method. The specifications of the Cu substrate involved are 10 mm×10 mm×2 mm, the SnAgCu solder is Sn3.0Ag0.5Cu, and the specifications for wetting are 1 mm×8 mm, the specification for brazing is 10 mm×10 mm×0.2 mm, and the composition of Sn-Zn solder used for preparing Cu5Zn8 diffusion barrier layer by dip soldering is 4 wt.% Zn, and the balance is Sn.
[0034] The specific process of this embodiment includes the following steps:
[0035] Step 1, the surface of the Sn-Zn solder is polished with two passes of SiC sandpaper of 240Cw and 400Cw in sequence to ensure that there is no oxide film on the surface, and then ultrasonically cleaned with acetone, alcohol, and deionized water for 15 minutes in sequence, and placed in a drying oven at a constant temperature of 41°C for 22 minutes;
[0036] Step 2, the surface of a 10 mm × 10 mm Cu substrate was polished with four SiC sandpapers of 400 Cw, 1000 Cw, 1500 Cw, and 2000 Cw in sequence. The substrate was rotated 90° and polished again when the sandpaper was changed each time. After the 2000 Cw sandpaper was polished, the substrate was rotated 90° again and gently rubbed on the sandpaper to make a cross or grid scratch on the surface of the substrate. After the polishing was completed, acetone, alcohol, and deionized water were used for ultrasonic cleaning for 15 minutes in sequence, and the substrate was placed in a drying oven with a constant temperature of 41°C for drying for 22 minutes;
[0037] Step 3, rinse the experimental fixture, crucible and ceramic plate with anhydrous ethanol and place them in a drying oven at a constant temperature of 41°C for 22 minutes;
[0038] Step 4, placing the polished, cleaned and dried Sn-Zn solder in an alumina crucible and placing it in a pit furnace, setting the temperature of the pit furnace to 250° C., and heating the solder in the furnace to a molten state;
[0039] Step 5, preparing a soldering flux according to the mass fraction of 90% ZnCl2:10% NH4Cl, dissolving the soldering flux powder in anhydrous ethanol at a volume fraction of 1:1 to prepare the soldering flux;
[0040] Step 6, evenly apply flux to the surface of the polished, cleaned and dried Cu substrate, and place it together with the fixture in a muffle furnace for preheating, and the preheating temperature of the muffle furnace is 250° C.;
[0041] Step 7, after the preheating is completed, the temperature of the pit furnace is kept at 250°C, and the Cu5Zn8 diffusion barrier layer is prepared by the dip soldering method. The Cu substrate is clamped and fixed with a fixture, and vertically and uniformly immersed in the molten Sn-Zn solder. After the dip soldering, it is taken out vertically at a uniform speed, and air-cooled. The dip soldering time is 2s;
[0042] Step 8, after cooling, the sample is placed in an etching solution and ultrasonicated for 65 minutes at room temperature to remove excess solder on the surface until the off-white Cu5Zn8 diffusion barrier layer is completely exposed on the surface;
[0043] Step 9, using an X-ray diffractometer to perform XRD analysis on the Cu5Zn8 diffusion barrier layer prepared after dip solder etching, calibrate the composition of the generated coating, scan the surface of the sample in the range of 10°~90° at a scanning rate of 2° / min, and the scanning mode is θ / 2θ linkage. The Cu5Zn8 diffraction peak is observed and the composition is determined to be Cu5Zn8;
[0044] Step 10, after grinding and removing the oxide scale, the SnAgCu solder is ultrasonically cleaned with acetone, alcohol, and deionized water for 15 minutes, and then placed in a drying oven at a constant temperature of 41° C. for 22 minutes;
[0045] Step 11, the Cu substrate prepared with the Cu5Zn8 diffusion barrier layer is ultrasonically cleaned with acetone, alcohol, and deionized water for 15 minutes in sequence, and then placed in a drying oven at a constant temperature of 41° C. for drying for 22 minutes;
[0046] Step 12, applying flux on the surface of the Cu substrate prepared with the Cu5Zn8 diffusion barrier layer, and placing the cleaned and dried spherical SnAgCu solder flat in the center of the substrate;
[0047] Step 13: Place the structure in step 12 into a high temperature wetting angle measuring instrument and evacuate the sample chamber to 5×10 -5 Pa;
[0048] Step 14, set the heating program to start heating: first heat to 180°C at a heating rate of 8.5°C / min and keep warm for 5 minutes, then heat to 250°C at a heating rate of 6°C / min and keep warm for 1 minute. The wetting angle is measured by a high-resolution camera system at the side of the sample chamber combined with graphic analysis software. The wetting angle of the SnAgCu / Cu brazing system is 16.710 o , the wettability of the Cu / SnAgCu / Cu brazing system was improved, and the sample was cooled to room temperature with the furnace after heating;
[0049] Step 15, placing the Sn3.0Ag0.5Cu solder with a specification of 10 mm×10 mm×0.2 mm after grinding, cleaning and drying between two Cu substrates prepared with Cu5Zn8 diffusion barrier layers after cleaning and drying, to form a sandwich structure of Cu substrate with Cu5Zn8 diffusion barrier layer / SnAgCu solder / Cu substrate with Cu5Zn8 diffusion barrier layer;
[0050] Step 16: Place the assembled pre-welded parts into the furnace of the CMD-238 high vacuum brazing furnace and evacuate the furnace. When the vacuum degree reaches 5×10 -3 Pa, heating was started, and the temperature was heated to 180°C at a heating rate of 8.5°C / min and kept at that temperature for 5 min, and then heated to 250°C at a heating rate of 6°C / min and kept at that temperature for 1 min, and then cooled with the furnace, to obtain a brazed joint of the structure of Cu substrate / Cu5Zn8 diffusion barrier layer / SnAgCu solder / Cu5Zn8 diffusion barrier layer / Cu substrate;
[0051] Step 17, put the sample obtained in step 16 into the constant temperature zone of the VTCE-2585 atmosphere protection furnace, flush with argon gas with a purity of 99.99% and start heating to 160°C. After keeping the temperature for 240 hours, cool the furnace at a cooling rate of about 5-10°C / min. When the furnace temperature drops to room temperature, open the furnace door and take out the sample;
[0052] Step 18, cut the sample obtained in step 17 along the axis, grind the interface with four passes of SiC sandpaper of 400 Cw, 1000 Cw, 1500 Cw, and 2000 Cw, and then polish it to prepare a metallographic sample. The microstructure of the joint was observed by scanning electron microscope. The average thickness of the intermetallic compound at the interface was 9.287 μm, and the average thickness of Cu3Sn at the interface was 1.112 μm. The brazed joint of the Cu substrate with a 0.496 μm thick Cu5Zn8 diffusion barrier layer was prepared by brazing with SnAgCu solder for 2s.o The interface structure after aging for 240 hours is as follows Figure 1 The black part at the bottom of the figure is the Cu substrate, the gray-white part at the top is the SnAgCu solder, and the gray-black part between the two is the interface intermetallic compounds Cu6Sn5 and Cu3Sn. The average thickness of the interface intermetallic compound layer is 9.287μm, indicating that the excessive growth of intermetallic compounds (IMC) at the interface of the brazed joint during the aging stage is significantly suppressed.
[0053] Example 2
[0054] This embodiment is a Cu / SnAgCu / Cu brazing method based on the preparation of Cu5Zn8 diffusion barrier layer. In this embodiment, the excessive growth of intermetallic compounds (Cu6Sn5 and Cu3Sn) at the interface during the aging process is significantly suppressed in the Cu substrate prepared by the dip soldering method. The specifications of the Cu substrate involved are 10 mm×10 mm×2 mm, the SnAgCu solder is Sn3.0Ag0.5Cu, and the specifications for wetting are 1 mm×8 mm, the specification for brazing is 10 mm×10 mm×0.2 mm, and the composition of Sn-Zn solder used for preparing Cu5Zn8 diffusion barrier layer by dip soldering is 4 wt.% Zn, and the balance is Sn.
[0055] The specific process of this embodiment includes the following steps:
[0056] Step 1, the surface of the Sn-Zn solder is polished with two passes of SiC sandpaper of 240Cw and 400Cw in sequence to ensure that there is no oxide film on the surface, and then ultrasonically cleaned with acetone, alcohol, and deionized water for 18 minutes in sequence, and placed in a drying oven at a constant temperature of 42°C for drying for 24 minutes;
[0057] Step 2: The surface of a 10 mm × 10 mm Cu substrate was polished with four SiC sandpapers of 400 Cw, 1000 Cw, 1500 Cw, and 2000 Cw in sequence. The substrate was rotated 90° and polished again when the sandpaper was changed each time. After the polishing with 2000 Cw sandpaper was completed, the substrate was rotated 90° again and gently rubbed on the sandpaper to make a cross or grid scratch on the surface of the substrate. After the polishing was completed, ultrasonic cleaning was performed with acetone, alcohol, and deionized water for 18 minutes in sequence, and the substrate was placed in a drying oven with a constant temperature of 42°C for 24 minutes;
[0058] Step 3, rinse the experimental fixture, crucible and ceramic plate with anhydrous ethanol and place them in a drying oven at a constant temperature of 42°C for 24 minutes;
[0059] Step 4, placing the polished, cleaned and dried Sn-Zn solder in an alumina crucible and placing it in a pit furnace, setting the temperature of the pit furnace to 255° C., and heating the solder in the furnace to a molten state;
[0060] Step 5, preparing a soldering flux according to the mass fraction of 90% ZnCl2:10% NH4Cl, dissolving the soldering flux powder in anhydrous ethanol at a volume fraction of 1:1 to prepare the soldering flux;
[0061] Step 6, evenly apply flux to the surface of the polished, cleaned and dried Cu substrate, and place it together with the fixture in a muffle furnace for preheating, and the preheating temperature of the muffle furnace is 255° C.
[0062] Step 7, after preheating, keep the temperature of the pit furnace at 255°C unchanged, and prepare the Cu5Zn8 diffusion barrier layer by dip soldering. Use a fixture to clamp and fix the Cu substrate, and immerse it vertically and uniformly in the molten Sn-Zn solder. After dip soldering, take it out vertically and uniformly, and air cool it. The dip soldering time is 5s;
[0063] Step 8, after cooling, the sample is placed in an etching solution and ultrasonicated at room temperature for 75 minutes to remove excess solder on the surface until the off-white Cu5Zn8 diffusion barrier layer is completely exposed on the surface;
[0064] Step 9, using an X-ray diffractometer to perform XRD analysis on the Cu5Zn8 diffusion barrier layer prepared after dip solder etching, calibrate the composition of the generated coating, scan the surface of the sample in the range of 10°~90° at a scanning rate of 2° / min, and the scanning mode is θ / 2θ linkage. The Cu5Zn8 diffraction peak is observed and the composition is determined to be Cu5Zn8;
[0065] Step 10, after grinding and removing the oxide scale, the SnAgCu solder is ultrasonically cleaned with acetone, alcohol, and deionized water for 18 minutes, and placed in a drying oven at a constant temperature of 42° C. for 24 minutes;
[0066] Step 11, the Cu substrate prepared with the Cu5Zn8 diffusion barrier layer is ultrasonically cleaned with acetone, alcohol, and deionized water for 18 minutes in sequence, and then placed in a drying oven at a constant temperature of 42° C. for drying for 24 minutes;
[0067] Step 12, applying flux on the surface of the Cu substrate prepared with the Cu5Zn8 diffusion barrier layer, and placing the cleaned and dried spherical SnAgCu solder flat in the center of the substrate;
[0068] Step 13: Place the structure in step 12 into a high temperature wetting angle measuring instrument and evacuate the sample chamber to 5×10 -5 Pa;
[0069] Step 14, set the heating program to start heating: first heat to 180°C at a heating rate of 8.5°C / min and keep warm for 5 minutes, then heat to 250°C at a heating rate of 6°C / min and keep warm for 1 minute. The wetting angle is measured by using a high-resolution camera system at the side of the sample chamber combined with graphic analysis software. The wetting angle of the SnAgCu / Cu brazing system is 21.781 o , the wettability of the Cu / SnAgCu / Cu brazing system was improved, and the sample was cooled to room temperature with the furnace after heating;
[0070] Step 15, placing the Sn3.0Ag0.5Cu solder with a specification of 10 mm×10 mm×0.2 mm after grinding, cleaning and drying between two Cu substrates prepared with Cu5Zn8 diffusion barrier layers after cleaning and drying, to form a sandwich structure of Cu substrate with Cu5Zn8 diffusion barrier layer / SnAgCu solder / Cu substrate with Cu5Zn8 diffusion barrier layer;
[0071] Step 16: Place the assembled pre-welded parts into the furnace of the CMD-238 high vacuum brazing furnace and evacuate the furnace. When the vacuum degree reaches 5×10 -3 Pa, heating was started, and the temperature was heated to 180°C at a heating rate of 8.5°C / min and kept at that temperature for 5 min, and then heated to 250°C at a heating rate of 6°C / min and kept at that temperature for 1 min, and then cooled with the furnace, to obtain a brazed joint of the structure of Cu substrate / Cu5Zn8 diffusion barrier layer / SnAgCu solder / Cu5Zn8 diffusion barrier layer / Cu substrate;
[0072] Step 17, put the sample obtained in step 16 into the constant temperature zone of the VTCE-2585 atmosphere protection furnace, flush with argon gas with a purity of 99.99% and start heating to 160°C. After keeping the temperature for 240 hours, cool the furnace at a cooling rate of about 5-10°C / min. When the furnace temperature drops to room temperature, open the furnace door and take out the sample;
[0073] Step 18, cut the sample obtained in step 17 along the axis, grind the interface with four passes of SiC sandpaper of 400 Cw, 1000 Cw, 1500 Cw, and 2000 Cw, and then polish it to prepare a metallographic sample. The microstructure of the joint was observed by scanning electron microscope. The average thickness of the intermetallic compound at the interface was 6.847 μm, and the average thickness of Cu3Sn at the interface was 1.167 μm. The brazed joint of the Cu substrate with a 0.571 μm thick Cu5Zn8 diffusion barrier layer was prepared by brazing with SnAgCu solder for 5s. o The interface structure after aging for 240 hours is as follows Figure 2The black part at the bottom of the figure is the Cu substrate, the gray-white part at the top is the SnAgCu solder, and the gray-black part between the two is the interface intermetallic compounds Cu6Sn5 and Cu3Sn. The average thickness of the interface intermetallic compound layer is 6.847μm, indicating that the excessive growth of intermetallic compounds (IMC) at the interface of the brazed joint during the aging stage is significantly suppressed.
[0074] Example 3
[0075] This embodiment is a method for improving the wettability of a SnAgCu / Cu soldering system based on a Cu5Zn8 diffusion barrier layer. The Cu substrate involved has a specification of 10 mm×10 mm×2 mm, the SnAgCu solder is Sn3.0Ag0.5Cu, and the wettability is 1 mm×8 mm, the specification for brazing is 10 mm×10 mm×0.2 mm, and the composition of Sn-Zn solder used for preparing Cu5Zn8 diffusion barrier layer by dip soldering is 4 wt.% Zn, and the balance is Sn.
[0076] The specific process of this embodiment includes the following steps:
[0077] Step 1, the surface of the Sn-Zn solder is polished with two passes of SiC sandpaper of 240Cw and 400Cw in sequence to ensure that there is no oxide film on the surface, and then ultrasonically cleaned with acetone, alcohol, and deionized water for 20 minutes in sequence, and placed in a drying oven at a constant temperature of 41°C for drying for 23 minutes;
[0078] Step 2, the surface of a 10 mm×10 mm Cu substrate was polished with four SiC sandpapers of 400 Cw, 1000 Cw, 1500 Cw, and 2000 Cw in sequence. The substrate was rotated 90° and polished again when the sandpaper was changed each time. After the 2000 Cw sandpaper was polished, the substrate was rotated 90° again and gently rubbed on the sandpaper to make a cross or grid scratch on the surface of the substrate. After the polishing was completed, acetone, alcohol, and deionized water were used for ultrasonic cleaning for 20 minutes in sequence, and the substrate was placed in a drying oven with a constant temperature of 41°C for drying for 23 minutes;
[0079] Step 3, rinse the experimental fixture, crucible and ceramic plate with anhydrous ethanol and place them in a drying oven at a constant temperature of 41°C for 23 minutes;
[0080] Step 4, placing the polished, cleaned and dried Sn-Zn solder in an alumina crucible and placing it in a pit furnace, setting the temperature of the pit furnace to 260° C., and heating the solder in the furnace to a molten state;
[0081] Step 5, preparing a soldering flux according to the mass fraction of 90% ZnCl2:10% NH4Cl, dissolving the soldering flux powder in anhydrous ethanol at a volume fraction of 1:1 to prepare the soldering flux;
[0082] Step 6, evenly apply flux to the surface of the polished, cleaned and dried Cu substrate, and place it together with the fixture in a muffle furnace for preheating, and the preheating temperature of the muffle furnace is 260° C.;
[0083] Step 7, after the preheating is completed, the temperature of the pit furnace is kept at 260°C, and the Cu5Zn8 diffusion barrier layer is prepared by the dip soldering method. The Cu substrate is clamped and fixed with a fixture, and vertically and uniformly immersed in the molten Sn-Zn solder. After the dip soldering, it is taken out vertically at a uniform speed and air-cooled. The dip soldering time is 10s;
[0084] Step 8, after cooling, the sample is placed in an etching solution and ultrasonicated for 85 minutes at room temperature to remove excess solder on the surface until the off-white Cu5Zn8 diffusion barrier layer is completely exposed on the surface;
[0085] Step 9, using an X-ray diffractometer to perform XRD analysis on the Cu5Zn8 diffusion barrier layer prepared after dip solder etching, calibrate the composition of the generated coating, scan the surface of the sample in the range of 10°~90° at a scanning rate of 2° / min, and the scanning mode is θ / 2θ linkage. The Cu5Zn8 diffraction peak is observed and the composition is determined to be Cu5Zn8;
[0086] Step 10, after grinding and removing the oxide scale, the SnAgCu solder is ultrasonically cleaned with acetone, alcohol, and deionized water for 20 minutes, and placed in a drying oven at a constant temperature of 41° C. for 23 minutes;
[0087] Step 11, the Cu substrate prepared with the Cu5Zn8 diffusion barrier layer is ultrasonically cleaned with acetone, alcohol, and deionized water for 20 minutes in sequence, and then placed in a drying oven at a constant temperature of 41° C. for drying for 23 minutes;
[0088] Step 12, applying flux on the surface of the Cu substrate prepared with the Cu5Zn8 diffusion barrier layer, and placing the cleaned and dried spherical SnAgCu solder flat in the center of the substrate;
[0089] Step 13: Place the structure in step 12 into a high temperature wetting angle measuring instrument and evacuate the sample chamber to 5×10 -5 Pa;
[0090] Step 14, set the heating program to start heating: first heat to 180°C at a heating rate of 8.5°C / min and keep warm for 5 minutes, then heat to 250°C at a heating rate of 6°C / min and keep warm for 1 minute. The wetting angle is measured by using a high-resolution camera system at the side of the sample chamber combined with graphic analysis software. The wetting angle of the SnAgCu / Cu brazing system is 21.161 o ,like Figure 3 As shown, the wettability of the Cu / SnAgCu / Cu brazing system is improved. After the sample is heated, it is cooled to room temperature in the furnace.
[0091] Step 15, placing the Sn3.0Ag0.5Cu solder with a specification of 10 mm×10 mm×0.2 mm after grinding, cleaning and drying between two Cu substrates prepared with Cu5Zn8 diffusion barrier layers after cleaning and drying, to form a sandwich structure of Cu substrate with Cu5Zn8 diffusion barrier layer / SnAgCu solder / Cu substrate with Cu5Zn8 diffusion barrier layer;
[0092] Step 16: Place the assembled pre-welded parts into the furnace of the CMD-238 high vacuum brazing furnace and evacuate the furnace. When the vacuum degree reaches 5×10 -3 Pa, heating was started, and the temperature was heated to 180°C at a heating rate of 8.5°C / min and kept at that temperature for 5 min, and then heated to 250°C at a heating rate of 6°C / min and kept at that temperature for 1 min, and then cooled with the furnace, to obtain a brazed joint of the structure of Cu substrate / Cu5Zn8 diffusion barrier layer / SnAgCu solder / Cu5Zn8 diffusion barrier layer / Cu substrate;
[0093] Step 17, put the sample obtained in step 16 into the constant temperature zone of the VTCE-2585 atmosphere protection furnace, flush with argon gas with a purity of 99.99% and start heating to 160°C. After keeping the temperature for 240 hours, cool the furnace at a cooling rate of about 5-10°C / min. When the furnace temperature drops to room temperature, open the furnace door and take out the sample;
[0094] Step 18, cut the sample obtained in step 17 along the axis, grind the interface with four passes of SiC sandpaper of 400 Cw, 1000 Cw, 1500 Cw, and 2000 Cw, and then polish it to prepare a metallographic sample. The microstructure of the joint was observed by scanning electron microscope. The average thickness of the intermetallic compound at the interface was 7.754 μm, and the average thickness of Cu3Sn at the interface was 1.111 μm. The brazed joint of the Cu substrate with a 0.674 μm thick Cu5Zn8 diffusion barrier layer was prepared by brazing with SnAgCu solder for 10s. o The interface structure after aging for 240 hours is as follows Figure 4The black part at the bottom of the figure is the Cu substrate, the gray-white part at the top is the SnAgCu solder, and the gray-black part between the two is the interface intermetallic compounds Cu6Sn5 and Cu3Sn. The average thickness of the interface intermetallic compound layer is 7.754μm, indicating that the excessive growth of the interface intermetallic compound (IMC) of the brazed joint during the aging stage is significantly suppressed.
[0095] The above are only embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application should be included within the scope of the claims of the present application.
Claims
1. A Cu / SnAgCu / Cu brazing method based on the preparation of Cu5Zn8 diffusion barrier layer, characterized in that: Taking the Cu / SnAgCu / Cu brazing system composed of SnAgCu solder and Cu substrate as the object, a Cu5Zn8 diffusion barrier layer is prepared on the surface of the Cu substrate, and then the Cu substrate prepared with the Cu5Zn8 diffusion barrier layer is brazed by using SnAgCu solder to obtain a brazed joint of the structure of Cu substrate / Cu5Zn8 diffusion barrier layer / SnAgCu solder / Cu5Zn8 diffusion barrier layer / Cu substrate. The specific process includes the following steps: Step 1, placing the polished, cleaned and dried Sn-Zn solder in a crucible and placing it in a pit furnace, setting the temperature of the pit furnace to 245-265° C., and heating the solder in the furnace to a molten state; Step 2, preparing a soldering flux according to the mass fraction of 90% ZnCl2:10% NH4Cl, and dissolving the soldering flux powder in anhydrous ethanol at a volume fraction of 1:1; Step 3, evenly apply flux to the surface of the polished, cleaned and dried Cu substrate, and place it together with the fixture in a muffle furnace for preheating; Step 4, use a fixture to clamp and fix the Cu substrate, immerse it vertically and uniformly in the molten Sn-Zn solder, take it out vertically and uniformly after dip soldering, and air cool it. The dip soldering time is 2 to 30 seconds; Step 5, after cooling, the sample is placed in an etching solution and ultrasonicated at room temperature for 60 to 90 minutes to remove excess solder on the surface until the off-white Cu5Zn8 diffusion barrier layer is completely exposed on the surface; Step 6, placing the polished, cleaned and dried SnAgCu solder between two cleaned and dried Cu substrates prepared with Cu5Zn8 diffusion barrier layers to form a sandwich structure of Cu substrate with Cu5Zn8 diffusion barrier layer / SnAgCu solder / Cu substrate with Cu5Zn8 diffusion barrier layer; Step 7, placing the assembled pre-welded parts into a high vacuum brazing furnace for brazing connection to obtain a brazed joint of the structure of Cu substrate / Cu5Zn8 diffusion barrier layer / SnAgCu solder / Cu5Zn8 diffusion barrier layer / Cu substrate.
2. The Cu / SnAgCu / Cu brazing method according to claim 1, characterized in that: The composition of the Sn-Zn solder is 3-12 wt.% Zn, with the balance being Sn.
3. The Cu / SnAgCu / Cu brazing method according to claim 1, characterized in that: The composition of the SnAgCu solder is Sn3.0Ag0.5Cu.
4. The Cu / SnAgCu / Cu brazing method according to claim 1, characterized in that: The crucible in step 1 is an alumina crucible.
5. The Cu / SnAgCu / Cu brazing method according to claim 1, characterized in that: The grinding, cleaning and drying treatment described in step 1 is to grind the Sn-Zn solder, then ultrasonically clean it with acetone, alcohol and deionized water for 15 to 20 minutes, and dry it in a drying oven at a constant temperature of 40 to 50° C. for 20 to 30 minutes.
6. The Cu / SnAgCu / Cu brazing method according to claim 1, characterized in that: The preheating temperature of the muffle furnace described in step 3 is 245~265℃.
7. The Cu / SnAgCu / Cu brazing method according to claim 1, characterized in that: The grinding, cleaning and drying treatment described in step 3 is to grind the Cu substrate, then ultrasonically clean it with acetone, alcohol and deionized water for 15 to 20 minutes, and dry it in a drying oven at a constant temperature of 40 to 50° C. for 20 to 30 minutes.
8. The Cu / SnAgCu / Cu brazing method according to claim 1, characterized in that: The SnAgCu solder after the grinding, cleaning and drying treatment in step 6 is that the SnAgCu solder is ground, ultrasonically cleaned with acetone, alcohol and deionized water for 15 to 20 minutes in sequence, and placed in a drying oven at a constant temperature of 40 to 50° C. for 20 to 30 minutes.
9. The Cu / SnAgCu / Cu brazing method according to claim 1, characterized in that: The cleaning and drying treatment of the Cu substrate prepared with the Cu5Zn8 diffusion barrier layer described in step 6 is to ultrasonically clean it with acetone, alcohol and deionized water for 15 to 20 minutes in sequence, and then put it in a drying oven at a constant temperature of 40 to 50°C for drying for 20 to 30 minutes.
10. The Cu / SnAgCu / Cu brazing method according to claim 1, characterized in that: The brazing connection in the high vacuum brazing furnace described in step 7 is carried out in a CMD-238 high vacuum brazing furnace. When the vacuum degree reaches 5×10 -3 Pa, start heating, heat to 180℃ at a heating rate of 8.5℃ / min and keep warm for 5min, then heat to 250℃ at a heating rate of 6℃ / min and keep warm for 1min, then cool with the furnace.