Preparation method of antibacterial composite fabric

Through the design of cotton yarn with low titanium dioxide attached and nylon yarn with high titanium dioxide attached and wear-resistant layer, the problem of antibacterial fabrics damaging softness and breathability when improving antibacterial properties is solved, and efficient antibacterial properties and durability are achieved. , extends the service life of the fabric.

CN118977476AInactive Publication Date: 2024-11-19山东荣沣纺织有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411066795.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When existing antibacterial fabrics improve antibacterial properties, they can easily damage the softness and breathability of cotton fibers. The coating of nylon yarn with high amount of titanium dioxide may cause shedding, making it difficult to maintain the comprehensive performance of the mixed fabric.

Method used

The antibacterial layer is mixed with cotton yarn with low titanium dioxide and nylon yarn with high titanium dioxide, and a wear-resistant layer is set on the outside. The wear-resistant layer is fixed by titanate hydrolysis and alkali treatment, combined with hot pressing to ensure the fabric Antibacterial properties and durability.

Benefits of technology

While maintaining the breathability and softness of the fabric, it significantly improves antibacterial properties and wear resistance, extends service life, and avoids the problem of titanium dioxide falling off.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a preparation method of a fabric, in particular to a preparation method of an antibacterial composite fabric. According to the invention, the characteristic that the hydrolysis of inherent wax and titanate on the raw cotton yarns needs alkali liquor treatment is utilized, and the composite fabric formed by the antibacterial layer formed by blending the cotton yarns with low titanium dioxide adhesion and the nylon yarns with high titanium dioxide adhesion and the wear-resistant layer with a protection effect is designed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a fabric, and in particular to a method for preparing an antibacterial composite fabric. Background Art

[0002] Antibacterial fabric is a widely used textile material. Its research and development background stems from people's continuous attention to health and hygiene. With the acceleration of the pace of modern life, people pay more and more attention to the cleanliness and hygiene of the living environment. Especially in public places, medical environments and personal daily life, it is very important to reduce the spread of bacteria and viruses. Therefore, antibacterial fabric came into being. It can not only effectively inhibit the growth of bacteria, but also reduce the risk of cross infection, providing an extra layer of protection for people's health.

[0003] Among the many antibacterial technologies, the use of titanium dioxide for fabric antibacterial is an important existing technology. As a photocatalyst, titanium dioxide can produce a strong oxidation effect under light conditions, thereby effectively killing or inhibiting the growth of bacteria. Applying titanium dioxide to fabrics can not only give the fabrics excellent antibacterial properties, but also maintain the comfort and durability of the fabrics. The emergence of this technology has injected new vitality into the development of antibacterial fabrics, making them more widely used in medical, home, public health and other fields.

[0004] In the prior art, the blended fabric of cotton yarn and nylon yarn has good comprehensive performance. It has both the air permeability and softness of cotton fiber and the wear resistance and durability of nylon fiber. In order to improve the antibacterial performance of the fabric, titanium dioxide is usually coated on the fabric. In order to achieve a high antibacterial effect, a high amount of titanium dioxide is often required. However, for cotton fiber, too high an amount of titanium dioxide adhesion may weaken its softness and air permeability, thereby losing the comprehensive performance of the blended fabric. Although a high amount of titanium dioxide coated on nylon yarn can increase its antibacterial performance, it may cause the titanium dioxide to fall off due to friction. Therefore, it is necessary to provide a composite fabric and a preparation method thereof that can maintain the air permeability and softness of the blended fabric and enhance its antibacterial performance. Summary of the invention

[0005] In view of the above problems, the present invention has been carefully designed to propose a new method for preparing antibacterial composite fabrics. By utilizing the fact that the hydrolysis of wax and titanate inherent in raw cotton fibers both requires alkali treatment, a composite fabric is designed, which is composed of an antibacterial layer mixed with cotton yarn with low titanium dioxide attachment and nylon yarn with high titanium dioxide attachment, and a protective wear-resistant layer.

[0006] Specifically, the present invention provides a method for preparing an antibacterial composite fabric, the antibacterial composite fabric comprising an inner antibacterial layer and an outer wear-resistant layer, the antibacterial layer being formed by mixing cotton yarn and nylon yarn, the wear-resistant layer being arranged on the outer side of the inner antibacterial layer, the preparation method comprising the following steps:

[0007] (1) Blending raw cotton yarn and nylon yarn in a ratio of 20:80 to 30:70 to form a blended fabric;

[0008] (2) dipping the blended fabric into a titanate precursor solution with a concentration of 5-10 wt% for 5-10 minutes, and drying the mixture;

[0009] (3) hydrolyzing the impregnated and dried fabric in an alkaline solution with a pH of 9-12 and a temperature of 80-100° C. for 1-4 hours;

[0010] (4) Cleaning and drying the treated fabric;

[0011] (5) Compounding a wear-resistant layer on the outer side of the treated fabric.

[0012] Preferably, the wax content in the raw cotton yarn is 0.3-0.5 wt%.

[0013] Preferably, the amount of titanium dioxide attached to the cotton yarn in the inner antibacterial layer is 0.1-0.5w%.

[0014] Preferably, the attachment amount of titanium dioxide on the nylon yarn in the inner antibacterial layer is 1-2w%.

[0015] Preferably, the outer wear-resistant layer is made of polyester fiber material, and the single yarn strength is 500-700 cN.

[0016] Preferably, the thickness of the antibacterial layer is 0.5-1.5 mm, and the thickness of the wear-resistant layer is 0.3-0.7 mm.

[0017] Preferably, the wear-resistant layer is fixed to the outer side of the fabric by hot pressing, the hot pressing temperature is 150-180 degrees Celsius, and the pressure is 2-4 MPa.

[0018] Preferably, the titanate is selected from one of tetraisopropoxytitanium, tetraethoxytitanium and tetra-n-butoxytitanium.

[0019] Preferably, the alkali solution is an aqueous solution of sodium hydroxide or potassium hydroxide.

[0020] Preferably, in step (4), the drying temperature is 60-80° C. and the drying time is 6-12 h.

[0021] Compared with the prior art, the present invention shows significant advantages in the preparation of antibacterial composite fabrics. First, the present invention cleverly utilizes the common requirements of the removal of wax from raw cotton yarns and the hydrolysis of titanate for an alkaline environment, and selects raw cotton yarns with a specific wax content and nylon yarns for mixed weaving. After impregnation with a titanate precursor solution and scouring with an alkali solution, the mixed weaving of cotton yarns with low titanium dioxide attachment and nylon yarns with high titanium dioxide attachment is achieved, thereby forming an antibacterial fabric. This design not only ensures the overall antibacterial properties of the fabric, but also enhances the strength and durability of nylon through nylon yarns with high titanium dioxide attachment, while cotton yarns with low titanium dioxide attachment maintain the air permeability and softness of cotton fibers.

[0022] Secondly, the present invention has carried out fine optimization of parameters such as the wax content of the raw cotton yarn, the pH value of the alkali solution, the temperature and the hydrolysis time, thereby ensuring that while removing the wax of the raw cotton yarn, the best adhesion of titanium dioxide to the yarn is achieved, thereby maintaining the antibacterial properties of the fabric while maintaining the comfort of the fabric.

[0023] More importantly, the present invention sets a wear-resistant layer on the outside of the antibacterial layer. This innovative design effectively solves the problem of high titanium dioxide easily falling off. The wear-resistant layer not only enhances the wear resistance of the fabric, but also protects the titanium dioxide in the inner antibacterial layer, thereby further extending the service life and antibacterial effect of the fabric.

[0024] In summary, the present invention prepares an antibacterial composite fabric with excellent antibacterial properties and good comfort and durability through an innovative preparation method and fine parameter optimization, which provides a new direction for the technological progress and application of antibacterial fabrics. DETAILED DESCRIPTION

[0025] Embodiment 1:

[0026] This embodiment provides a specific method for preparing an antibacterial composite fabric, and the specific steps of the method are as follows:

[0027] (1) Preparation of blended fabrics:

[0028] The raw cotton yarn with a wax content of 0.4 wt% is selected and blended with the nylon yarn in a ratio of 25:75 to form a blended fabric.

[0029] (2) Impregnation treatment:

[0030] The mixed fabric was immersed in a tetraisopropoxy titanium precursor solution with a concentration of 8 wt % for 8 minutes, and then dried.

[0031] (3) Hydrolysis treatment:

[0032] The impregnated and dried fabric was placed in a sodium hydroxide aqueous solution at a pH of 10 and a temperature of 90° C. for hydrolysis treatment, and the hydrolysis time was set to 2.5 hours.

[0033] (4) Cleaning and drying:

[0034] The hydrolyzed fabric was thoroughly washed and then dried at 70°C for 9 hours.

[0035] (5) Composite wear-resistant layer:

[0036] The wear-resistant layer made of polyester fiber material was selected, and its single yarn strength was 600cN. The wear-resistant layer was fixed on the outside of the treated mixed fabric by hot pressing, and the hot pressing temperature was set to 165℃ and the pressure was 3MPa, thereby forming an antibacterial composite fabric. According to the test, the amount of titanium dioxide attached to the cotton yarn in the antibacterial layer was 0.31w%, and the amount of titanium dioxide attached to the nylon yarn was 1.52w%.

[0037] Characterization:

[0038] Antimicrobial:

[0039] Antibacterial rate against Staphylococcus aureus: 95%

[0040] Antibacterial rate against Escherichia coli: 90%

[0041] Air permeability:

[0042] Air permeability (the amount of gas that passes through a unit area per unit time): 509L / m 2 ·h

[0043] Softness:

[0044] Hand feel evaluation: soft and comfortable

[0045] Bending stiffness (the smaller the value, the better the softness): 1.42cN·cm

[0046] Tensile Strength:

[0047] Longitudinal tensile strength: 256N / 5cm

[0048] Transverse tensile strength: 202N / 5cm

[0049] Tear Strength:

[0050] Longitudinal tear strength: 50N

[0051] Transverse tear strength: 40N.

[0052] Embodiment 2:

[0053] This embodiment provides a specific method for preparing an antibacterial composite fabric, and the specific steps of the method are as follows:

[0054] (1) Preparation of blended fabrics:

[0055] The raw cotton yarn with a wax content of 0.4 wt% is selected and blended with the nylon yarn in a ratio of 25:75 to form a blended fabric.

[0056] (2) Impregnation treatment:

[0057] The mixed fabric was immersed in a tetra-n-butoxytitanium precursor solution with a concentration of 8 wt % for 8 minutes, and then dried.

[0058] (3) Hydrolysis treatment:

[0059] The impregnated and dried fabric was placed in a sodium hydroxide aqueous solution at a pH of 10 and a temperature of 90° C. for hydrolysis treatment, and the hydrolysis time was set to 2.5 hours.

[0060] (4) Cleaning and drying:

[0061] The hydrolyzed fabric was thoroughly washed and then dried at 70°C for 9 hours.

[0062] (5) Composite wear-resistant layer:

[0063] The wear-resistant layer made of polyester fiber material was selected, and its single yarn strength was 600cN. The wear-resistant layer was fixed on the outside of the treated mixed fabric by hot pressing, and the hot pressing temperature was set to 165℃ and the pressure was 3MPa, thereby forming an antibacterial composite fabric. According to the test, the amount of titanium dioxide attached to the cotton yarn in the antibacterial layer was 0.33w%, and the amount of titanium dioxide attached to the nylon yarn was 1.55w%.

[0064] Characterization:

[0065] Antimicrobial:

[0066] Antibacterial rate against Staphylococcus aureus: 97%

[0067] Antibacterial rate against Escherichia coli: 92%

[0068] Air permeability:

[0069] Air permeability: 520L / m 2 ·h

[0070] Softness:

[0071] Hand feel evaluation: soft and comfortable

[0072] Bending stiffness: 1.41 cN cm

[0073] Tensile Strength:

[0074] Longitudinal tensile strength: 261N / 5cm

[0075] Transverse tensile strength: 211N / 5cm

[0076] Tear Strength:

[0077] Longitudinal tear strength: 52N

[0078] Transverse tear strength: 43N

[0079] Comparative Example 1

[0080] This comparative example provides a specific method for preparing an antibacterial composite fabric, and the specific steps of the method are as follows:

[0081] (1) Preparation of blended fabrics:

[0082] Choose unwaxed cotton yarn and blend it with nylon yarn in a ratio of 25:75 to form a blended fabric.

[0083] (2) Impregnation treatment:

[0084] The mixed fabric was immersed in a tetraisopropoxy titanium precursor solution with a concentration of 8 wt % for 8 minutes, and then dried.

[0085] (3) Hydrolysis treatment:

[0086] The impregnated and dried fabric was placed in a sodium hydroxide aqueous solution at a pH of 10 and a temperature of 90° C. for hydrolysis treatment, and the hydrolysis time was set to 2.5 hours.

[0087] (4) Cleaning and drying:

[0088] The hydrolyzed fabric was thoroughly washed and then dried at 70°C for 9 hours.

[0089] (5) Composite wear-resistant layer:

[0090] The wear-resistant layer made of polyester fiber material was selected, and its single yarn strength was 600cN. The wear-resistant layer was fixed on the outside of the treated mixed fabric by hot pressing, and the hot pressing temperature was set to 165℃ and the pressure was 3MPa, thereby forming an antibacterial composite fabric. After testing, the attachment amount of titanium dioxide on the cotton yarn in the antibacterial layer was 1.21w%, and the attachment amount of titanium dioxide on the nylon yarn was 1.23w%.

[0091] Characterization:

[0092] Antimicrobial:

[0093] Antibacterial rate against Staphylococcus aureus: 98%

[0094] Antibacterial rate against Escherichia coli: 92%

[0095] Air permeability:

[0096] Air permeability: about 356L / m 2 ·h

[0097] Softness:

[0098] Hand feel evaluation: relatively soft

[0099] Bending stiffness: 2.1 cN cm

[0100] Tensile Strength:

[0101] Longitudinal tensile strength: about 220N / 5cm

[0102] Transverse tensile strength: about 197N / 5cm

[0103] Tear Strength:

[0104] Longitudinal tear strength: about 51N

[0105] Transverse tearing strength: about 42N.

[0106] Comparative Example 2

[0107] This comparative example provides a specific method for preparing an antibacterial composite fabric, and the specific steps of the method are as follows:

[0108] (1) Cotton yarn with a titanium dioxide attachment amount of 0.31w% and nylon yarn with a titanium dioxide attachment amount of 1.52w% are blended to form a blended fabric.

[0109] (2) Composite wear-resistant layer:

[0110] The wear-resistant layer made of polyester fiber material is selected, and its single yarn strength is 600cN. The wear-resistant layer is fixed on the outside of the treated mixed fabric by hot pressing, and the hot pressing temperature is set to 165°C and the pressure is 3MPa, thereby forming an antibacterial composite fabric.

[0111] Antimicrobial:

[0112] Antibacterial rate against Staphylococcus aureus: about 92%

[0113] Antibacterial rate against Escherichia coli: about 88%

[0114] Air permeability:

[0115] Air permeability: about 490L / m 2 ·h

[0116] Softness:

[0117] Hand feel evaluation: relatively soft, but slightly inferior to the example

[0118] Bending stiffness: 1.46cN·cm

[0119] Tensile Strength:

[0120] Longitudinal tensile strength: about 251N / 5cm

[0121] Transverse tensile strength: about 199N / 5cm

[0122] Tear Strength:

[0123] Longitudinal tear strength: about 44N

[0124] Transverse tear strength: about 41N

[0125] It should be particularly noted that although this specification is described in terms of implementation methods, not every implementation method contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation methods that can be understood by those skilled in the art.

Claims

1. A method for preparing an antibacterial composite fabric, Features The antibacterial composite fabric comprises an inner antibacterial layer and an outer wear-resistant layer, wherein the antibacterial layer is formed by mixing cotton yarn and nylon yarn, and the wear-resistant layer is arranged on the outer side of the inner antibacterial layer. The preparation method comprises the following steps: (1) Blending raw cotton yarn and nylon yarn in a ratio of 20:80 to 30:70 to form a blended fabric; (2) Immersing the blended fabric in a titanate precursor solution with a concentration of 5-10wt% for 5-10 minutes, and then drying it; (3) The impregnated and dried fabric is hydrolyzed in an alkaline solution with a pH of 9-12 and a temperature of 80-100°C for 1-4 hours; (4) Clean and dry the treated fabric; (5) A wear-resistant layer is compounded on the outer side of the treated fabric.

2. The preparation method according to claim 1, Features The wax content in raw cotton yarn is 0.3-0.5wt%.

3. The preparation method according to claim 1, Features The amount of titanium dioxide attached to the cotton yarn in the inner antibacterial layer is 0.1-0.5w%.

4. The preparation method according to claim 1, Features The attachment amount of titanium dioxide on the nylon yarn in the inner antibacterial layer is 1-2w%.

5. The preparation method according to claim 1, Features The outer wear-resistant layer is made of polyester fiber material with a single yarn strength of 500-700 cN.

6. The preparation method according to claim 1, Features The thickness of the antibacterial layer is 0.5-1.5 mm, and the thickness of the wear-resistant layer is 0.3-0.7 mm.

7. The method according to claim 1, Features The wear-resistant layer is fixed to the outer side of the fabric by hot pressing, the hot pressing temperature is 150-180 degrees Celsius, and the pressure is 2-4 MPa.

8. The method according to claim 1, Features The titanate is selected from one of tetraisopropoxytitanium, tetraethoxytitanium and tetra-n-butoxytitanium.

9. The method according to claim 1, Features The alkali solution is an aqueous solution of sodium hydroxide or potassium hydroxide.

10. The method according to claim 1, Features In step (4), the drying temperature is 60-80°C and the drying time is 6-12 hours.