High-strength composite board welding method
Through galvanomic laser-arc composite welding and pulse laser induced arc composite welding technology, the interface structure of high-strength composite panels is optimized, and the residual stress and layering problems of high-strength steel/stainless steel interface are solved, and the welding strength and corrosion resistance are improved. Application scope.
Patent Information
- Application Number
- CN202411098825.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-19
AI Technical Summary
After welding of high-strength composite plates, there is a large residual stress on the interface of high-strength steel/stainless steel, which is prone to interface layering, which affects the welding strength and corrosion resistance.
The galvanometer laser-arc composite welding method and the galvanometer pulse laser induced arc composite welding method are adopted to design the welding wire components and interface structure. Through the single-pulse laser energy and laser swing characteristics, a serrated high-strength steel/stainless steel special-shaped interface is formed to reduce interface residues. Stress and stratification phenomena.
It improves the interface bonding strength of high-strength composite boards, reduces heat input, enhances the metallurgical and physical connection characteristics of welding, and expands the application range of high-strength composite board connections.
Smart Images

Figure CN118976993A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a welding method, in particular to a high-strength composite plate welding method. Background Art
[0002] The rapid development of the domestic economy has driven the upgrading and reconstruction of railways and highways, among which the construction of steel structure bridges is an important part of railway and highway construction. At present, the construction of steel structure bridges in my country has selected steel grades with higher strength levels to replace steel grades with lower strength levels, and is gradually realizing the rapid upgrading of steel structure bridges. Since the corrosion performance of steel structure bridges is greatly affected by the environment, traditional paint anti-corrosion can no longer meet the service life of bridges. The composite plate composed of high-strength steel plates and stainless steel plates not only maintains the original strength, plasticity, good weldability, and fatigue resistance of high-strength steel, but also has the good corrosion resistance of stainless steel, providing important technical support for improving the corrosion resistance life of steel structure bridges.
[0003] However, after the bridge is welded with high-strength composite plates, there is a large residual stress at the high-strength steel / stainless steel interface, and problems such as high-strength steel / stainless steel interface delamination are prone to occur. Summary of the invention
[0004] Purpose of the invention: The purpose of the invention is to provide a high-strength composite plate welding method to improve the interface bonding strength of the high-strength composite plate.
[0005] Technical solution: The present invention comprises the following steps: processing the groove of the high-strength composite steel plate; selecting solid welding wire for the base layer bottom welding of the high-strength composite steel plate, and adopting the galvanometer laser-arc composite welding method; selecting flux-cored welding wire for the base layer filling welding, and adopting the galvanometer laser-arc composite welding method; selecting welding wire with the same or similar composition and performance as the coating for the interface filling welding of the high-strength composite plate, and adopting the galvanometer pulse laser induced arc composite welding; selecting welding wire with the same or similar composition and performance as the coating for the coating cover welding, and adopting the galvanometer laser-arc composite welding method.
[0006] The interface is a serrated high-strength steel / stainless steel special-shaped interface.
[0007] The high-strength composite steel plates are butt-welded, and the bottoms of the high-strength composite steel plates are aligned during welding.
[0008] The high-strength composite steel plate comprises a base layer and a cladding layer.
[0009] The base layer is made of high-strength steel, and the cladding layer is made of stainless steel.
[0010] The high-strength composite plate is welded using a narrow gap groove, such as a U-shaped or I-shaped groove.
[0011] Before the interface filling welding, the upper surface of the base layer after the filling welding is 0.5 to 1.5 mm away from the high-strength steel / stainless steel interface. After the high-strength steel / stainless steel interface filling welding, the upper surface of the cladding stainless steel is 0.5 to 1.5 mm away from the high-strength steel / stainless steel interface.
[0012] In the galvanometer laser-arc hybrid welding method, the laser power is 600-6000W, the laser swing width is 0-20mm, the arc current is 150-300A, and the welding speed is 8-15mm / s.
[0013] During the galvanometer pulse laser induced arc hybrid welding, the galvanometer pulse laser peak power is 3000-10000W, the laser scanning width is 0-20mm, the galvanometer pulse laser frequency is 100-300Hz, the welding speed is 8-15mm / s, and the arc current is 150-300A.
[0014] During the base layer filling welding and the cladding layer capping welding, the interlayer temperature is controlled at 40-100°C.
[0015] Beneficial effects: The present invention designs the welding wire composition, optimizes the interface structure, and adopts a galvanometer pulse laser induced arc composite welding method to reduce the residual stress at the high-strength steel / stainless steel interface while reducing heat input. The high energy of a single-pulse laser and the swingable laser are used to obtain a serrated high-strength steel / stainless steel special-shaped interface at the interface, reduce the stratification phenomenon at the high-strength steel / stainless steel interface, and provide data support for the precise control of high-strength composite plate welding. This method overcomes many shortcomings of the prior art, has the characteristics of controllable alloy composition, and the interface takes into account the characteristics of both metallurgical and physical connections, which is convenient for improving the interface bonding strength of high-strength composite plates and expanding the application range of high-strength composite plate connections. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a schematic diagram of the weld filling and interface structure of the high-strength composite plate of the present invention. DETAILED DESCRIPTION
[0017] The present invention will be further described below in conjunction with the accompanying drawings.
[0018] The high-strength composite plate welding method of the present invention is aimed at composite plates with large differences in alloy composition and physical property parameters, such as S31603+Q420qE composite plates, S31603+Q500qE composite plates and S31603+Q690qE composite plates. By designing the welding wire composition and optimizing the interface structure, a galvanometer pulse laser induced arc composite welding method is adopted to reduce heat input while utilizing the high energy of a single pulse laser and the swingability of the laser to obtain a serrated high-strength steel / stainless steel special-shaped interface at the interface, thereby providing data support for the precise control of high-strength composite plate welding.
[0019] The welding sequence of high-strength composite steel plates is: first perform base welding, then fill the base high-strength steel, and finally use welding wire with the same or similar composition and performance as the cladding to fill the high-strength steel / stainless steel interface and cladding. The high-strength composite plate welding method adopts galvanometer continuous laser-arc composite welding and galvanometer pulse laser induced arc composite welding. The swing of the galvanometer laser during welding can promote the fusion of the side walls on the one hand, and the stirring effect of the galvanometer laser can improve the weld formation quality on the other hand. For the base welding and filling of the high-strength composite plate, galvanometer continuous laser-arc composite welding is adopted, while galvanometer pulse laser induced arc composite welding is adopted for the filling welding of the high-strength steel / stainless steel interface, and galvanometer continuous laser-arc composite welding is adopted for the cladding filling welding. Specifically, the following steps are included:
[0020] S1. Processing the groove of high-strength composite steel plate
[0021] High-strength composite steel plates include a base layer and a cladding layer. The base layer is made of high-strength steel, such as Q420qE, Q500qE or Q690qE, and the cladding layer is made of stainless steel, such as austenitic stainless steel. High-strength composite plate welding uses narrow gap grooves, such as U-shaped or I-shaped grooves; the bottom blunt edge of the U-shaped groove is 3 to 6 mm, the blunt edge arc radius is 4 to 10 mm, and the groove angle is 0 to 3°; the back of the I-shaped groove is added with ceramic precipitation, and the groove angle is 0 to 5°;
[0022] S2. The high-strength composite steel plate is butt-welded and fixed by a special fixture, and the bottom of the high-strength composite steel plate is aligned;
[0023] S3. For base layer welding, solid welding wire with good crack resistance is selected, and the galvanometer laser-arc hybrid welding method is adopted. The laser power is 600-6000W, the laser swing width is 0-20mm, the arc current is 150-300A, and the welding speed is 8-15mm / s;
[0024] S4, base layer high-strength steel filling welding, select flux-cored wire with low carbon content, and adopt galvanometer laser-arc hybrid welding method, the interlayer temperature is controlled at 40-100℃, the laser power is 600-6000W, the laser swing width is 0-20mm, the arc current is 150-300A, and the welding speed is 8-15mm / s;
[0025] S5. Before the high-strength steel / stainless steel interface filling welding, the upper surface position of the base layer after the filling welding is 0.5 to 1.5 mm away from the high-strength steel / stainless steel interface. After the high-strength steel / stainless steel interface filling welding, the upper surface of the cladding stainless steel is 0.5 to 1.5 mm away from the high-strength steel / stainless steel interface.
[0026] S6. When filling welding the high-strength steel / stainless steel interface of high-strength composite plates, select welding wire with the same or similar composition and performance as the cladding stainless steel, use galvanometer pulse laser induced arc composite welding, the galvanometer pulse laser peak power is 3000-10000W, the laser scanning width is 0-20mm, the galvanometer pulse laser frequency is 100-300Hz, the welding speed is 8-15mm / s, and the arc current is 150-300A; When filling welding the high-strength steel / stainless steel interface of high-strength composite plates, the periodic light emission of pulse laser and the high energy density of single pulse laser are utilized, and in the process of periodic swing of laser along the high-strength steel / stainless steel interface, a serrated high-strength steel / stainless steel special-shaped interface is obtained near the interface;
[0027] S7. When welding the cladding stainless steel cap, choose welding wire with the same or similar composition and performance as the cladding stainless steel, and adopt the galvanometer laser-arc composite welding method. The interlayer temperature is controlled at 40-100°C, the laser power is 600-6000W, the laser swing width is 0-20mm, the arc current is 150-300A, and the welding speed is 8-15mm / s.
[0028] Example 1
[0029] This embodiment uses S31603+Q500qE high-strength composite steel plate, the thickness of the base Q500qE high-strength steel is 24.0mm, and the thickness of the cladding S31603 stainless steel plate is 3.0mm. Specifically, the following steps are included:
[0030] The first step is to process the groove of S31603+Q500qE high-strength composite steel plate. The bottom blunt edge of the U-shaped groove is 4mm, the radius of the blunt edge arc is 5mm, and the groove angle is 1°; Figure 1 As shown;
[0031] Step 2: The S31603+Q500qE high-strength composite steel plate is butt-welded and fixed with a special fixture to align the bottom of the high-strength composite steel plate;
[0032] Step 3: For the base layer welding, G69A4M21ZN2M4T solid welding wire with good crack resistance is selected, and the galvanometer laser-arc hybrid welding method is adopted. The laser power is 3000W, the laser swing width is 0.2mm, the arc current is 180A, and the welding speed is 8mm / s.
[0033] Step 4: For the base Q500qE high-strength steel filling welding, T624T1-1C1A-GXU flux-cored welding wire with low carbon content is selected, and the galvanometer laser-arc hybrid welding method is adopted. The interlayer temperature is controlled at 40-100°C, the laser power is 3000W, the laser swing width is 9mm, the arc current is 180A, and the welding speed is 10mm / s;
[0034] Step 5. Before the high-strength steel / stainless steel interface filling welding, the upper surface position of the base layer after the filling welding is 1mm away from the high-strength steel / stainless steel interface. After the high-strength steel / stainless steel interface filling welding, the upper surface of the cladding stainless steel is 1mm away from the high-strength steel / stainless steel interface.
[0035] Step 6. When filling the high-strength steel / stainless steel interface of the high-strength composite plate, select TS316LMo-FC11 welding wire, adopt galvanometer pulse laser induced arc hybrid welding, the galvanometer pulse laser peak power is 8000W, the laser scanning width is 9mm, the galvanometer pulse laser frequency is 150Hz, the welding speed is 10mm / s, and the arc current is 180A;
[0036] Step 7. When welding the cladding S31603 stainless steel cap, use TS316LMo-FC11 welding wire and adopt the galvanometer laser-arc hybrid welding method. The interlayer temperature is controlled at 40-100°C, the laser power is 3000W, the laser swing width is 10mm, the arc current is 180A, and the welding speed is 10mm / s.
[0037] The S31603+Q500qE high-strength composite steel plate was welded using galvanometer laser-arc hybrid welding and galvanometer pulse laser induced arc hybrid welding methods to obtain a better joint, the tensile strength of the joint was greater than 650MPa and the elongation was close to 20%.
[0038] Example 2
[0039] This embodiment uses S31603+Q420qE high-strength composite steel plate, the base Q420qE high-strength steel thickness is 24.0mm, and the cladding S31603 stainless steel plate thickness is 3.0mm. Specifically, the following steps are included:
[0040] The first step is to process the groove of S31603+Q420qE high-strength composite steel plate. The bottom blunt edge of the U-shaped groove is 5mm, the radius of the blunt edge arc is 6mm, and the groove angle is 2°;
[0041] Step 2: The S31603+Q420qE high-strength composite steel plate is butt-welded and fixed with a special fixture to align the bottom of the high-strength composite steel plate;
[0042] Step 3: For the base layer welding, G69A4M21ZN2M4T solid welding wire with good crack resistance is selected, and the galvanometer laser-arc hybrid welding method is adopted. The laser power is 4000W, the laser swing width is 0.3mm, the arc current is 200A, and the welding speed is 10mm / s.
[0043] Step 4: For the base Q420qE high-strength steel filling welding, T624T1-1C1A-GXU flux-cored welding wire with low carbon content is selected, and the galvanometer laser-arc hybrid welding method is adopted. The interlayer temperature is controlled at 40-100°C, the laser power is 4000W, the laser swing width is 10mm, the arc current is 200A, and the welding speed is 12mm / s;
[0044] Step 5. Before the high-strength steel / stainless steel interface filling welding, the upper surface position of the base layer after the filling welding is 1.2mm away from the high-strength steel / stainless steel interface. After the high-strength steel / stainless steel interface filling welding, the upper surface of the cladding stainless steel is 1.2mm away from the high-strength steel / stainless steel interface.
[0045] Step 6. When filling the high-strength steel / stainless steel interface of the high-strength composite plate, select TS316LMo-FC11 welding wire, adopt galvanometer pulse laser induced arc hybrid welding, the galvanometer pulse laser peak power is 9000W, the laser scanning width is 10mm, the galvanometer pulse laser frequency is 180Hz, the welding speed is 12mm / s, and the arc current is 200A;
[0046] Step 7. When welding the cladding S31603 stainless steel cap, use TS316LMo-FC11 welding wire and adopt the galvanometer laser-arc hybrid welding method. The interlayer temperature is controlled at 40-100°C, the laser power is 4000W, the laser swing width is 10mm, the arc current is 200A, and the welding speed is 12mm / s.
[0047] The S31603+Q420qE high-strength composite steel plate was welded using galvanometer laser-arc hybrid welding and galvanometer pulse laser induced arc hybrid welding methods to obtain a better joint, the tensile strength of the joint was greater than 650MPa and the elongation was close to 20%.
[0048] Example 3
[0049] This embodiment uses S31603+Q690qE high-strength composite steel plate, the base Q690qE high-strength steel thickness is 24.0mm, and the cladding S31603 stainless steel plate thickness is 3.0mm. Specifically, the following steps are included:
[0050] The first step is to process the groove of S31603+Q690qE high-strength composite steel plate, add ceramic precipitation on the back of the I-type groove, and the groove angle is 2°;
[0051] Step 2: The S31603+Q690qE high-strength composite steel plate is butt-welded and fixed with a special fixture to align the bottom of the high-strength composite steel plate;
[0052] Step 3: For the base layer welding, G69A4M21ZN2M4T solid welding wire with good crack resistance is selected, and the galvanometer laser-arc hybrid welding method is adopted. The laser power is 4000W, the laser swing width is 0.3mm, the arc current is 200A, and the welding speed is 10mm / s.
[0053] Step 4: For the base Q690qE high-strength steel filling welding, T624T1-1C1A-GXU flux-cored welding wire with low carbon content is selected, and the galvanometer laser-arc hybrid welding method is adopted. The interlayer temperature is controlled at 40-100°C, the laser power is 4000W, the laser swing width is 10mm, the arc current is 200A, and the welding speed is 12mm / s;
[0054] Step 5. Before the high-strength steel / stainless steel interface filling welding, the upper surface position of the base layer after the filling welding is 1.2mm away from the high-strength steel / stainless steel interface. After the high-strength steel / stainless steel interface filling welding, the upper surface of the cladding stainless steel is 1.2mm away from the high-strength steel / stainless steel interface.
[0055] Step 6. When filling the high-strength steel / stainless steel interface of the high-strength composite plate, select TS316LMo-FC11 welding wire, adopt galvanometer pulse laser induced arc hybrid welding, the galvanometer pulse laser peak power is 9000W, the laser scanning width is 10mm, the galvanometer pulse laser frequency is 180Hz, the welding speed is 12mm / s, and the arc current is 200A;
[0056] Step 7. When welding the cladding S31603 stainless steel cap, use TS316LMo-FC11 welding wire and adopt the galvanometer laser-arc hybrid welding method. The interlayer temperature is controlled at 40-100°C, the laser power is 4000W, the laser swing width is 10mm, the arc current is 200A, and the welding speed is 12mm / s.
[0057] The S31603+Q690qE high-strength composite steel plate was welded using galvanometer laser-arc hybrid welding and galvanometer pulse laser induced arc hybrid welding methods to obtain a better joint, the tensile strength of the joint was greater than 650MPa and the elongation was close to 20%.
Claims
1. A high-strength composite plate welding method, characterized in that: The method comprises the following steps: processing the groove of the high-strength composite steel plate; selecting solid welding wire for base layer bottom welding of the high-strength composite steel plate, and adopting a galvanometer laser-arc composite welding method; selecting flux-cored welding wire for base layer filling welding, and adopting a galvanometer laser-arc composite welding method; selecting welding wire with the same composition and performance as the cladding layer for interface filling welding of the high-strength composite plate, and adopting a galvanometer pulse laser induced arc composite welding; selecting welding wire with the same composition and performance as the cladding layer for cladding cover welding, and adopting a galvanometer laser-arc composite welding method.
2. A high-strength composite plate welding method according to claim 1, characterized in that: The interface is a sawtooth-shaped special-shaped interface.
3. A high-strength composite plate welding method according to claim 1, characterized in that: The high-strength composite steel plates are butt-welded, and the bottoms of the high-strength composite steel plates are aligned during welding.
4. A high-strength composite plate welding method according to claim 1 or 3, characterized in that: The high-strength composite steel plate comprises a base layer and a cladding layer.
5. A high-strength composite plate welding method according to claim 4, characterized in that: The base layer is made of high-strength steel, and the cladding layer is made of stainless steel.
6. A high-strength composite plate welding method according to claim 5, characterized in that: The high-strength composite plate is welded using a narrow gap groove.
7. A high-strength composite plate welding method according to claim 1, characterized in that: Before the interface filling welding, the upper surface of the base layer after the filling welding is 0.5 to 1.5 mm away from the interface. After the interface filling welding, the upper surface of the cladding layer is 0.5 to 1.5 mm away from the interface.
8. A high-strength composite plate welding method according to claim 1, characterized in that: In the galvanometer laser-arc hybrid welding method, the laser power is 600-6000W, the laser swing width is 0-20mm, the arc current is 150-300A, and the welding speed is 8-15mm / s.
9. A high-strength composite plate welding method according to claim 1, characterized in that: During the galvanometer pulse laser induced arc hybrid welding, the galvanometer pulse laser peak power is 3000-10000W, the laser scanning width is 0-20mm, the galvanometer pulse laser frequency is 100-300Hz, the welding speed is 8-15mm / s, and the arc current is 150-300A.
10. A high-strength composite plate welding method according to claim 1, characterized in that: During the base layer filling welding and the cladding layer capping welding, the interlayer temperature is controlled at 40-100°C.