Silicon carbide composite substrate and preparation method thereof

By using alkaline polishing liquid with pH value of 10-11 and polishing liquid with titanium carbide and other components, the corrosive pit defects and uneven distribution of abrasives in the preparation of silicon carbide composite substrates in the prior art are solved, and the problem of corrosion pit defects and uneven distribution of abrasives is achieved. Efficient polishing and bonding quality improvement.

CN118977194APending Publication Date: 2024-11-19TJ INNOVATIVE SEMICON SUBSTRATE TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411065950.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

When preparing silicon carbide composite substrates, the strong acidity of the existing polishing liquid leads to corrosive pit defects and uneven distribution of abrasives, affecting the bonding quality.

Method used

An alkaline polishing liquid with a pH of 10-11 is used, and titanium carbide is used as abrasive, combined with components such as potassium ferrate and carboxylate to improve the stability and oxidation rate of the polishing liquid, avoiding corrosive damage and abrasive deposition.

Benefits of technology

It improves the polishing rate and quality, reduces the roughness of the substrate surface, extends the service life of the polishing pad, ensures the bonding quality of the composite substrate, and reaches atomic level flatness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118977194A_ABST
    Figure CN118977194A_ABST
Patent Text Reader

Abstract

The invention provides a silicon carbide composite substrate and a preparation method thereof. The preparation method comprises the following steps: (1) respectively polishing a to-be-bonded surface of a supporting substrate and a to-be-bonded surface of a single crystal silicon carbide substrate by using a polishing solution to obtain a polished supporting substrate and a polished single crystal silicon carbide substrate; wherein the polishing solution comprises the following components: an oxidizing agent, titanium carbide, a pH regulator, a dispersing agent and a solvent; the pH value of the polishing solution is 10-11; and (2) respectively pretreating the polished support substrate and the polished monocrystalline silicon carbide substrate, and then bonding to obtain the silicon carbide composite substrate. By adopting the polishing solution for polishing, the polishing speed and the polishing quality can be improved, and the bonding quality of the silicon carbide composite substrate is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor materials and relates to a silicon carbide composite substrate and a preparation method thereof. Background Art

[0002] Single-crystal silicon carbide substrate is a wide bandgap semiconductor material. Devices made of single-crystal silicon carbide substrate have the advantages of high temperature resistance, high voltage resistance, high frequency, high power, radiation resistance and high efficiency. They have important application value in the fields of radio frequency and new energy vehicles. However, the manufacturing cycle of single-crystal silicon carbide material is long and the cost is high. One solution to reduce costs is to use a composite substrate structure to bond the single-crystal silicon carbide substrate and the supporting substrate to reduce costs.

[0003] When preparing a silicon carbide composite substrate, it is usually necessary to perform chemical mechanical polishing (CMP) on the single crystal silicon carbide substrate and the supporting substrate to facilitate subsequent bonding. The abrasives of the commonly used polishing liquid are mostly aluminum oxide, silicon oxide and cerium oxide, and the pH value of the polishing liquid is about 2-4, among which nitric acid is mostly used as the pH adjuster. The problems are: (1) The polishing liquid is strongly acidic and corrosive, and it is easy to corrode the surface of the silicon carbide substrate during polishing, resulting in corrosive pit defects; and the strongly acidic polishing liquid is easy to corrode the polishing pad, causing the groove of the polishing pad to quickly become shallow, affecting the polishing effect; (2) The abrasive is also easy to deposit and foam and deform in the acidic polishing liquid, resulting in uneven distribution of abrasives and uneven abrasive particle size in the polishing liquid, affecting the polishing effect. If the polishing effect is not good, the bonding quality of the composite substrate will be reduced. Therefore, it is urgent to provide a solution that can solve the above problems. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a silicon carbide composite substrate and a preparation method thereof. In the preparation method of the present invention, the polishing liquid used has a pH value of 10-11, is alkaline, has low corrosiveness, and will not corrode the surface of the single-crystal silicon carbide substrate and the supporting substrate, which can avoid the occurrence of corrosive pit defects on the single-crystal silicon carbide substrate after polishing, and can reduce the corrosion damage to the polishing pad; and the titanium carbide in the polishing liquid, as an abrasive, has good stability in the polishing liquid with a pH value of 10-11, and will not react and deform even after long-term immersion, and has good suspension, uniform suspension, and no deposition or agglomeration. Therefore, the use of the polishing liquid can improve the polishing effect and improve the bonding quality of the silicon carbide composite substrate.

[0005] To achieve this object, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a method for preparing a silicon carbide composite substrate, the preparation method comprising:

[0007] (1) polishing the surface to be bonded of the support substrate and the surface to be bonded of the single-crystal silicon carbide substrate respectively using a polishing liquid to obtain a polished support substrate and a polished single-crystal silicon carbide substrate;

[0008] The polishing liquid comprises an oxidant, titanium carbide, a pH regulator, a dispersant and a solvent; the pH value of the polishing liquid is 10-11, for example, 10.1, 10.2, 10.3, 10.4, 10.5, 10.6, 10.7, 10.8, 10.9 or 11;

[0009] (2) The polished support substrate and the polished single-crystal silicon carbide substrate are pretreated separately and then bonded to obtain a silicon carbide composite substrate.

[0010] It should be noted that, since titanium carbide is soluble in nitric acid, nitric acid cannot be used in the polishing solution of the present invention.

[0011] The present invention provides a method for preparing a silicon carbide composite substrate, wherein a specific polishing liquid is used to polish the supporting substrate and the bonding surface of the single-crystal silicon carbide substrate respectively, and the polishing liquid has the following advantages:

[0012] (1) The pH value of the polishing liquid is 10-11, which is alkaline and has low corrosiveness. It will not corrode the surface of the single-crystal silicon carbide substrate and the supporting substrate, and can avoid the appearance of corrosive pit defects on the single-crystal silicon carbide substrate after polishing, thereby improving the polishing quality; and the polishing liquid has low corrosiveness, which can reduce the corrosion damage to the polishing pad, extend the service life of the polishing pad, and improve the polishing effect;

[0013] (2) Titanium carbide in the polishing liquid is an abrasive. Titanium carbide is hard and has excellent impact and wear resistance, which can improve the polishing rate. Titanium carbide has good chemical stability and good stability in the polishing liquid with a pH value of 10-11. It will not react or deform even after long-term immersion. At the same time, titanium carbide has good suspension in the polishing liquid with a pH value of 10-11, and the suspension is uniform without sedimentation or agglomeration. The polishing liquid does not need to be frequently and vigorously shaken when used. In addition, titanium carbide has good thermal conductivity. Good thermal conductivity can transfer the heat generated by mechanical friction during the polishing process to the polishing disc, and cool it down through the condensed water inside the polishing disc;

[0014] Therefore, the present invention adopts a limited polishing liquid for polishing, which can improve the polishing rate, reduce the roughness of the substrate surface and improve the polishing quality, especially can improve the polishing rate and polishing quality of the single crystal silicon carbide substrate, the surface to be bonded of the single crystal silicon carbide substrate after polishing can reach atomic level flatness, which is beneficial to improve the bonding quality of the silicon carbide composite substrate.

[0015] The present invention does not limit the material of the support substrate, including but not limited to silicon carbide. The silicon carbide support substrate and the single crystal silicon carbide substrate can be Si-C surface bonded, Si-Si surface bonded, or CC surface bonded.

[0016] In the present invention, if the pH value of the polishing solution is too low or too high, the oxidizing property of the oxidant and the stability of the polishing solution will be affected.

[0017] Preferably, the oxidizing agent comprises ferrate.

[0018] Preferably, the ferrate comprises potassium ferrate and / or sodium ferrate.

[0019] In the present invention, potassium ferrate has the highest stability and strongest oxidizing property when the pH value is 10-11. Its oxidizing effect is stronger than that of potassium permanganate, but its corrosiveness is much lower than that of potassium permanganate polishing liquid whose pH is adjusted by nitric acid. Potassium ferrate can form a large amount of OH in water. - , the chemical formula is as follows: FeO4 2- +4H2O+3e=Fe(OH)3+5OH - , OH - After losing an electron, hydroxyl radicals are formed. The large amount of hydroxyl radicals generated can oxidize the SiC surface and increase the polishing rate. In addition, potassium ferrate oxidant is an "environmentally friendly" oxidant, without any toxic or environmentally polluting byproducts, and polishing waste liquid does not need to be treated with special hazardous waste chemicals.

[0020] Preferably, the particle size D50 of the titanium carbide is 100-300nm, for example, it can be 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm, 190nm, 200nm, 210nm, 220nm, 230nm, 240nm, 250nm, 260nm, 270nm, 280nm, 290nm or 300nm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] In the present invention, within the range of particle size D50 of 100-300 nm, the larger the particle size of titanium carbide is, the higher the probability of abnormal scratches after polishing is.

[0022] Preferably, the pH adjuster comprises H2O2 and / or KOH.

[0023] In the present invention, neither H2O2 nor KOH reacts with titanium carbide. H2O2 plays a role in adjusting the pH value of the polishing liquid through its stability and decomposition characteristics under different pH conditions, and H2O2 also plays a role in assisting oxidation.

[0024] Preferably, the dispersant comprises pyrrolidone and / or sulfonate, preferably a combination of pyrrolidone and sulfonate.

[0025] The present invention does not limit the specific types of pyrrolidone substances, including but not limited to at least one of γ-valerolactone, pyrrolone, 4-pyrrolone, 3-pyrrolone and α-pyrrolidone.

[0026] The present invention does not limit the specific type of sulfonate, including but not limited to at least one of alkylbenzene sulfonate, α-olefin sulfonate, alkyl sulfonate and α-sulfonic monocarboxylate.

[0027] Preferably, the solvent comprises water.

[0028] Preferably, the polishing liquid further comprises a rate accelerator.

[0029] In the present invention, the rate accelerator is introduced to further increase the oxidation rate of the polishing liquid and ultimately increase the polishing rate.

[0030] Preferably, the rate enhancer comprises a carboxylate.

[0031] In the present invention, the carboxylate can slowly release OH - Ion, OH - When an ion loses an electron, it forms a hydroxyl radical, which promotes oxidation, thus further increasing the oxidation rate and ultimately the polishing rate. At the same time, carboxylate acts as a sustained-release agent, and the supplemented hydroxide ions facilitate the maintenance of the pH value of the polishing liquid, making the abrasive in the polishing liquid evenly dispersed, thus ensuring good surface quality of the silicon carbide crystal after polishing.

[0032] Preferably, the carboxylate salt comprises at least one of sodium acetate, potassium acetate and calcium acetate.

[0033] Preferably, based on the total mass of the polishing liquid as 100%, the mass fraction of the oxidant is ≤10%, for example, it can be 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1% or 0.5%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] In the present invention, when the polishing liquid contains too much oxidant (such as potassium ferrate), the pH value of the polishing liquid will increase and reduce its oxidizability, and excessive addition will cause water acidification, seriously affecting the stability of the polishing liquid and affecting the ecological environment.

[0035] Preferably, based on the total mass of the polishing liquid as 100%, the mass fraction of titanium carbide is ≤8%, for example, it can be 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1% or 0.5%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] In the present invention, if the content of titanium carbide is too high, the grooves of the polishing pad will be clogged during polishing, forming a large number of particles, thereby causing scratch defects and affecting the roughness and uniformity.

[0037] Preferably, based on the total mass of the polishing liquid as 100%, the mass fraction of the rate accelerator is ≤1.4%, for example, it can be 1.4%, 1.3%, 1.2%, 1.1%, 1%, 0.9%, 0.8%, 0.7%, 0.6%, 0.5%, 0.4%, 0.3%, 0.2%, 0.1% or 0.05%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] In the present invention, when the rate accelerator is a carboxylate, the hydroxide ions released by it and the pH adjuster jointly affect the pH value of the polishing liquid. If an excessive amount of carboxylate is added, the pH value of the polishing liquid will be too high. When the pH value is >11, the oxidation ability will be reduced, affecting the rate.

[0039] Preferably, based on the total mass of the polishing liquid as 100%, the mass fraction of the pH adjuster is ≤0.5%, for example, it can be 0.5%, 0.4%, 0.3%, 0.2%, 0.1% or 0.05%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] Preferably, based on the total mass of the polishing liquid as 100%, the mass fraction of the dispersant is ≤0.1%, for example, it can be 0.1%, 0.09%, 0.08%, 0.07%, 0.06%, 0.05%, 0.03% or 0.01%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0041] Preferably, based on the total mass of the polishing liquid as 100%, the mass fraction of the solvent is ≥80%, for example, it can be 80%, 81%, 83%, 85%, 88%, 90%, 92%, 95%, 98% or 99%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] Preferably, the material of the polishing pad used for polishing includes any one of damping cloth, PU material, polyurethane and non-woven fabric.

[0043] In the present invention, a suitable polishing pad material is selected according to the particle size of titanium carbide. When large-particle titanium carbide (particle size D50 is 200nm-300nm and not 200nm) is selected, it is suitable to be matched with a softer polishing pad, such as damping cloth or PU material. When small-particle titanium carbide (particle size D50 is 100nm-200nm and not 200nm) is selected, it is suitable to be matched with a harder polishing pad, such as polyurethane or non-woven fabric. When the titanium carbide particle size D50 is 200nm, it can be arbitrarily matched with a polishing pad made of damping cloth, PU material, polyurethane or non-woven fabric, and the material of the polishing pad is selected according to the hardness of the material to be polished.

[0044] Preferably, the polishing includes preliminary polishing and main polishing performed sequentially.

[0045] In the present invention, the pre-polishing step is performed before the main polishing to ensure that the parameters such as the rotation speed, pressure and flow rate of the main polishing step are easily increased to the target values ​​and reach a stable state.

[0046] It should be noted that, when performing the pre-polishing and the main polishing, the workpiece to be polished is adsorbed on the polishing head and the polishing pad is placed on the polishing plate.

[0047] Preferably, the specific parameters of the pre-polishing include: a polishing head speed of 10-50rpm, for example, 10rpm, 20rpm, 30rpm, 40rpm or 50rpm; a polishing disc speed of 10-50rpm, for example, 10rpm, 20rpm, 30rpm, 40rpm or 50rpm; a polishing head pressure of 1-4psi, for example, 1psi, 2psi, 3psi or 4psi; a polishing liquid flow rate of 50-100mL / min, for example, 50mL / min, 60mL / min, 70mL / min, 80mL / min, 90mL / min or 100mL / min; a polishing time of 5-10s, for example, 5s, 6s, 7s, 8s, 9s or 10s, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0048] Preferably, during the pre-polishing process, the polishing head and the polishing disc have different rotation speeds.

[0049] Preferably, during the pre-polishing process, the polishing head and the polishing disc rotate counterclockwise.

[0050] Preferably, the specific parameters of the main polishing include: a polishing head rotation speed of 50-120rpm, for example, 50rpm, 60rpm, 70rpm, 80rpm, 90rpm, 100rpm, 110rpm or 120rpm, etc.; an optical disc rotation speed of 50-120rpm, for example, 50rpm, 60rpm, 70rpm, 80rpm, 90rpm, 100rpm, 110rpm or 120rpm, etc.; a polishing head pressure of 5-12psi, for example, 5psi, 6psi, 7psi, 8psi, 9psi, 10psi, 11psi or 12psi, etc.; the polishing liquid flow rate is 80-200mL / min, for example, it can be 80mL / min, 90mL / min, 100mL / min, 110mL / min, 150mL / min, 180mL / min or 200mL / min, etc.; the polishing time is 1-20min, for example, it can be 1min, 3min, 5min, 8min, 10min, 15min, 18min or 20min, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0051] Preferably, during the main polishing process, the rotational speeds of the polishing head and the polishing disk are different.

[0052] Preferably, during the main polishing process, the polishing head and the polishing disc rotate counterclockwise.

[0053] By using the polishing liquid of the present invention and under the limitation of the above-mentioned polishing method and parameters, the polishing rate and polishing quality of the single-crystal silicon carbide substrate can be significantly improved, and the damage to the polishing pad can be significantly reduced.

[0054] Preferably, during the polishing process, after the main polishing, a surface cleaning step is also performed.

[0055] Preferably, the specific parameters of the surface cleaning include: a polishing head speed of 50-120rpm, for example, 50rpm, 60rpm, 70rpm, 80rpm, 90rpm, 100rpm, 110rpm or 120rpm, etc.; a polishing disc speed of 50-120rpm, for example, 50rpm, 60rpm, 70rpm, 80rpm, 90rpm, 100rpm, 110rpm or 120rpm, etc.; a polishing head pressure of 5-12psi, for example, 5psi, 6psi, 7psi, 8psi, 9psi, 10psi, 11psi or 12psi, etc.; a pure water flow rate of 5-8L / min, for example, 5L / min, 6L / min, 7L / min or 8L / min, etc.; a cleaning time of 20-60s, for example, 20s, 30s, 40s, 50s or 60s, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0056] In the present invention, after the main polishing, pure water is used to clean the surface of the substrate and the polishing pad after the main polishing, so as to wash away the byproducts and particles generated by the polishing.

[0057] Preferably, during the surface cleaning process, the polishing head and the polishing disc have different rotation speeds.

[0058] Preferably, during the surface cleaning process, the polishing head and the polishing disc rotate in a counterclockwise direction.

[0059] Preferably, the pretreatment in step (2) includes a cleaning step.

[0060] In the present invention, cleaning is required after polishing to remove surface particles, by-products, metal ions and polishing liquid residues.

[0061] Preferably, the cleaning comprises megasonic vibration, brushing and spin drying performed sequentially.

[0062] In the present invention, after megasonic vibration and brushing, the drying is performed to achieve dry-in and dry-out.

[0063] Preferably, specific parameters of the megasonic vibration include: megasonic power of 200-600W, for example, 200W, 220W, 250W, 300W, 400W, 500W or 600W; megasonic time of 80-180s, for example, 80s, 90s, 100s, 120s, 150s or 180s, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0064] Preferably, in the process of the megasonic vibration, the reagents used include citric acid, dilute sulfuric acid or SC1 solution (wherein the volume ratio of ammonia water: hydrogen peroxide: water = 1:2:10) and the like.

[0065] Preferably, the scrubbing time is 120-300 s, for example, 120 s, 150 s, 200 s, 250 s or 300 s, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0066] Preferably, during the scrubbing process, the reagents used include a 3-5% hydrofluoric acid solution or an SC1 solution (wherein the volume ratio of ammonia water: hydrogen peroxide: water = 1:2:10), in combination with a wafer brush made of PVA (polyvinyl alcohol).

[0067] Preferably, the pretreatment in step (2) further comprises: injecting ions into the surface to be bonded of the cleaned single crystal silicon carbide substrate to form an ion implantation layer.

[0068] Preferably, the energy of the implanted ions is 15-750keV, for example, it can be 15keV, 30keV, 50keV, 100keV, 200keV, 300keV, 400keV, 500keV, 600keV, 700keV or 750keV, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0069] Preferably, the dose of implanted ions is 5E16-1E18 ions / cm 2 , for example, 5E16ions / cm 2 、8E16ions / cm 2 、1E17ions / cm 2 、2E17ions / cm 2 、5E17ions / cm 2 、8E17ions / cm 2 or 1E18ions / cm 2 The above range is not limited to the listed values, and other values ​​not listed within the above range are also applicable.

[0070] Preferably, the implanted ions include H + and / or He + .

[0071] Preferably, in step (2), after the bonding, an annealing treatment is performed to cause the bonded body obtained by the bonding to be cleaved along the ion implantation layer, thereby obtaining the silicon carbide composite substrate and the remaining single crystal silicon carbide substrate.

[0072] In the present invention, the single crystal silicon carbide substrate can be called a donor substrate. Through the steps of ion implantation, bonding and annealing, part of the single crystal silicon carbide substrate can be transferred to a supporting substrate in the form of a film to obtain a composite substrate; and the remaining single crystal silicon carbide substrate obtained can be used as a new donor substrate for preparing a composite substrate until the single crystal silicon carbide substrate is consumed. In this way, an original piece of single crystal silicon carbide substrate material can be recycled multiple times to reduce costs.

[0073] The remaining single crystal silicon carbide substrate has undergone processing steps such as ion implantation, bonding and annealing. The ion implantation step will cause a damaged layer to appear on the wafer, and the SiC is modified to become relatively less corrosion-resistant. A large number of corrosive pit defects will appear after polishing with a traditional acidic polishing solution. However, by using the polishing solution of the present invention to polish the remaining single crystal silicon carbide substrate, the appearance of corrosive pit defects can be avoided.

[0074] In a second aspect, the present invention provides a silicon carbide composite substrate, which is prepared by the preparation method described in the first aspect.

[0075] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0076] Compared with the prior art, the present invention has the following beneficial effects:

[0077] The present invention provides a method for preparing a silicon carbide composite substrate, wherein a specific polishing liquid is used to polish the supporting substrate and the bonding surface of the single-crystal silicon carbide substrate respectively, and the polishing liquid has the following advantages:

[0078] (1) The pH value of the polishing liquid is 10-11, which is alkaline and has low corrosiveness. It will not corrode the surface of the single-crystal silicon carbide substrate and the supporting substrate, and can avoid the appearance of corrosive pit defects on the single-crystal silicon carbide substrate after polishing, thereby improving the polishing quality; and the polishing liquid has low corrosiveness, which can reduce the corrosion damage to the polishing pad, extend the service life of the polishing pad, and improve the polishing effect;

[0079] (2) Titanium carbide in the polishing liquid is an abrasive. Titanium carbide is hard and has excellent impact and wear resistance, which can improve the polishing rate. Titanium carbide has good chemical stability and good stability in the polishing liquid with a pH value of 10-11. It will not react or deform even after long-term immersion. At the same time, titanium carbide has good suspension in the polishing liquid with a pH value of 10-11, and the suspension is uniform without sedimentation or agglomeration. The polishing liquid does not need to be frequently and vigorously shaken when used. In addition, titanium carbide has good thermal conductivity. Good thermal conductivity can transfer the heat generated by mechanical friction during the polishing process to the polishing disc, and cool it down through the condensed water inside the polishing disc;

[0080] Therefore, the present invention adopts a limited polishing liquid for polishing, which can improve the polishing rate, reduce the roughness of the substrate surface and improve the polishing quality, especially can improve the polishing rate and polishing quality of the single crystal silicon carbide substrate, wherein the Si surface polishing rate can reach 10-12μm / h, the C surface polishing rate can reach 24-26μm / h, the roughness of the bonding surface of the single crystal silicon carbide substrate after polishing is 0.1-0.15nm, which can achieve atomic level flatness, thereby helping to improve the bonding quality of the silicon carbide composite substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0081] Figure 1 This is a schematic diagram of the structure of the polishing equipment used in Examples 1-2 of the present invention;

[0082] Figure 2 An atomic force microscope image of the surface to be bonded after polishing of the polished single-crystal silicon carbide substrate provided in Example 1 of the present invention;

[0083] Figure 3 An optical microscope image of the polishing pad after 30 polishings provided in Example 1 of the present invention;

[0084] Figure 4 An atomic force microscope image of the surface to be bonded after polishing of the polished single-crystal silicon carbide substrate provided in Comparative Example 1 of the present invention;

[0085] Among them, 1-polishing head; 2-part to be polished; 3-polishing liquid pipeline; 4-polishing pad; 5-polishing disc. DETAILED DESCRIPTION

[0086] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0087] Example 1

[0088] This embodiment provides a method for preparing a silicon carbide composite substrate, the preparation method comprising the following steps:

[0089] (1) providing a support substrate and a donor substrate, wherein the support substrate is a silicon carbide substrate, and its C surface is a surface to be bonded; the donor substrate is a single crystal silicon carbide substrate, and its Si surface is a surface to be bonded; using SC1 solution to wet clean the surfaces to be bonded of the support substrate and the single crystal silicon carbide substrate, wherein the volume ratio of ammonia water: hydrogen peroxide: water in the SC1 solution is 1:2:10, the concentration of ammonia water is 28%, and the concentration of hydrogen peroxide is 31%;

[0090] (2) providing a polishing liquid, wherein the polishing liquid is composed of the following components by mass fraction: 8% potassium ferrate, 5% titanium carbide, 1% sodium acetate, 0.3% KOH, 0.1% of a mixture of γ-valerolactone and sodium dodecylbenzene sulfonate, and 85.6% water, the total mass fraction of the above components is 100%, the mass ratio of γ-valerolactone to sodium dodecylbenzene sulfonate is 1:1; the particle size D50 of the titanium carbide is 150 nm; and the pH value of the polishing liquid is 10.5;

[0091] (3) polishing the surface to be bonded of the single crystal silicon carbide substrate using a polishing liquid, wherein the polishing is performed on a polishing device such as Figure 1 As shown, the polishing equipment includes a rotatable polishing head 1, a rotatable polishing disc 5, a polishing liquid pipeline 3, a pure water pipeline and a pressure applying mechanism, the bottom surface of the polishing head 1 adsorbs a workpiece 2 to be polished, and the workpiece 2 to be polished is a single-crystal silicon carbide substrate; a polishing pad 4 is arranged on the top surface of the polishing disc 5, and the material of the polishing pad 4 is non-woven fabric; the single-crystal silicon carbide substrate is located above the polishing pad 4, and the surface to be bonded of the single-crystal silicon carbide substrate is in contact with the polishing pad 4; the liquid outlet end of the polishing liquid pipeline 3 and the liquid outlet end of the pure water pipeline are both located above the polishing disc 5; the pressure applying mechanism is connected to the polishing head 1, and is used to apply pressure to the polishing head 1; the polishing liquid is introduced through the polishing liquid pipeline 3, and pre-polishing is first performed: the rotation speed of the polishing head 1 is 30rpm, the rotation speed of the polishing disc 5 is 20rpm, and the pressure of the polishing head 1 is 20rpm. is 2.5psi, the polishing liquid flow rate is 80mL / min, the polishing time is 8s, and the rotation directions of the polishing head 1 and the polishing disk 5 are both counterclockwise; then the main polishing is performed: the speed of the polishing head 1 is 90rpm, the speed of the polishing disk 5 is 80rpm, the pressure of the polishing head 1 is 8.5psi, the polishing liquid flow rate is 140mL / min, the polishing time is 10min, and the rotation directions of the polishing head 1 and the polishing disk 5 are both counterclockwise; then pure water is introduced through the pure water pipeline for surface cleaning: the speed of the polishing head 1 is 90rpm, the speed of the polishing disk 5 is 80rpm, the pressure of the polishing head 1 is 8.5psi, the pure water flow rate is 6.5L / min, the cleaning time is 40s, and the rotation directions of the polishing head 1 and the polishing disk 5 are both counterclockwise, to obtain a polished single crystal silicon carbide substrate;

[0092] (4) polishing the surface to be bonded of the support substrate using the same method as step (3) to obtain a polished support substrate;

[0093] (5) The polished single crystal silicon carbide substrate was cleaned by first using 15% citric acid for megasonic vibration, with a megasonic power of 400 W and a megasonic time of 130 s; then using a 4% hydrofluoric acid solution with a PVA wafer brush for scrubbing, with a scrubbing time of 200 s; then using a large amount of pure water to spray the substrate surface, and after the spraying of water, the substrate was rotated at high speed and sprayed with nitrogen for drying;

[0094] (6) cleaning and polishing the supporting substrate in the same manner as in step (5);

[0095] (7) The bonding surface of the cleaned single crystal silicon carbide substrate obtained in step (5) is implanted with an energy of 350 keV and a dose of 1.7E17 ions / cm 2 H + , forming an ion implantation layer; bonding the surface to be bonded of the single crystal silicon carbide substrate containing the ion implantation layer to the surface to be bonded of the cleaned supporting substrate obtained in step (6), and then annealing at 1050° C. for 6 hours to cause the bonded body to be cracked along the ion implantation layer, thereby obtaining a silicon carbide composite substrate and a remaining single crystal silicon carbide substrate.

[0096] The polished surface to be bonded of the polished single crystal silicon carbide substrate obtained in step (3) of this embodiment was observed using an atomic force microscope. The results are as follows: Figure 2 As shown, it can be seen that there are no defects under the field of view of the atomic force microscope, and a clear atomic-level surface can be obtained.

[0097] The substrate was polished using a non-woven fabric polishing pad in the same manner as in step (3) of Example 1 for a total of 30 polishings. The microscopic morphology of the polishing pad after 30 polishings was as follows: Figure 3 As shown, it can be seen that the polishing pad still has less damage after polishing 30 times.

[0098] Example 2

[0099] This embodiment provides a method for preparing a silicon carbide composite substrate, the preparation method comprising the following steps:

[0100] (1) providing a support substrate and a donor substrate, wherein the support substrate is a silicon carbide substrate, and its C surface is the surface to be bonded; the donor substrate is a single crystal silicon carbide substrate, and the C surface of the single crystal silicon carbide substrate is the surface to be bonded; using SC1 solution to wet clean the surfaces to be bonded of the support substrate and the single crystal silicon carbide substrate, wherein the volume ratio of ammonia water: hydrogen peroxide: water in the SC1 solution is 1:2:10, the concentration of ammonia water is 28%, and the concentration of hydrogen peroxide is 31%;

[0101] (2) providing a polishing liquid, wherein the polishing liquid is composed of the following components by mass fraction: 4% sodium ferrate, 3% titanium carbide, 1.3% sodium acetate, 0.2% KOH, 0.05% a mixture of pyrrolidone and sodium dodecylbenzene sulfonate, and 91.45% water, the total mass fraction of the above components is 100%, the mass ratio of pyrrolidone to sodium dodecylbenzene sulfonate is 1:1; the particle size D50 of titanium carbide is 250 nm; and the pH value of the polishing liquid is 11;

[0102] (3) polishing the surface to be bonded of the single crystal silicon carbide substrate using a polishing liquid, wherein the polishing is performed on a polishing device such as Figure 1 As shown, the polishing equipment includes a rotatable polishing head 1, a rotatable polishing disc 5, a polishing liquid pipeline 3, a pure water pipeline and a pressure applying mechanism, the bottom surface of the polishing head 1 adsorbs a workpiece 2 to be polished, and the workpiece 2 to be polished is a single-crystal silicon carbide substrate; a polishing pad 4 is arranged on the top surface of the polishing disc 5, and the material of the polishing pad 4 is a damping cloth; the single-crystal silicon carbide substrate is located above the polishing pad 4, and the surface to be bonded of the single-crystal silicon carbide substrate is in contact with the polishing pad 4; the liquid outlet end of the polishing liquid pipeline 3 and the liquid outlet end of the pure water pipeline are both located above the polishing disc 5; the pressure applying mechanism is connected to the polishing head 1, and is used to apply pressure to the polishing head 1; the polishing liquid is introduced through the polishing liquid pipeline 3, and pre-polishing is first performed: the rotation speed of the polishing head 1 is 45rpm, the rotation speed of the polishing disc 5 is 30rpm, and the pressure of the polishing head 1 is 45rpm. The force is 3psi, the polishing liquid flow rate is 90mL / min, the polishing time is 10s, and the rotation directions of the polishing head 1 and the polishing disk 5 are both counterclockwise; then the main polishing is performed: the speed of the polishing head 1 is 100rpm, the speed of the polishing disk 5 is 85rpm, the pressure of the polishing head 1 is 10psi, the polishing liquid flow rate is 180mL / min, the polishing time is 15min, and the rotation directions of the polishing head 1 and the polishing disk 5 are both counterclockwise; then pure water is introduced through the pure water pipeline for surface cleaning: the speed of the polishing head 1 is 100rpm, the speed of the polishing disk 5 is 85rpm, the pressure of the polishing head 1 is 10psi, the pure water flow rate is 7L / min, the cleaning time is 50s, and the rotation directions of the polishing head 1 and the polishing disk 5 are both counterclockwise, to obtain a polished single crystal silicon carbide substrate;

[0103] (4) polishing the surface to be bonded of the support substrate using the same method as step (3) to obtain a polished support substrate;

[0104] (5) The polished single crystal silicon carbide substrate is cleaned by first using 5% dilute sulfuric acid to vibrate it, the megasonic power is 500 W, and the megasonic time is 120 seconds; then the SC1 solution same as step (1) is used with a PVA wafer brush for scrubbing, and the scrubbing time is 180 seconds; then a large amount of pure water is used to spray the substrate surface, and after the spraying is completed, the substrate is rotated at a high speed and sprayed with nitrogen for drying;

[0105] (6) cleaning and polishing the supporting substrate in the same manner as in step (5);

[0106] (7) The bonding surface of the cleaned single crystal silicon carbide substrate obtained in step (5) is implanted with an energy of 350 keV and a dose of 1.7E17 ions / cm 2 H +, forming an ion implantation layer; bonding the surface to be bonded of the single crystal silicon carbide substrate containing the ion implantation layer to the surface to be bonded of the cleaned supporting substrate obtained in step (6), and then annealing at 1050° C. for 6 hours to cause the bonded body to be cracked along the ion implantation layer, thereby obtaining a silicon carbide composite substrate and a remaining single crystal silicon carbide substrate.

[0107] Example 3

[0108] The difference between this embodiment and embodiment 1 is that the mass fraction of titanium carbide is adjusted to 9%, and the mass fraction of water is adjusted to 81.6%.

[0109] The remaining steps and parameters remain the same as those in Example 1.

[0110] Example 4

[0111] The difference between this embodiment and embodiment 1 is that the mass of potassium ferrate is replaced by potassium permanganate.

[0112] The remaining steps and parameters remain the same as those in Example 1.

[0113] Comparative Example 1

[0114] The difference between this comparative example and Example 1 is that in step (2), the polishing liquid is composed of the following components, measured by mass fraction: 8% potassium permanganate, 5% cerium oxide, 1% sodium acetate, 0.3% HNO3, 0.1% mixture of γ-valerolactone and sodium dodecylbenzenesulfonate and 85.6% water, the total mass fraction of the above components is 100%, the mass ratio of γ-valerolactone to sodium dodecylbenzenesulfonate is 1:1, and the pH value of the polishing liquid is 3.

[0115] The remaining steps and parameters remain the same as those in Example 1.

[0116] The polished surface to be bonded of the polished single crystal silicon carbide substrate obtained in step (3) of this comparative example was observed using an atomic force microscope. The results are as follows: Figure 4 As shown, it can be seen that there are a large number of corrosion pit defects in the field of view of the atomic force microscope.

[0117] Comparative Example 2

[0118] The difference between this comparative example and Example 1 is that the mass fraction of potassium ferrate is adjusted to 11%, and the mass fraction of water is adjusted to 82.6%, so that the pH value of the polishing liquid becomes 14.

[0119] The remaining steps and parameters remain the same as those in Example 1.

[0120] Comparative Example 3

[0121] The difference between this comparative example and Example 1 is that the mass fraction of sodium acetate is adjusted to 1.5%, and the mass fraction of water is adjusted to 85.1%, so that the pH value of the polishing liquid becomes 12.

[0122] The remaining steps and parameters remain the same as those in Example 1.

[0123] Comparative Example 4

[0124] The difference between this comparative example and Example 1 is that the mass fraction of sodium acetate is adjusted to 0%, and the mass fraction of water is adjusted to 86.6%, so that the pH value of the polishing liquid becomes 8.

[0125] The remaining steps and parameters remain the same as those in Example 1.

[0126] Comparative Example 5

[0127] The difference between this comparative example and Example 1 is that the mass fraction of KOH is adjusted so that the pH value of the polishing liquid is 9.5.

[0128] The remaining steps and parameters remain the same as those in Example 1.

[0129] Comparative Example 6

[0130] The difference between this comparative example and Example 1 is that the mass fraction of KOH is adjusted so that the pH value of the polishing liquid is 11.5.

[0131] The remaining steps and parameters remain the same as those in Example 1.

[0132] The polishing rates of the surfaces to be bonded of the single crystal silicon carbide substrates in the above embodiments and comparative examples were statistically analyzed; and the roughness of the surfaces to be bonded of the single crystal silicon carbide substrates after polishing was tested by atomic force microscopy.

[0133] The results are shown in Table 1.

[0134] Table 1

[0135]

[0136] analyze:

[0137] As can be seen from Table 1, the polishing rate of the single crystal silicon carbide substrate Si surface polished by the polishing liquid in Example 1 is fast, and the roughness of the Si surface after polishing is low, and the polishing quality is good. The polishing rate of the single crystal silicon carbide substrate C surface polished by the polishing liquid in Example 2 is very fast, and the roughness of the C surface after polishing is low, and the polishing quality is good.

[0138] It can be seen from Examples 1 and 3 that if the titanium carbide content in the polishing liquid is too high, the polishing pad grooves will be clogged during polishing, forming a large number of particles, thereby causing scratch defects and affecting the roughness of the bonding surface after polishing.

[0139] It can be seen from Examples 1 and 4 that if potassium ferrate is replaced by potassium permanganate, potassium permanganate is difficult to oxidize in an alkaline environment, resulting in a decrease in the polishing rate, defects on the bonding surface of the single-crystal silicon carbide substrate after polishing, and poor roughness.

[0140] It can be seen from Example 1 and Comparative Example 1 that the use of a conventional acidic polishing liquid to polish the surface to be bonded of a single crystal silicon carbide substrate will result in a low polishing rate and poor roughness, and a large number of corrosive pit defects will appear.

[0141] It can be seen from Example 1 and Comparative Example 2 that when the polishing liquid contains too much potassium ferrate, the pH value of the polishing liquid will increase, reducing its oxidizability, resulting in a decrease in polishing rate and a deterioration in roughness.

[0142] It can be seen from Example 1 and Comparative Example 3 that when excessive sodium acetate is added, that is, when the rate accelerator is added in an excessive amount, the pH value of the polishing liquid will be too high (>11), which will reduce the oxidation ability and affect the polishing rate.

[0143] It can be seen from Example 1 and Comparative Example 4 that when the mass fraction of sodium acetate is 0%, that is, when the polishing liquid does not contain a rate accelerator, the polishing rate is significantly reduced.

[0144] It can be seen from Example 1 and Comparative Examples 5-6 that when the pH value of the polishing solution is too low, the polishing rate is significantly reduced and the roughness is slightly increased; when the pH value of the polishing solution is too high, the polishing rate is significantly reduced and the roughness is slightly increased.

[0145] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a silicon carbide composite substrate, characterized in that: The preparation method comprises: (1) polishing the surface to be bonded of the support substrate and the surface to be bonded of the single-crystal silicon carbide substrate respectively using a polishing liquid to obtain a polished support substrate and a polished single-crystal silicon carbide substrate; The polishing liquid comprises an oxidant, titanium carbide, a pH regulator, a dispersant and a solvent; the pH value of the polishing liquid is 10-11; (2) The polished support substrate and the polished single-crystal silicon carbide substrate are pretreated separately and then bonded to obtain a silicon carbide composite substrate.

2. The preparation method according to claim 1, characterized in that: The oxidant includes ferrate; Preferably, the ferrate comprises potassium ferrate and / or sodium ferrate; Preferably, the particle size D50 of the titanium carbide is 100-300 nm; Preferably, the pH adjuster comprises H2O2 and / or KOH; Preferably, the dispersant comprises a pyrrolidone substance and / or a sulfonate, preferably a combination of a pyrrolidone substance and a sulfonate; Preferably, the solvent comprises water.

3. The preparation method according to claim 1 or 2, characterized in that: The polishing liquid also includes a rate accelerator; Preferably, the rate accelerator comprises a carboxylate; Preferably, the carboxylate salt comprises at least one of sodium acetate, potassium acetate and calcium acetate.

4. The preparation method according to claim 3, characterized in that: Based on the total mass of the polishing liquid being 100%, the mass fraction of the oxidant is ≤10%; Preferably, based on the total mass of the polishing liquid being 100%, the mass fraction of the titanium carbide is ≤8%; Preferably, based on the total mass of the polishing liquid being 100%, the mass fraction of the rate accelerator is ≤1.4%; Preferably, based on the total mass of the polishing liquid being 100%, the mass fraction of the pH regulator is ≤0.5%; Preferably, based on the total mass of the polishing liquid being 100%, the mass fraction of the dispersant is ≤0.1%; Preferably, based on the total mass of the polishing liquid being 100%, the mass fraction of the solvent is ≥80%.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The material of the polishing pad used for polishing includes any one of damping cloth, PU material, polyurethane and non-woven fabric.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The polishing includes pre-polishing and main polishing which are performed sequentially; Preferably, the specific parameters of the pre-polishing include: a polishing head speed of 10-50 rpm, a polishing disc speed of 10-50 rpm, a polishing head pressure of 1-4 psi, a polishing liquid flow rate of 50-100 mL / min, and a polishing time of 5-10 s; Preferably, during the pre-polishing process, the polishing head and the polishing disc have different rotation speeds; Preferably, during the pre-polishing process, the polishing head and the polishing disc rotate counterclockwise; Preferably, the specific parameters of the main polishing include: polishing head speed of 50-120rpm, polishing disc speed of 50-120rpm, polishing head pressure of 5-12psi, polishing liquid flow rate of 80-200mL / min, polishing time of 1-20min; Preferably, during the main polishing process, the polishing head and the polishing disc have different rotation speeds; Preferably, during the main polishing process, the polishing head and the polishing disc rotate counterclockwise.

7. The preparation method according to claim 6, characterized in that: During the polishing process, after the main polishing, a surface cleaning step is also performed; Preferably, the specific parameters of the surface cleaning include: polishing head speed of 50-120rpm, polishing disc speed of 50-120rpm, polishing head pressure of 5-12psi, pure water flow of 5-8L / min, and cleaning time of 20-60s; Preferably, during the surface cleaning process, the polishing head and the polishing disc have different rotation speeds; Preferably, during the surface cleaning process, the polishing head and the polishing disc rotate in a counterclockwise direction.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The pretreatment in step (2) includes a cleaning step; Preferably, the cleaning comprises megasonic vibration, brushing and drying in sequence; Preferably, the specific parameters of the megasonic vibration include: megasonic power of 200-600W, megasonic time of 80-180s; Preferably, the scrubbing time is 120-300s.

9. The preparation method according to claim 8, characterized in that: The pretreatment in step (2) further includes: implanting ions into the surface to be bonded of the cleaned single crystal silicon carbide substrate to form an ion implantation layer; Preferably, in step (2), after the bonding, an annealing treatment is performed to cause the bonded body obtained by the bonding to be cleaved along the ion implantation layer, thereby obtaining the silicon carbide composite substrate and the remaining single crystal silicon carbide substrate.

10. A silicon carbide composite substrate, characterized in that: The silicon carbide composite substrate is prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Polishing liquid for ultra-precision sharpening of diamond cutting tool and preparation method thereof

    CN102516874A

  • Composite substrate manufacturing method and composite substrate

    CN107004573A

  • Ferrate-containing silicon carbide polishing solution and preparation method and application thereof

    CN111748285A

  • METHOD FOR POLISHING SiC SUBSTRATE

    JP2022066931A

  • Polishing composition and polishing method

    US20200123413A1