Composite film for milk powder packaging and preparation process thereof
By modifying the sodium-based montmorillonite nanosheets with light-blocking coupling agent and preparing the photo-blocking and water-blocking EVOH composite material, the multi-layer co-extrusion blow molding film forming process is used to solve the moisture-proof and light-proof properties of milk powder packaging materials. The problem of insufficient results has achieved significantly improved water and light blocking effects.
Patent Information
- Application Number
- CN202411104652.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-19
AI Technical Summary
The existing milk powder packaging materials have shortcomings in moisture-proof and light-blocking properties, especially the moisture-resistant properties of ethylene-vinyl alcohol copolymers in plastic flexible packaging composite films are greatly affected by humidity, and light will promote the oxidative degradation of vitamin C in milk powder. It is necessary to improve the photo-blocking and water-blocking performance.
Design and synthesize photo-blocking water-resisting modifiers, and prepare photo-blocking water-resisting EVOH composite materials by modifying sodium-based montmorillonite nanosheets, and blow-molded films using multi-layer coextrusion Process, a composite film with a five-layer coextruded film structure was prepared, including low-density polyethylene resin, maleic anhydride grafted polyethylene resin and photo-blocking and water-blocking functionally modified EVOH composite material as intermediate layers.
It significantly improves the water and light-blocking properties of the composite film, and reduces the water vapor transmission to 0.04~0.1[g/(m2·24h), and controls the light transmittance to 25~35%, meeting the moisture-proof and light-proof requirements of milk powder packaging. .
Smart Images

Figure CN118977447A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of research and development of milk powder packaging materials, in particular to a composite film for milk powder packaging and a preparation process thereof. Background Art
[0002] Milk powder is a dry product with very low moisture content. It is easy to absorb moisture and agglomerate during storage, which accelerates the process of lactose crystallization, non-enzymatic browning and oxidative rancidity. At present, the common packaging forms of milk powder mainly include aluminum foil composite film, aluminum-plated composite film, paper box, metal iron can and plastic flexible packaging composite film. Among them, plastic flexible packaging composite materials have gradually become one of the mainstream packaging methods due to their good flexibility, excellent impact resistance and low price.
[0003] Plastic flexible packaging composite films usually use ethylene-vinyl alcohol copolymer as a barrier layer, but the hydroxyl groups in traditional ethylene-vinyl alcohol copolymers are easily combined with water in the environment to form hydrogen bonds, and their moisture barrier properties are greatly affected by humidity, which limits their practical application in the packaging field. At present, the methods for improving the moisture resistance of materials mainly include surface coating modification, multi-layer composite modification, blending modification, and nano-composite modification. For example, the patent with authorization number CN102408624B discloses a montmorillonite-EVOH-PET composite material and its preparation method. The moisture barrier properties of the material can be improved by the interaction of modified montmorillonite with ethylene-vinyl alcohol copolymer and polyethylene terephthalate.
[0004] The search found that montmorillonite nanosheets have good barrier properties for small molecules and can significantly improve their moisture resistance when compounded with polymers, while unmodified montmorillonite has strong hydrophilicity and is difficult to achieve good dispersion in the polymer matrix. Currently, there are two main ways to modify montmorillonite: surfactant modification and coupling agent modification.
[0005] In addition, light will promote the oxidative degradation of vitamin C in milk powder, so the light-blocking performance of milk powder packaging materials is also crucial. Further search found that benzotriazole compounds are common ultraviolet absorbers that can inhibit light and effectively protect food and materials from damage by ultraviolet rays. Summary of the invention
[0006] The present invention provides a composite film for milk powder packaging and a preparation process thereof. A light-blocking and water-blocking modifier is designed, synthesized and prepared, and the existing milk powder packaging material is modified by the composite film, thereby achieving the technical goal of improving the light-blocking and water-blocking properties of the existing milk powder packaging material.
[0007] A preparation process of a light-blocking and water-blocking composite film comprises the following steps:
[0008] Step 1: preparing a light-blocking and water-blocking functional modified EVOH composite material, wherein the preparation method comprises: modifying sodium montmorillonite nanosheets with a light-blocking coupling agent to obtain a light-blocking and water-blocking modifier, and uniformly dispersing the modifier in an ethylene-vinyl alcohol copolymer matrix to prepare a light-blocking and water-blocking functional modified EVOH composite material;
[0009] Step 2: A multi-layer co-extrusion blow molding film forming process is adopted, using low-density polyethylene resin as the raw material for the inner and outer layers, light-blocking and water-blocking functional modified EVOH composite material as the raw material for the middle layer, and maleic anhydride grafted polyethylene resin as the raw material for the bonding layer to prepare a light-blocking and water-blocking composite film.
[0010] Preferably, the light-blocking coupling agent is light-blocking coupling agent I and / or light-blocking coupling agent II.
[0011] Preferably, the preparation method of the light-blocking coupling agent I is: utilizing a nucleophilic substitution reaction mechanism to generate a light-blocking coupling agent I by a thioesterification reaction between the carboxyl functional group of 3-(2-benzotriazolyl)-4-hydroxy-5-tert-butylbenzenepropionic acid and the mercapto functional group of 3-mercaptopropyltrimethoxysilane.
[0012] Preferably, the preparation method of the light-blocking coupling agent II is:
[0013] Step S1: generating a tertiary amine monomer by esterifying the carboxyl functional group of 3-(2-benzotriazolyl)-4-hydroxy-5-tert-butylbenzenepropionic acid with the hydroxyl functional group of 3-dimethylamino-1-propanol;
[0014] Step S2: utilizing a nucleophilic substitution reaction mechanism to generate a carboxyammonium bromide monomer by reacting the tertiary amine group of the tertiary amine monomer with the bromine functional group of 4-bromobutyric acid to undergo a quaternization reaction;
[0015] Step S3: utilizing the nucleophilic substitution reaction mechanism, the carboxyl functional group of the carboxyammonium bromide monomer and the mercapto functional group of 3-mercaptopropyltrimethoxysilane undergo a thioesterification reaction to generate a light-blocking coupling agent II.
[0016] Preferably, the preparation method of the light-blocking and water-blocking composite film in the step two is: first set up a membrane structure of a five-layer co-extruded film, and then sequentially put the raw materials of each layer of the film into the corresponding hoppers of the five screw extruders of the five-layer co-extruded film blow molding unit, after stirring and mixing, the molten resin is converged at the head of the machine through a diverter, and is blown and extruded through a die head to obtain a light-blocking and water-blocking composite film.
[0017] A light-blocking and water-blocking composite film prepared according to the above process is a five-layer co-extruded film, and the structure of the five-layer co-extruded film is an inner layer, a bonding layer, a middle layer, a bonding layer, and an outer layer;
[0018] The mass ratio of the inner layer, the bonding layer, the middle layer, the bonding layer and the outer layer in the five-layer co-extruded film is (30-50): (1-10): (10-30): (1-10): (30-50).
[0019] Preferably, the water vapor permeability of the composite membrane is 0.04 to 0.1 [g / (m 2 ·24h)], light transmittance is 25-35%;
[0020] The light-blocking and water-blocking composite film prepared according to the above process is used in milk powder packaging.
[0021] Beneficial Effects
[0022] The present invention first designs and synthesizes two light-blocking coupling agents, then uses the light-blocking coupling agents to modify montmorillonite nanosheets to prepare modified montmorillonite, and evenly disperses the modified montmorillonite in an ethylene-vinyl alcohol copolymer matrix to prepare a new EVOH / MMT composite material. The new EVOH / MMT composite material is used as the raw material for the light-blocking and water-blocking functional layer, and a multi-layer co-extrusion blow molding film-forming process is adopted to prepare a composite film, which achieves the beneficial technical effect of significantly improving the water-blocking and light-blocking properties of the film material. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The performance test results of the composite membrane. DETAILED DESCRIPTION
[0024] Experimental Example 1:
[0025] The light-blocking coupling agent I was prepared, and its synthesis route is as follows:
[0026]
[0027] The preparation method of light-blocking coupling agent I is as follows: using a nucleophilic substitution reaction mechanism, a carboxyl functional group of 3-(2-benzotriazolyl)-4-hydroxy-5-tert-butylbenzenepropionic acid and a mercapto functional group of 3-mercaptopropyltrimethoxysilane undergo a thioesterification reaction to generate light-blocking coupling agent I. The specific experimental steps are as follows: 1.7 g of 3-(2-benzotriazolyl)-4-hydroxy-5-tert-butylbenzenepropionic acid, 1.0 g of 3-mercaptopropyltrimethoxysilane, 0.5 g of p-toluenesulfonic acid and 50 mL of cyclohexane are added to a three-necked flask, the temperature is raised to 85° C. and refluxed for 6 hours under mechanical stirring, the cyclohexane is recovered by reduced pressure distillation, and the mixture is washed with a saturated sodium bicarbonate aqueous solution and deionized water to neutrality, filtered, and dried to obtain light-blocking coupling agent I;
[0028] The H NMR spectrum of the light-blocking coupling agent I is characterized as follows: 1H NMR (CDCl3, 400MHz) δ: 0.68-0.70 (t, 2H), 1.40 (s, 9H), 1.82-1.88 (m, 2H), 2.83-2.96 (m, 6H), 3.57 (s, 9H), 7.03-7.74 (m, 6H, Ar-H).
[0029] Experimental Example 2:
[0030] The light-blocking coupling agent II is prepared by the following synthetic route:
[0031]
[0032] The preparation process of light-blocking coupling agent II is as follows:
[0033] (1) Synthesizing a tertiary amine monomer, wherein the synthesis method comprises: generating a tertiary amine monomer by an esterification reaction between the carboxyl functional group of 3-(2-benzotriazolyl)-4-hydroxy-5-tert-butylbenzenepropionic acid and the hydroxyl functional group of 3-dimethylamino-1-propanol, wherein the specific experimental steps are: adding 1.7 g of 3-(2-benzotriazolyl)-4-hydroxy-5-tert-butylbenzenepropionic acid, 0.5 g of 3-dimethylamino-1-propanol and 50 mL of cyclohexane into a three-necked flask, adding 1 mL of concentrated sulfuric acid dropwise into the three-necked flask under mechanical stirring, heating to 85° C. and reflux reaction for 6 h, recovering cyclohexane by vacuum distillation, washing with a saturated sodium bicarbonate aqueous solution and deionized water to neutrality, filtering and drying to obtain a tertiary amine monomer;
[0034] (2) Synthesizing carboxyammonium bromide monomer, the synthesis method of which is: utilizing the nucleophilic substitution reaction mechanism, the tertiary amine group of the tertiary amine monomer reacts with the bromine functional group of 4-bromobutyric acid to generate carboxyammonium bromide monomer, the specific experimental steps are: adding 1.1g of tertiary amine monomer and cyclohexane into a three-necked flask, under nitrogen protection and mechanical stirring, heating to 40°C, after the temperature stabilizes, adding 10mL of 3-bromobutyric acid solution (prepared with 0.5g of 3-bromobutyric acid and 10mL of cyclohexane) dropwise into the three-necked flask, maintaining the temperature at 40°C for 12h, and after cooling, rotary evaporation, washing with ethyl acetate, and vacuum drying to obtain carboxyammonium bromide monomer;
[0035] (3) Synthesizing a light-blocking coupling agent II, wherein the synthesis method is as follows: utilizing a nucleophilic substitution reaction mechanism, a carboxyl functional group of carboxyammonium bromide monomer and a mercapto functional group of 3-mercaptopropyltrimethoxysilane undergo a thioesterification reaction to generate a light-blocking coupling agent II, wherein the specific experimental steps are as follows: adding 1.5 g of carboxyammonium bromide monomer, 1.0 g of 3-mercaptopropyltrimethoxysilane, 0.5 g of p-toluenesulfonic acid and 50 mL of cyclohexane into a three-necked flask, heating to 75° C. and stirring for 10 h, recovering cyclohexane by vacuum distillation, washing with a saturated sodium bicarbonate aqueous solution and deionized water in turn until neutral, filtering and drying to obtain a light-blocking coupling agent II;
[0036] The nuclear magnetic resonance hydrogen spectrum of the light-blocking coupling agent II is characterized as follows: 1 H NMR (CDCl3, 400MHz) δ: 0.68-0.70 (t, 2H), 1.38 (s, 9H), 1.85-2.12 (m, 6H), 2.60-2.95 (m, 8H), 3. 31(s, 6H), 3.57-3.66(m, 13H), 3.57-3.66(m, 13H), 4.18-4.21(t, 2H), 7.03-7.74(m, 6H, Ar-H).
[0037] Embodiment 1:
[0038] (1) Prepare modified montmorillonite I, the preparation method of which is: modify sodium montmorillonite nanosheets with light-blocking coupling agent I to obtain modified montmorillonite I, the specific experimental steps are: add 1g of light-blocking coupling agent I, 20mL of methanol and 30mL of deionized water into a three-necked flask, add glacial acetic acid dropwise to adjust the pH to 4.5, heat to 50°C and stir for 2h, then continue to heat to 80°C under mechanical stirring, add 5g of sodium montmorillonite nanosheets into the three-necked flask and reflux for 3h, cool to room temperature, wash with methanol, precipitate, centrifuge, and dry to obtain modified montmorillonite I;
[0039] (2) preparing modified montmorillonite II, wherein the preparation method is as follows: modifying montmorillonite nanosheets with a light-blocking coupling agent II to obtain modified montmorillonite II. The specific experimental steps refer to the preparation experiment of modified montmorillonite I. The difference between the modified montmorillonite II and the preparation experiment of modified montmorillonite I is that the light-blocking coupling agent II is used to replace the light-blocking coupling agent I.
[0040] The sodium montmorillonite nanosheets were purchased from Zhejiang Fenghong Clay Co., Ltd., with the following specifications: purity 75%, cation exchange capacity 100 mmol / 100 g, and fineness 200 mesh.
[0041] Embodiment 2:
[0042] (1) EVOH / MMT composite material I was prepared. The preparation method was as follows: modified montmorillonite I was uniformly dispersed in an ethylene-vinyl alcohol copolymer matrix to prepare EVOH / MMT composite material I. The specific experimental steps were as follows: 25 g ethylene-vinyl alcohol copolymer resin and 100 mL N, N-dimethylformamide were added to a three-necked flask, the temperature was raised to 100°C and stirred until completely dissolved, 20 mL modified montmorillonite I solution (prepared with 2 g modified montmorillonite I and 20 mL N, N-dimethylformamide) was slowly added dropwise to the three-necked flask, the temperature was raised to 120°C and stirred for reaction for 2 h, the solution after the reaction was completed was poured into a polytetrafluoroethylene mold while hot, and dried in an oven at 60°C, 80°C, and 100°C for 12 h, respectively, to obtain EVOH / MMT composite material I.
[0043] (2) preparing EVOH / MMT composite material II, wherein the preparation method is as follows: uniformly dispersing modified montmorillonite II in an ethylene-vinyl alcohol copolymer matrix to prepare EVOH / MMT composite material II. The specific experimental steps refer to the preparation experiment of EVOH / MMT composite material I. The difference between the preparation experiment of EVOH / MMT composite material I and the preparation experiment of EVOH / MMT composite material I is that modified montmorillonite II is used to replace modified montmorillonite I.
[0044] The ethylene-vinyl alcohol copolymer resin was purchased from Dongguan Kaixili Plastic Raw Materials Co., Ltd., and its specifications are: E105B, Mn-10000, and ethylene content 44%.
[0045] Embodiment three:
[0046] (1) Preparing composite membrane I, comprising the following steps:
[0047] Step 1: Set the composite film I as a five-layer co-extruded film, and its film structure is as follows:
[0048] First layer: low-density polyethylene resin layer, 35 parts by weight;
[0049] Second layer: maleic anhydride grafted polyethylene resin layer, 5 parts by weight;
[0050] The third layer: 20 parts by weight of ethylene-vinyl alcohol copolymer resin layer prepared with EVOH / MMT composite material I as raw material;
[0051] The fourth layer: maleic anhydride grafted polyethylene resin layer, 5 parts by weight;
[0052] Fifth layer: low-density polyethylene resin layer, 35 parts by weight;
[0053] Step 2, respectively putting the raw materials in step 1 into a five-layer co-extrusion film blowing unit, melt extruding, merging at the mouth of the five-layer die head through their respective flow channels, and then undergoing inflation molding, with the inflation ratio controlled at 2.7, cooling, and winding to obtain a composite film I with a thickness of 80 μm;
[0054] The process parameters of the screw extruder corresponding to the low-density polyethylene resin layer are set as follows: the temperatures of zones 1-3 are 120°C, 150°C, and 170°C, respectively, the flow channel temperature is 165°C, and the rotation speed is 30r / min;
[0055] The process parameters of the screw extruder corresponding to the maleic anhydride grafted polyethylene resin layer were set as follows: the temperatures of zones 1-3 were 125°C, 150°C, and 165°C, respectively, the flow channel temperature was 160°C, and the rotation speed was 15 r / min;
[0056] The process parameters of the screw extruder corresponding to the ethylene-vinyl alcohol copolymer resin layer are set as follows: the temperatures of zones 1-3 are 180°C, 200°C, and 210°C, respectively, the flow channel temperature is 205°C, and the rotation speed is 40r / min.
[0057] Among them, the low-density polyethylene resin was purchased from CNOOC Shell Petrochemical Co., Ltd., with the specifications of 2420H, Mn-180000, MFR 2.0-2.5g / 10min; the maleic anhydride grafted low-density polyethylene resin was purchased from Dongguan Taotao Plastic Raw Materials Co., Ltd., with the specifications of 4288, Mn-130000, and grafting rate 4.5%.
[0058] (2) Preparation of composite membrane II: EVOH / MMT composite material II was used to replace the above EVOH / MMT composite material I, referring to the preparation steps and experimental conditions of composite membrane I, to prepare composite membrane II.
[0059] (3) Preparation of composite membrane: See the preparation steps and experimental conditions of composite membrane I. The difference between this method and the preparation experiment of composite membrane I is that EVOH / MMT composite material I is replaced by ethylene-vinyl alcohol copolymer resin to prepare the composite membrane.
[0060] Performance Test:
[0061] (1) Moisture resistance: The water vapor transmission rate of the sample is tested according to GB / T 1037-2021 "Determination of water vapor transmission rate of plastic films and sheets - Cup weight gain and weight loss method". The specific test steps are as follows: a 30 cm circular film sample is placed in a glass desiccator at an ambient temperature of 25°C and anhydrous calcium chloride is used as a desiccant for 72 hours, and then the moisture resistance is tested using a W3 / 060 water vapor transmission rate tester;
[0062] (2) Light blocking performance: Lambda 950 UV-visible spectrophotometer was used to test the light transmittance of the samples in accordance with GB / T2410-2008 “Determination of light transmittance and haze of transparent plastics”. The test wavelength range was 250-800 nm, and the light transmittance of the samples at 380 nm was recorded.
[0063] (3) Mechanical properties: The tensile strength of the samples was tested using an Instron 5565 universal tensile testing machine. The specific test steps are as follows: a 30 mm × 5 mm sample was fixed on the tensile testing machine and a tensile test was performed at a tensile rate of 5 mm / min. The longitudinal and transverse tensile strengths were recorded respectively.
[0064] The above experimental results are shown in Table 1 and Figure 1 .
[0065] Table 1 Performance test results of composite membrane
[0066]
[0067] The hygienic properties of the samples were tested according to GB / T 5009.60-2003 "Analysis Method for Hygienic Standards of Polyethylene, Polystyrene and Polypropylene Molded Products for Food Packaging", and the experimental results confirmed that the composite film prepared by the present invention can meet the requirements of the hygienic standards;
[0068] By comprehensively analyzing the above experimental results, the following conclusions can be drawn:
[0069] The novel composite film developed by the present invention achieves significantly improved technical effects in terms of water-blocking and light-blocking properties.
Claims
1. A process for preparing a light-blocking and water-blocking composite film, characterized in that: The following steps are involved: Step 1: preparing a light-blocking and water-blocking functional modified EVOH composite material, wherein the preparation method comprises: modifying sodium montmorillonite nanosheets with a light-blocking coupling agent to obtain a light-blocking and water-blocking modifier, and uniformly dispersing the modifier in an ethylene-vinyl alcohol copolymer matrix to prepare a light-blocking and water-blocking functional modified EVOH composite material; Step 2: A multi-layer co-extrusion blow molding film forming process is adopted, using low-density polyethylene resin as the raw material for the inner and outer layers, light-blocking and water-blocking functional modified EVOH composite material as the raw material for the middle layer, and maleic anhydride grafted polyethylene resin as the raw material for the bonding layer to prepare a light-blocking and water-blocking composite film.
2. The process for preparing a light-blocking and water-blocking composite film according to claim 1, characterized in that: The light-blocking coupling agent is light-blocking coupling agent I and / or light-blocking coupling agent II.
3. The process for preparing a light-blocking and water-blocking composite film according to claim 2, characterized in that: The preparation method of the light-blocking coupling agent I is as follows: utilizing a nucleophilic substitution reaction mechanism, a carboxyl functional group of 3-(2-benzotriazolyl)-4-hydroxy-5-tert-butylbenzenepropionic acid and a mercapto functional group of 3-mercaptopropyltrimethoxysilane undergo a thioesterification reaction to generate the light-blocking coupling agent I.
4. The process for preparing a light-blocking and water-blocking composite film according to claim 2, characterized in that: The preparation method of the light-blocking coupling agent II is as follows: Step S1: generating a tertiary amine monomer by esterifying the carboxyl functional group of 3-(2-benzotriazolyl)-4-hydroxy-5-tert-butylbenzenepropionic acid with the hydroxyl functional group of 3-dimethylamino-1-propanol; Step S2: utilizing a nucleophilic substitution reaction mechanism to generate a carboxyammonium bromide monomer by reacting the tertiary amine group of the tertiary amine monomer with the bromine functional group of 4-bromobutyric acid to undergo a quaternization reaction; Step S3: utilizing the nucleophilic substitution reaction mechanism, the carboxyl functional group of the carboxyammonium bromide monomer and the mercapto functional group of 3-mercaptopropyltrimethoxysilane undergo a thioesterification reaction to generate a light-blocking coupling agent II.
5. The process for preparing a light-blocking and water-blocking composite film according to claim 1, characterized in that: The preparation method of the light-blocking and water-blocking composite film in the step 2 is: first set up a film structure of a five-layer co-extruded film, then sequentially put the raw materials of each layer of the film into the corresponding hoppers of the five screw extruders of the five-layer co-extruded film blow molding unit, after stirring and mixing, the molten resin is converged at the head of the machine through a diverter, and is blown and extruded through a die head to obtain a light-blocking and water-blocking composite film.
6. A light-blocking and water-blocking composite film prepared by the process according to any one of claims 1 to 5, characterized in that: The light-blocking and water-blocking composite film is a five-layer co-extruded film, and the structure of the five-layer co-extruded film is an inner layer, a bonding layer, a middle layer, a bonding layer, and an outer layer; The mass ratio of the inner layer, the bonding layer, the middle layer, the bonding layer and the outer layer in the five-layer co-extruded film is (30~50):(1~10):(10~30):(1~10):(30~50).
7. The light-blocking and water-blocking composite film according to claim 6, characterized in that: The water vapor permeability of the composite film is 0.04-0.1 [g / (m 2 •24h)], light transmittance is 25~35%.
8. Use of a light-blocking and water-blocking composite film prepared according to the process according to any one of claims 1 to 5 in milk powder packaging.
Citation Information
Cited By
Seven-layer co-extrusion pesticide-resistant high-barrier agricultural film and production process thereof
CN120003138A