Welding method for 1900 MPa-grade low-alloy ultrahigh-strength steel high-pressure vessel shell
By combining tungsten inert gas welding and vacuum quenching, the problems of insufficient tensile strength and welding defects in high-pressure vessel shell materials were solved, and the high-performance and high-precision 1900MPa grade low alloy ultra-high strength steel high-pressure vessel shells were prepared.
Patent Information
- Application Number
- CN202410656995.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-24
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-05-24
AI Technical Summary
Existing technologies are insufficient to manufacture high-pressure vessel shells that meet the performance and precision requirements of 1900MPa, mainly due to insufficient tensile strength of materials, defects easily caused by welding processes, and decarburization layers and poor surface cleanliness resulting from heat treatment.
The method of tungsten inert gas welding combined with vacuum quenching is adopted. By strictly controlling the welding parameters and shielding gas, the quality of the weld is ensured. The material properties are improved by vacuum quenching, cold treatment and two tempering treatments, so as to achieve the tensile strength and precision of the high-pressure vessel shell.
The preparation of high-pressure vessel shells made of 1900MPa grade low alloy ultra-high strength steel was achieved. The tensile strength of the weld reached over 1900MPa, the straightness was less than 2mm per meter, and the surface finish was good, meeting the performance and precision requirements of high-pressure vessels.
Smart Images

Figure CN118977060A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of mechanical processing, in particular to a welding method for a 1900MPa-grade low-alloy ultra-high-strength steel shell. Background Art
[0002] The steel high-pressure container shells used in the machinery industry are generally made of high-strength steel materials such as 30CrMnSiA and D406A. The general preparation process is: gather typical high-pressure container welding parts such as the front head, cylinder, and rear head, among which the front head and rear head are formed by mechanical processing, and the cylinder is formed by strong spinning, and the welding parts are formed respectively; the welding parts are combined and formed by argon arc welding, and then the whole is tempered in an air heat treatment furnace, and finally mechanically processed to prepare the high-pressure container shell. The tensile strength of the weld of this type of steel high-pressure container shell is generally lower than 1600MPa, and the product shape and position accuracy is poor, and the straightness is generally more than 2mm per meter, which cannot meet the performance and accuracy requirements of the 1900MPa high-pressure container shell. The main reasons are: 1. The materials used cannot reach the required tensile strength after heat treatment; 2. The traditional welding process parameters are difficult to match and easily cause defects such as cracks and pores, resulting in subsequent performance failing to meet the requirements; 3. The heat treatment process uses an ordinary air furnace. During the heat treatment process, the inner and outer surfaces of the high-pressure container shell react with oxygen and other gases in the air to produce a certain proportion of decarburization layer, resulting in a decrease in the performance of the high-pressure container shell weld. At the same time, the surface cleanliness of the shell is poor after heat treatment, and further sandblasting and other treatments are required to meet the surface cleanliness requirements. The shell is severely deformed and requires strong shape correction treatment to meet the requirements.
[0003] The invention patent ZL202210420958.0 discloses an efficient production method for 1900MPa grade suspension spring steel. The method relates to the field of iron and steel metallurgy technology. By optimizing the spring steel production process, the central shrinkage cavity of the ingot is eliminated, the central segregation of the ingot is improved, and the ingot opening process of the continuous casting large square billet with high temperature and long time heating and the billet peeling and finishing process after opening are omitted. After the continuous casting billet passes the flaw detection, it is rolled into the required 1900MPa grade suspension spring high-quality spring steel hot-rolled coil wire product through rough rolling, pre-finishing rolling and finishing rolling units, which meets the processing and use requirements of automobile suspension springs and shortens the processing flow and production time. The method only involves smelting and casting to make billets and then rolling them into spring steel wire. The spring steel wire is used to make elastic elements. Due to its material properties, it cannot be welded or spun, which is irrelevant to the welding method of the high-pressure vessel shell described in this article.
[0004] The invention patent ZL 202010670350.4 discloses a 1900MPa-grade high-strength and toughness aluminum-silicon coated steel plate for hot stamping and a welding method thereof. The 1900MPa-grade high-strength and toughness aluminum-silicon coated steel plate for hot stamping, a composite steel plate comprising a steel substrate and an aluminum-silicon coating. The tensile strength is improved through the hot stamping process. It is a welding method for high-performance composite steel plates. Since the aluminum-silicon coating is mixed with steel on its surface and multiple components are mixed, it cannot be welded and is not related to the production of container products.
[0005] The invention patent ZL 201810454283.5 discloses a 1900MPa grade ultra-high strength alloy steel welding flux-cored wire, which involves the field of welding materials in material processing. In order to ensure that the alloy has high strength and toughness, the carbon content in the flux-cored wire is strictly controlled, and elements such as titanium, vanadium, molybdenum, and cobalt are added with scientifically optimized proportions to improve the strength and high-temperature strength of the welding flux core. It is a new type of flux-cored wire and has nothing to do with the welding method in this article.
[0006] In November 2011, Pei Jian published "Effect of Ni Content and Tempering Process on the Structure and Properties of 300M Steel" (Issue 11, 2011) at Yanshan University. In order to improve the toughness of 300M steel, the content of toughening element Ni was adjusted to study the influence of Ni content on the continuous cooling transformation, microstructural evolution and mechanical properties of 300M steel. The influence of high Ni content on the structure and properties of 300M steel was also studied, which has no correlation with the welding method of 1900MPa grade low alloy ultra-high strength steel high-pressure vessel shell.
[0007] In 2008, Liu Zhenbao et al. published "Development of 1900MPa Ultra-High Strength Stainless Steel" in the third issue of Volume 32 of "Mechanical Engineering Materials". They proposed a 1900MPa chromium-nickel-cobalt-platinum large-size bar (φ200mm) ultra-high strength martensitic aging stainless steel. By studying the influence of heat treatment process on the mechanical properties of eight different compositions of chromium-nickel-cobalt-platinum martensitic aging stainless steel, they further optimized the alloy composition and realized the development of 1900MPa stainless steel bars. This paper focuses on high-performance stainless steel bars. Martensitic aging stainless steel and low-alloy ultra-high strength steel are not the same type of steel. Martensitic stainless steel has a large tendency to harden and weak thermal conductivity, which makes it poor in weldability and prone to cold cracking. At the same time, the welding area is prone to embrittlement. It is generally not used as a material for high-pressure vessels and has no relevance to the present invention. Summary of the invention
[0008] In order to overcome the deficiency in the prior art that high-performance steel cannot be prepared into a high-pressure container shell, the present invention proposes a welding method for a 1900MPa-grade low-alloy ultra-high-strength steel high-pressure container shell.
[0009] The welding process of the 1900MPa grade low alloy ultra-high strength steel high pressure vessel shell proposed by the present invention is:
[0010] Step 1: Preparation before welding:
[0011] Step 2: Assembly of parts to be welded:
[0012] According to the design requirements, the front head and the cylinder to be welded, and the cylinder and the rear head are assembled into a whole to obtain an unfixed high-pressure container shell;
[0013] When the welded parts are assembled, the gap between adjacent welded parts is less than 0.5mm; the straightness of the shell after assembly is less than 1mm / m. The welding grooves between the front head and the cylinder, and the welding grooves between the cylinder and the rear head are coaxially aligned; the misalignment of the alignment is less than 0.2mm.
[0014] Step 3: Weld the front head and cylinder:
[0015] The specific process is:
[0016] The assembled high-pressure container shell is clamped on a ring welding machine, and the roundness is set to be ≤0.2 mm.
[0017] Preheating the welded part of the assembled high-pressure container shell at a preheating temperature of 120-160° C. and a heating rate of 50° C. / min.
[0018] When the welding part reaches the preheating temperature, welding is carried out. During the welding process, the connection between the front end cap and the cylinder is welded first. The arc voltage of welding is 11V, the arc current is 45A, and the pulse current is 135A; the weld is formed through three passes.
[0019] Before argon arc welding, argon gas with a purity of 99.99% is provided in advance to protect the back of the weld. The gas flow rate of the argon gas is 18L / min, and the input direction is kept at 90° to the welding gun. Argon gas is continuously input during welding.
[0020] The specific process of the three-pass welding is:
[0021] The first pass of welding is performed with the 12 o'clock position of the cross section of the cylinder as the arc starting point of welding.
[0022] Move the welding gun to 2mm above the arc starting point, perform the first pass of welding clockwise toward the front head axis, and keep the welding gun at a 50° angle to the cylinder axis and a 75° angle to the welding direction. During welding, use the method of advancing two and retreating one, advancing 2mm and retreating 1mm, and maintain the welding speed at 110mm / min. Complete the first pass of welding.
[0023] The second pass of welding. Move the welding gun to the arc starting point of the first pass of welding for the second pass of welding. Adjust the angle of the welding gun to 55° with the axis and 75° with the welding direction. The welding speed is 55mm / min. Use 30° bevel gear welding and weld clockwise until the welding is completed.
[0024] The third welding pass was performed. The welding gun was adjusted to an angle of 50° with the axis and 75° with the welding direction. The welding speed was 110mm / min. The third welding pass was completed counterclockwise by advancing two times and retreating one time, with the method of advancing 2mm and retreating 1mm.
[0025] The 30° bevel gear method is to weld in a reciprocating bevel direction with a 30° angle between the welding gun and the weld normal.
[0026] Step 4: Weld the head and cylinder:
[0027] When welding the rear head and the cylinder, the welding process of the front head and the cylinder in step 3 is repeated to complete the welding of the cylinder and the rear head. The semi-finished high-pressure container shell is obtained.
[0028] Step 5: Vacuum quenching heat treatment:
[0029] The obtained semi-finished high-pressure container shell is subjected to vacuum air quenching heat treatment. The whole process of the vacuum air quenching heat treatment is vacuum air quenching, cold treatment and secondary tempering in sequence. The semi-finished high-pressure container shell subjected to vacuum air quenching heat treatment is obtained.
[0030] During the vacuum gas quenching heat treatment:
[0031] In the first step, the semi-finished high-pressure container shell is placed in a vacuum furnace and evacuated to a vacuum degree of 30×10 ~5 The vacuum furnace was heated to 880° C. at a heating rate of 28° C. / min and kept at this temperature for 1 h.
[0032] The second step is to fill the furnace with 99.999% pure liquid nitrogen after the insulation is completed. When the nitrogen pressure in the furnace reaches 5 bar, stop filling with liquid nitrogen.
[0033] In the third step, the nitrogen in the furnace cools down the semi-finished high-pressure vessel shell; gas quenching begins, and the temperature in the vacuum furnace drops to 0-30°C in 3 hours, and the gas quenching is completed.
[0034] The temperature of the cold treatment is -40°C and the cold treatment time is 60 minutes.
[0035] During the secondary tempering:
[0036] The first tempering treatment is performed on the semi-finished high-pressure vessel shell after cold treatment, specifically, the semi-finished high-pressure vessel shell after cold treatment is placed in a room temperature environment, and the semi-finished high-pressure vessel shell is heated to 0-30°C within 2 hours, and then the semi-finished high-pressure vessel shell is tempered for the first time. First, the semi-finished high-pressure vessel shell is heated to 290°C at a heating rate of 20°C / min, and the semi-finished high-pressure vessel shell is kept warm for 60 minutes; after the insulation is completed, it is taken out of the furnace. The first tempering treatment is completed.
[0037] After the first tempering treatment is completed, the second tempering treatment is immediately carried out.
[0038] When performing the second tempering, the process of the first tempering treatment is repeated to complete the second tempering treatment of the semi-finished high-pressure container shell.
[0039] Step 6: Machining:
[0040] According to the design requirements, the heat-treated high-pressure vessel shell is processed into a finished high-pressure vessel shell by traditional machining. At this point, the welding of the 1900MPa-grade low-alloy ultra-high-strength steel high-pressure vessel shell is completed.
[0041] The invention discloses a welding method for a 1900MPa-grade low alloy ultra-high strength steel high-pressure container shell with a diameter of φ100-φ1000mm, a wall thickness of 1.0-5.0mm and a straightness of no more than 2mm per meter.
[0042] The shell material of the high-pressure vessel is 300M low-alloy ultra-high strength steel, and is composed of three parts: a front head 1, a cylinder 2, and a rear head 3. The front head 1 and the rear head 3 are formed by machining or stamping and are bowl-shaped. The cylinder is a straight cylindrical part with a wall thickness of 1.0 to 5.0 mm, which is formed by strong spinning. The front head, the cylinder, and the rear head are welded into an integral container shell by tungsten inert gas welding. After vacuum gas quenching heat treatment, the tensile strength of the shell weld reaches more than 1900MPa, thereby realizing the preparation of the high-pressure container shell.
[0043] Before tungsten inert gas arc welding, the processing tool is used to ensure that the front head and the cylinder welding groove are coaxially aligned, and the straightness of the welding process meets the requirements. Argon protection is required during the welding process. The protective gas is 100% argon gas with a purity of 99.99%. The gas flow rate is strictly controlled at 12-20L / min according to the size of the high-pressure container to ensure the cleanliness of the welding joint, prevent oxygen and other impurities from entering the welding area, and corrode the weld to form defects such as inclusions and pores, thereby causing poor weld quality, and ultimately causing the performance of the high-pressure container to fail to reach 1900MPa. The arc voltage is controlled at 9-12V, the arc maintenance current is 30-50A, the pulse current needs to be controlled at 120-150A, and the welding speed is 80-100mm / min. Through multiple weld formations, the weld quality meets 100% X-ray flaw detection and appearance requirements; after the front head and cylinder welds are completed, the cylinder and rear head sides are welded in turn, and the operation method and parameter settings are the same as above.
[0044] The shell after assembly welding is subjected to vacuum gas quenching heat treatment. The vacuum degree during vacuum gas quenching is strictly required to be 20~30×10 ~5 Pa range, to prevent the oxidation of the inner and outer surfaces of the shell by impurity gases in the air, so that there is no decarburization layer during the heat treatment; put the welded shell into a vacuum furnace, heat it to 850-970°C at 20-30°C / min, and keep it warm for 1-2h; after the welded shell meets the insulation requirements, liquid nitrogen is poured into the furnace, the purity of the liquid nitrogen is required to be 99.999%, and the shell is gas-quenched and air-cooled to room temperature. The cooling rate needs to be strictly controlled to make the weld structure of the welded shell undergo phase transformation to form residual austenite and martensite; after vacuum gas quenching, a cold treatment process of -40-60°C is carried out to cool the high-pressure container shell after cold treatment. A tempering treatment is performed at 250-320° C. to transform the residual austenite and martensite composite into martensite and tempered martensite respectively, and then a tempering treatment is performed at 250-320° C. again; the high-pressure vessel shell material composite is completely transformed into tempered martensite, that is, the tensile strength of the 300M steel high-pressure vessel shell weld reaches more than 1900MPa, while the shell deformation is small, the straightness is not more than 2mm per meter, and the surface finish is good; then, the high-pressure vessel shell is mechanically processed into a finished product, thereby realizing the preparation of a 1900MPa-grade low-alloy ultra-high strength steel high-pressure vessel shell.
[0045] The shell material of the high-pressure container is 300M steel, which is a low-alloy ultra-high strength steel with good comprehensive mechanical properties. It is welded by tungsten inert gas arc welding of multiple parts and achieves a tensile strength of more than 1900MPa through vacuum quenching heat treatment.
[0046] When welding traditional high-strength steel, the gas flow rate is 8 to 12 L / min, the welding process parameters are welding pulse current of 160 to 220 A, arc voltage of 14 to 16 V, and welding speed of 50 to 70 mm / min.
[0047] The key technical point of the present invention is that when 300M steel weldments with a diameter of 100 to φ1000 mm and a wall thickness of 1.0 to 5.0 mm are welded by tungsten inert gas arc welding, different welding methods are adopted and welding is performed in a multi-pass combination in a certain order; through the "vacuum gas quenching + cold treatment + double tempering" heat treatment scheme, the high-pressure container weld performance and linear accuracy meet the requirements, and the preparation of 1900MPa low-alloy ultra-high strength steel shell is realized.
[0048] The present invention adopts tungsten inert gas welding in the preparation process of the high-pressure container shell using 300M steel. Through argon protection, impurity erosion is strictly limited. Before welding, the welding point is preheated in a temperature range that is greatly different from that of traditional steel. Since a certain amount of heat can slow down the cooling rate after welding, it is easy to achieve the escape of hydrogen in the weld metal, and at the same time, the hardening degree of the weld is greatly attenuated, effectively avoiding the generation of cracks in the welding process, and adopting appropriate process parameters for welding to reduce welding deformation. The high-pressure container shell welding process needs to control the pulse current to 120-150A and the welding speed to 80-120mm / min to prevent defects in the weld. Through clockwise two forward and one backward, 30° bevel teeth, counterclockwise two forward and one backward three different welding methods, multiple passes are combined and welded in a certain order. The relationship between the welding passes and the wall thickness is shown in Table 1, and preliminary preparations are made for the subsequent high-pressure container to reach 1900MPa.
[0049] Table 1 Relationship between welding pass and wall thickness
[0050]
[0051] The preparation process of the high-pressure vessel shell using 300M steel adopts vacuum quenching heat treatment technology to prevent the oxidation of the inner and outer surfaces of the shell by impurity gases in the air, so that there is no decarburization layer in the heat treatment of the weld. After vacuum quenching, a cold treatment process of -40 to 60 ° C is carried out. The heat treatment system adopts adaptive process parameters and strictly controls the cooling rate. The high-pressure vessel shell is tempered twice at 250 to 320 ° C, which is very different from the traditional low-temperature tempering and medium-temperature tempering system. The tempering temperature and other parameters are controlled as shown in Table 2 to ensure that the tensile strength of the 300M material shell reaches more than 1900MPa; the shell deformation is small, meeting the requirement of straightness not more than 2mm per meter, ensuring the dimensional accuracy of the high-pressure vessel shell heat treatment, and good surface finish.
[0052] Table 2 Tempering heat treatment parameters
[0053] BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1 It is a 1900MPa grade low alloy ultra-high strength steel high pressure vessel shell.
[0055] Figure 2This is a schematic diagram of the front head.
[0056] Figure 3 It is a schematic diagram of a cylinder.
[0057] Figure 4 It is a schematic diagram of the rear head.
[0058] Figure 5 It is a flow chart of the present invention.
[0059] In the figure: 1. front head; 2. cylinder; 3. rear head; 4. weld.
[0060] This embodiment is a method for welding a 1900MPa grade low alloy ultra-high strength steel high pressure container shell. DETAILED DESCRIPTION
[0061] This embodiment is a method for welding a 1900MPa grade low alloy ultra-high strength steel high pressure container shell.
[0062] like Figure 1 As shown, the high-pressure container shell structure of this embodiment includes a front head 1, a cylinder 2, and a rear head 3, which are welded together. Tungsten inert gas welding is adopted and vacuum gas quenching heat treatment is performed to realize the preparation of a 1900MPa high-pressure container shell.
[0063] Step 1: Preparation before welding:
[0064] The pre-welding preparation is the preparation of the front head 1, cylinder 2 and rear head 3 to be welded. The front head 1 and rear head 3 are both machined from 300M material forgings, and are connected to the cylinder 2 with a 45° groove to be welded. The cylinder 2 is formed by spinning of 300M steel forgings, and a cylinder with a length of 1000mm and a wall thickness of 3.0mm is formed by spinning, and a 45° groove to be welded is machined at both ends.
[0065] The 60 mm width of the front end cap 1, the cylinder 2 and the rear end cap 3 to be welded is cleaned by oxidizing with cotton yarn dipped in anhydrous ethanol. The welded area is sanded with a steel wire wheel.
[0066] Step 2: Assembly of parts to be welded:
[0067] According to the design requirements, the front head 1 and the cylinder 2, and the cylinder 2 and the rear head 3 to be welded are assembled as a whole to obtain a high-pressure container shell that is not fixedly connected; the gap between adjacent welded parts is less than 0.5mm; the straightness of the shell after assembly is less than 1mm / m.
[0068] During assembly, the tooling is used to ensure that the welding grooves of the front head 1 and the cylinder 2, and the welding grooves of the cylinder 2 and the rear head 3 are coaxially aligned; the misalignment of the alignment is less than 0.2 mm. The tooling adopts the existing technology.
[0069] Step 3: Weld the front head and cylinder:
[0070] The specific process is:
[0071] In the first step, the unfixed high-pressure container shell is clamped on a ring welding machine, and the circular runout is ensured to be ≤0.2 mm with the welding machine axis as the center.
[0072] The second step is to preheat the welded part of the unfixed high-pressure container shell; the preheating temperature is 150°C. The heating rate is 50°C / min. The preheating temperature range of traditional alloy steel is less than 80°C. The preheating range of the material involved in the present invention should be 120-160°C, which greatly reduces the crack incidence rate of the weld. When the welded part reaches the preheating temperature, welding is carried out.
[0073] Before argon arc welding, argon gas with a purity of 99.99% is provided to the back of the weld in advance. The gas flow rate of the argon gas is 18L / min, and the input direction is maintained at 90° to the welding gun. Argon gas is continuously input during welding; the argon gas protection is stopped only after the welding is completed, ensuring that the welding process of the weld joint is fully and completely protected to prevent oxygen and other impurities from entering the welding area.
[0074] During the welding process, the connection between the front end cap 1 and the cylinder 2 is first welded. During welding, the arc voltage is 11V, the arc current is 45A, the pulse current is 135A, and the weld is formed through 3 passes.
[0075] During welding, the welding of the front end cap 1 and the cylinder 2 is completed by three passes. Specifically,
[0076] The first pass of welding is performed with the highest point of the cylinder cross section, i.e., the 12 o'clock position, as the arc starting point of welding.
[0077] Move the welding gun to 10mm above the welding arc starting point and turn on the welding gun switch. Under the action of high-voltage electric pulse, the argon gas is ionized to ignite the welding arc to achieve arc initiation. After the welding arc is generated, it is immediately lowered to 2mm above the arc starting point. The first pass of welding is carried out clockwise toward the front head 1, and the welding gun is kept at a 50° angle to the cylinder axis and a 75° angle to the welding direction. The conventional two-step forward and one-step backward method is used during welding, with 2mm forward and 1mm backward, and the welding speed is maintained at 110mm / min. After completing the first pass of welding, the weld width is 7mm.
[0078] The second welding pass. Move the welding gun to the arc starting point of the first pass for the second welding, adjust the angle of the welding gun to 55° with the axis, and at the same time form an angle of 75° with the welding direction. The welding speed is 55mm / min. Use 30° bevel gear method to weld, and weld clockwise until the welding is completed; the 30° bevel gear method is a reciprocating bevel direction of 30° between the welding gun and the weld normal. The welding width is 10mm. The high-temperature weld pool formed during the second welding process and the first weld structure are fully stirred and evenly formed at a cross angle of 30°, and the internal stress of the welding is offset, so that the structure of the first weld layer and the second weld layer are fully and evenly fused.
[0079] The third welding pass was performed. The welding gun was adjusted to an angle of 50° with the axis and 75° with the welding direction. The welding speed was 110 mm / min. The third welding pass was completed counterclockwise by advancing two times and retreating one time, with an advance of 2 mm and a retreat of 1 mm. The welding width of the third welding pass was 10 mm.
[0080] The third pass improves the density of the weld and ensures the final weld quality and morphology. The above three passes of welding must be strictly followed. Changing the order will increase the difficulty of tissue fusion, and a large number of weld pores and unfused defects will be generated, resulting in the risk of welding failure of 300M steel.
[0081] Step 4: Weld the head and cylinder:
[0082] When welding the rear head and the cylinder, the welding process of the front head 1 and the cylinder 2 in step 3 is repeated to complete the welding of the cylinder 2 and the rear head 3.
[0083] The obtained semi-finished high-pressure container shell.
[0084] Step 5: Vacuum quenching heat treatment:
[0085] The obtained semi-finished high-pressure vessel shell is subjected to vacuum air quenching heat treatment. The entire process of the vacuum air quenching heat treatment is vacuum air quenching, cold treatment and secondary tempering, specifically:
[0086] In the first step, the semi-finished high-pressure container shell is placed in a vacuum furnace and evacuated to a vacuum degree of 30×10 ~5 The vacuum furnace was heated to 880° C. at a heating rate of 28° C. / min and kept at this temperature for 1 h.
[0087] The second step is to fill the furnace with 99.999% pure liquid nitrogen after the insulation is completed. When the nitrogen pressure in the furnace reaches 5 bar, stop filling with liquid nitrogen.
[0088] In the third step, the nitrogen in the furnace cools down the semi-finished high-pressure vessel shell; gas quenching begins, and the temperature in the vacuum furnace drops to 0-30°C in 3 hours, and the gas quenching is completed.
[0089] The semi-finished high-pressure vessel shell is transferred to a cold box furnace at -40°C within 1 minute for cold treatment for 60 minutes before being taken out of the furnace; the cold treatment makes the grain boundary diaphragm in the 300M steel weld structure disappear, reduces the residual austenite, prepares for the subsequent tempering process to improve the performance, and eliminates the residual stress of the material in the vacuum gas quenching process, which is beneficial to stabilize the size of the high-pressure vessel shell.
[0090] The first tempering treatment is performed on the semi-finished high-pressure vessel shell after cold treatment. Specifically, the semi-finished high-pressure vessel shell after cold treatment is placed in a room temperature environment, and the semi-finished high-pressure vessel shell is brought back to the temperature of 0-30°C within 2 hours, and then the semi-finished high-pressure vessel shell is tempered for the first time. First, the semi-finished high-pressure vessel shell is heated to 290°C at a heating rate of 20°C / min, and the semi-finished high-pressure vessel shell is kept warm for 60 minutes; after the insulation is completed, it is taken out of the furnace, so that the residual austenite and martensite complex are transformed into martensite and tempered martensite respectively, so as to achieve the first increase in the tensile strength of the weld of the semi-finished high-pressure vessel shell, reaching 1600-1700MPa. The first tempering treatment is completed.
[0091] After the first tempering treatment is completed, the second tempering treatment is immediately carried out.
[0092] During the second tempering, the process of the first tempering treatment is repeated, and the second tempering treatment of the semi-finished high-pressure container shell is completed, so that the weld of the high-pressure container shell is transformed into tempered martensite, so that the tensile strength of the welding part of the 300M steel high-pressure container shell reaches more than 1900MPa, and at the same time, the shell deformation is small, the straightness is not more than 2mm per meter, and the surface finish is good.
[0093] Step 6: Machining:
[0094] According to the design requirements, the heat-treated high-pressure vessel shell is processed into a finished high-pressure vessel shell by traditional machining. At this point, the welding of the 1900MPa-grade low-alloy ultra-high-strength steel high-pressure vessel shell is completed.
[0095] In the present invention, the high-pressure container shell material is 300M steel, which is a low-alloy ultra-high strength steel with good comprehensive mechanical properties. It is welded by tungsten inert gas arc welding of multiple parts and achieves a tensile strength of more than 1900MPa through vacuum quenching heat treatment.
[0096] The common gas flow rate of traditional steel welding is 8-12L / min, and the welding process parameters are 160-220A welding pulse current, 14-16V arc voltage, and 50-70mm / min welding speed; the preheating temperature range of traditional alloy steel is less than 80℃. In the preparation process of 300M steel high-pressure container shell, tungsten inert gas welding is used to ensure that the preheating range of the welded part reaches 120-160℃ before welding, and the argon protection is used to strictly limit the erosion of impurities; using the appropriate welding process parameters, the pulse current is controlled to be 120-150A and the welding speed is 80-120mm / min during the welding process. According to the different thickness and structural requirements of the container shell, three different welding methods are used, namely, clockwise advance two and retreat one, 30° bevel teeth, and counterclockwise advance two and retreat one. According to a certain order of multi-pass combination welding, the welding organization is effectively fused, the weld is fine, the welding quality is improved, and the risk of weld defects is reduced, making preliminary preparations for the subsequent high-pressure container to reach 1900MPa.
[0097] The three-pass welding method in the present invention must be strictly followed. Changing the order will increase the difficulty of tissue fusion, and a large number of weld pores and unfused defects will be generated, resulting in the risk of welding failure of 300M material steel. It will also cause tissue problems and affect the subsequent heat treatment performance.
[0098] In the post-welding vacuum quenching heat treatment of the semi-finished 300M steel high-pressure container shell, the present invention provides a vacuum quenching process through a "vacuum quenching + cold treatment + two tempering" heat treatment scheme to prevent the oxidation of the inner and outer surfaces of the shell by impurity gases in the air, so that there is no decarburization layer in the heat treatment, and the influence of surface oxidation on the performance of the high-pressure container shell is reduced to the greatest extent; the residual austenite grain boundary diaphragm in the weld and structure of the vacuum quenching process is eliminated through cold treatment, so as to prepare for the subsequent two tempering structure transformations, and at the same time, the residual stress of the vacuum quenching process is eliminated, which is beneficial to stabilize the size of the pressure container shell. The heat treatment system adopts optimized process parameters, strictly controls the cooling rate, and the high-pressure container shell is tempered twice continuously at 250-320°C to ensure that the tensile strength of the high-pressure container shell weld of the 300M material reaches more than 1900MPa.
[0099] The vacuum quenching heat treatment process system and process of the 300M steel welded shell involved in the present invention are greatly different from the traditional ultra-high strength steel heat treatment system. Taking 30CrMnSiA and D406A typical ultra-high strength steel as examples, the heat treatment system is quenching + one tempering treatment, and generally cold treatment process and secondary tempering process are not allowed, because adding cold treatment and secondary tempering process cannot improve the tensile strength of 30CrMnSiA and D406A steel, and secondary tempering treatment will cause tissue hardening and the risk of reverse grain growth, resulting in reduced tensile strength, hardness and plasticity, resulting in product performance failing to meet requirements and being scrapped.
[0100] The welding + heat treatment technical solution adopted in the present invention has little effect on the deformation of the high-pressure container shell manufacturing process, meets the requirement of straightness not greater than 2mm per meter, ensures the dimensional accuracy of the heat treatment of the high-pressure container shell weld, and has good surface finish. The tensile strength of the weld of the high-pressure vessel shell made of traditional 30CrMnSiA and D406A typical ultra-high strength steel is generally lower than 1600MPa, and the product shape and position accuracy is poor, and the straightness is generally more than 2mm per meter. The main reason is that the welding process adopts a two-step forward and one-step back method, and multiple passes are also the same welding method, resulting in uneven weld structure, inability to offset welding internal stress, and large deformation near the weld. At the same time, the heat treatment process adopts air furnace heat treatment. During the heat treatment process, the inner and outer surfaces of the high-pressure vessel shell weld react with oxygen and other gases in the air to produce a certain proportion of decarburization layer, resulting in a decrease in the performance of the high-pressure vessel shell weld. The oxidation reaction causes a surge in internal stress, resulting in serious deformation of the high-pressure vessel shell weld, which requires strong shape correction treatment to meet the requirements. At the same time, the surface cleanliness of the high-pressure vessel after heat treatment is poor, and a sandblasting process needs to be added to treat the surface to remove the oxide scale. The rework process is cumbersome and difficult.
Claims
1. A welding method for a 1900MPa grade low alloy ultra-high strength steel high pressure vessel shell, characterized in that: The specific process is: Step 1: Preparation before welding; Step 2: Assembly of parts to be welded: According to the design requirements, the front head and the cylinder to be welded, and the cylinder and the rear head are assembled into a whole to obtain an unfixed high-pressure container shell; Step 3: Weld the front head and cylinder: The specific process is: Clamping the assembled high-pressure container shell on a ring welding machine, and making the roundness ≤0.2mm; Preheating the welded portion of the assembled high-pressure container shell; the preheating temperature is 120-160° C.; the heating rate is 50° C. / min; When the welded part reaches the preheating temperature, welding is performed; during the welding process, the connection between the front end cap and the cylinder is welded first; The arc voltage of welding is 11V, the arc current is 45A, and the pulse current is 135A; the weld is formed through three passes; Step 4: Weld the head and cylinder: When welding the rear head and the cylinder, repeat the welding process of the front head and the cylinder in step 3 to complete the welding of the cylinder and the rear head; the semi-finished high-pressure vessel shell is obtained; Step 5: Vacuum quenching heat treatment: The obtained semi-finished high-pressure container shell is subjected to vacuum air quenching heat treatment; the whole process of the vacuum air quenching heat treatment is vacuum air quenching, cold treatment and secondary tempering in sequence; the semi-finished high-pressure container shell subjected to vacuum air quenching heat treatment is obtained; Step 6: Machining: According to the design requirements, the heat-treated high-pressure vessel shell is processed into a finished high-pressure vessel shell through traditional machining; at this point, the welding of the 1900MPa grade low-alloy ultra-high strength steel high-pressure vessel shell is completed.
2. The welding method for the 1900MPa grade low alloy ultra-high strength steel high pressure vessel shell according to claim 1, characterized in that: When the welded parts are assembled, the gap between adjacent welded parts is less than 0.5mm; the straightness of the shell after assembly is less than 1mm / m; the welding grooves between the front head and the cylinder, and the welding grooves between the cylinder and the rear head are coaxially aligned; the misalignment of the alignment is less than 0.2mm.
3. The welding method for the 1900MPa grade low alloy ultra-high strength steel high pressure vessel shell according to claim 1, characterized in that: Before argon arc welding, argon gas with a purity of 99.99% is provided in advance to protect the back of the weld; the gas flow rate of the argon gas is 18L / min, the input direction is maintained at 90° to the welding gun, and argon gas is continuously input during the welding process.
4. The welding method for the 1900MPa grade low alloy ultra-high strength steel high pressure vessel shell according to claim 1, characterized in that: The specific process of the three-pass welding is: The first welding pass is performed with the 12 o'clock position of the cross section of the cylinder as the arc starting point of welding; Move the welding gun to 2mm above the arc starting point, perform the first welding in a clockwise direction toward the front head axis, and keep the welding gun at a 50° angle to the cylinder axis and a 75° angle to the welding direction; use the two-step forward and one-step backward method during welding, advance 2mm and retreat 1mm, and maintain the welding speed at 110mm / min; complete the first welding; The second welding process is performed; the welding gun is moved to the arc starting point of the first welding process for the second welding process, and the angle between the welding gun and the axis is adjusted to 55°, and the angle between the welding gun and the axis is 75°; the welding speed is 55mm / min; Use 30° bevel teeth to weld, and weld in a clockwise direction until the welding is completed; The third welding pass was performed; the angle between the welding gun and the axis was adjusted to 50°, and the angle with the welding direction was 75°; the welding speed was 110mm / min; the method of advancing two and retreating one was adopted during welding, and the third welding pass was completed counterclockwise in a manner of advancing 2mm and retreating 1mm.
5. The welding method for the 1900MPa grade low alloy ultra-high strength steel high pressure vessel shell according to claim 4, characterized in that: The 30° bevel gear method is to weld in a reciprocating bevel direction with a 30° angle between the welding gun and the weld normal.
6. The welding method for the 1900MPa grade low alloy ultra-high strength steel high pressure vessel shell according to claim 1, characterized in that: During the vacuum gas quenching heat treatment: In the first step, the semi-finished high-pressure container shell is placed in a vacuum furnace and evacuated to a vacuum degree of 30×10 ~ 5 Pa; the vacuum furnace is heated to 880°C at a heating rate of 28°C / min and kept at this temperature for 1h; The second step is to fill the furnace with 99.999% pure liquid nitrogen after the insulation is completed; stop filling the liquid nitrogen when the nitrogen pressure in the furnace reaches 5 bar; In the third step, the nitrogen in the furnace cools down the semi-finished high-pressure vessel shell; gas quenching is started to reduce the temperature in the vacuum furnace to 0-30°C in 3 hours, and gas quenching is completed; and the semi-finished product is taken out of the furnace.
7. The welding method for the 1900MPa grade low alloy ultra-high strength steel high pressure vessel shell according to claim 1, characterized in that: The temperature of the cold treatment is -40°C and the cold treatment time is 60 minutes.
8. The welding method for the 1900MPa grade low alloy ultra-high strength steel high pressure vessel shell according to claim 1, characterized in that: During the secondary tempering: The semi-finished high-pressure vessel shell after the cold treatment is subjected to the first tempering treatment, specifically, the semi-finished high-pressure vessel shell after the cold treatment is placed in a room temperature environment, and the semi-finished high-pressure vessel shell is heated to 0-30°C within 2 hours, and then the semi-finished high-pressure vessel shell is subjected to the first tempering treatment; firstly, the semi-finished high-pressure vessel shell is heated to 290°C at a heating rate of 20°C / min, and the semi-finished high-pressure vessel shell is kept warm for 60 minutes; after the insulation is completed, the semi-finished high-pressure vessel shell is taken out of the furnace; and the first tempering treatment is completed; When the first tempering treatment is completed, the second tempering treatment is immediately carried out; When performing the second tempering, the process of the first tempering treatment is repeated to complete the second tempering treatment of the semi-finished high-pressure container shell.
Citation Information
Patent Citations
Heat treatment method capable of reducing out-of-round deformation of large-diameter ring part
CN104593783A
Cutting part and manufacturing method thereof
CN107662084A
Pressure-resisting welding method for circular seam of pressure container
CN110039266A
Softening heat treatment process of small-specification 22Si2MnCrNi2MoA rolled steel
CN110551880A
Preparation method of stainless steel thin-walled cylinder
CN114473370A