Lightweight high-density leather for safety shoes as well as preparation method and application of lightweight high-density leather
By using a combined structure of polyurethane surface layer, adhesive layer, aluminum foil layer and broken adhesive layer in labor protection shoes, a high-density crosslinking network is formed, which solves the structural strength of ultra-light simulated leather in the prior art, and significantly improves the Service life and hydrolysis resistance.
Patent Information
- Application Number
- CN202411085716.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-08
AI Technical Summary
The structural strength of the existing ultra-light simulated leather microfiber synthetic leather is poor, resulting in weak hydrolysis resistance and cracking and powdering, which affects the service life.
The combined structure of polyurethane surface layer, adhesive layer, aluminum foil layer and crushed adhesive layer is adopted. The structural strength and service life of the material are improved through the cross-linking network structure of the through holes of the aluminum foil layer and the adhesive layer and crushed adhesive layer.
It significantly improves the service life of the labor protection upper, avoids cracking and powdering, and improves mechanical strength and hydrolysis resistance.
Smart Images

Figure BDA0004985126200000101 
Figure BDA0004985126200000111 
Figure HDA0004985126210000011
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of labor protection shoes, and in particular to a lightweight and high-density leather for labor protection shoes, and a preparation method and application thereof. Background Art
[0002] The best choice for shoe leather is genuine leather, which is a natural material formed by tightly woven collagen fibers, and has the advantages of good hand feel and good water vapor permeability. However, genuine leather is easily polluted during its own production process, resulting in excessive heavy metal content, and the yield rate during processing is low, which leads to high costs and difficulty for ordinary consumers to accept. Therefore, artificial leather came into being. Artificial leather not only solves the problems of material cleanliness and cost of genuine leather, but also can achieve the purpose of environmental protection, energy saving, sustainable development and green environmental protection, thereby avoiding harming animals and destroying the natural environment.
[0003] The Chinese patent application document with the publication number CN109972414A discloses a processing method of ultra-light simulated leather ultra-fine fiber synthetic leather, which includes the following steps: ① production of base fabric: PA slices and PE slices are mixed and nylon blended sea island fibers are obtained through spinning process; ② the prepared nylon blended sea island fibers are used to produce ultra-fine fiber non-woven fabrics through needle punching process; ③ the ultra-fine fiber non-woven fabrics are shaped to achieve thickness and gram weight to complete the production of base fabric; ④ the ultra-fine fiber non-woven fabrics are used to obtain unopened semi-finished products through wet impregnation process; ⑤ the semi-finished products are opened by benzene reduction method to obtain opened semi-finished products; ⑥ the opened semi-finished products are dried and oiled for setting, and kneaded; ⑦ the kneaded semi-finished products are kneaded by hot kneading machine. ⑧ the kneaded semi-finished products are veneered with resin to obtain ultra-light simulated leather ultra-fine fiber synthetic leather.
[0004] However, the ultra-light simulated leather microfiber synthetic leather obtained by this processing method has poor structural strength, resulting in weak hydrolysis resistance and short service life due to cracking and powdering, which needs to be improved. Summary of the invention
[0005] In view of this, the first purpose of this application is to provide a lightweight and high-density leather for labor protection shoes to achieve the purpose of improving structural strength and extending service life. The specific scheme is as follows:
[0006] A lightweight and high-density leather for labor protection shoes, comprising a polyurethane surface layer, an adhesive layer, an aluminum foil layer, a crushable adhesive layer and a bottom base; the aluminum foil layer is provided with a plurality of through holes distributed in an array, and the adhesive layer or a corresponding part of the crushable adhesive layer passes through the through holes; the adhesive layer comprises 60-100 parts by weight of polyester polyol, 30-50 parts of diphenylmethane diisocyanate, 17-30 parts of phthalic anhydride, 10-20 parts of ethylene glycol, 1-3 parts of epoxy resin, 0.1-1 parts of methanol, 0.1-3 parts of polycarbonate diol and 0.01-3 parts of zinc oxide; the crushable adhesive layer is composed of a crushable layer dispersed in a semi-cured adhesive layer.
[0007] Preferably, the polyurethane surface layer comprises, by weight, 50-80 parts of polyurethane resin, 0.1-3 parts of antioxidant, 0.1-5 parts of curing agent and 0-3 parts of color paste.
[0008] Preferably: the antioxidant is antioxidant V76-P, and the curing agent is polyisocyanate trimer HTBL-175S purchased from Wanhua.
[0009] Preferably, the crushing layer is formed by mixing and curing a glue solution comprising 16-24 parts by weight of vinyl acetate, 22-28 parts of butyl rubber, 7-12 parts of polyethylene, 0.01-2 parts of graphene, 0.01-1 parts of antioxidant, 0.5-1 parts of epoxy resin and 0.5-1 parts of calcium carbonate.
[0010] Preferably: the polyethylene is a linear low-density polyethylene, and the antioxidant is a phenol-free phosphite antioxidant 3010.
[0011] Preferably, the semi-cured adhesive layer is formed by curing a light / heat curing adhesive.
[0012] Preferably: the light / heat curing adhesive comprises a binary or multi-polymer of ethylene and propylene, butene, pentene, hexene, octene, butadiene, 1,4-pentadiene, isoprene, ethylidene norbornene, dicyclopentadiene, 1,4-hexadiene containing active groups as a base resin, ethylene glycol, a silane coupling agent, tert-butyl peroxyisopropyl carbonate and N,N-dimethylcyclohexylamine, and the weight ratio is 70-98:0.05-10:0.01-2:0.01-2:0.01-2.
[0013] The second object of the present application is to provide a method for preparing a lightweight and high-density leather for labor protection shoes as described above, comprising the following steps:
[0014] Step 1, coating the polyurethane surface layer slurry on the release paper, controlling the coating thickness to be 0.05-0.2 mm, and obtaining the polyurethane surface layer after drying;
[0015] Step 2, evenly coating the viscose on the polyurethane surface layer, controlling the coating thickness to be 0.1-0.2 mm, and obtaining the viscose surface layer after drying by 20-80%;
[0016] Step 3: attach the laminated substrate to the adhesive surface layer, peel off the release paper after drying, and obtain a lightweight and high-density leather for labor protection shoes.
[0017] Preferably: in step 3, the laminating substrate is composed of an aluminum foil layer, a crushing layer, a semi-cured adhesive layer and a bottom base fabric; the bottom base fabric is a fiber woven fabric or a non-woven fabric; the thickness of the aluminum foil layer is 0.05-0.1 mm and is laser-perforated; the crushing layer is formed by mixing and curing a glue solution including 16-24 parts by weight of vinyl acetate, 22-28 parts of butyl rubber, 7-12 parts of polyethylene, 0.01-2 parts of graphene, 0.01-1 parts of antioxidants, 0.5-1 parts of epoxy resins and 0.5-1 parts of calcium carbonate; the semi-cured adhesive layer is formed by curing a light / heat curing adhesive.
[0018] The third object of the present application is to provide the application of the lightweight and high-density leather for labor protection shoes as described above in labor protection shoe uppers.
[0019] It can be known from the above scheme that the present application provides a lightweight and high-density leather for labor protection shoes and its preparation method and application. The lightweight and high-density leather for labor protection shoes realizes the connection and support of the polyurethane surface layer and the bottom base through aluminum foil, an adhesive layer and a broken adhesive layer. The adhesive layer and the broken adhesive layer intersecting through the through holes form a high-density polymer cross-linked network structure, achieving the purpose of improving structural strength and extending service life. The preparation method of the lightweight and high-density leather for labor protection shoes has the function of effectively obtaining a broken adhesive layer composed of a broken layer dispersed in a semi-cured adhesive layer, and cross-linking and curing the broken adhesive layer with the adhesive layer to achieve the purpose of effectively improving structural strength. The application of the lightweight and high-density leather for labor protection shoes in the upper of labor protection shoes plays a role in significantly improving the service life of the upper of labor protection shoes and effectively avoiding cracking and powdering. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying any creative work.
[0021] Figure 1 This is a schematic diagram of the structure of the lightweight and high-density leather for labor protection shoes disclosed in this application.
[0022] Explanation of the reference numerals: 1. polyurethane surface layer; 2. adhesive layer; 3. aluminum foil layer; 31. through hole; 4. crushing adhesive layer; 5. bottom layer base. DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0024] It is worth mentioning that there is no phenol phosphite antioxidant 3010 was purchased from Guangzhou Zhiyi Chemical Co., Ltd. Polyisocyanate trimer HTBL-175S was purchased from Wanhua Chemical.
[0025] The lightweight and high-density leather for labor protection shoes of the present application and its preparation method and application are described in detail below.
[0026] like Figure 1 As shown, a lightweight and high-density leather for labor protection shoes includes a polyurethane surface layer 1, an adhesive layer 2, an aluminum foil layer 3, a crushable adhesive layer 4 and a bottom base 5. The crushable adhesive layer 4 is composed of a crushable layer dispersed in a semi-cured adhesive layer. The crushable layer has adhesive force and has the effect of connecting the aluminum foil layer 3 and the semi-cured adhesive layer when it is not crushed, and forms a combined structure combined with the semi-cured adhesive layer during the processing of the aluminum foil layer 3, and is used to form the crushable adhesive layer 4 after being fully cured.
[0027] It should be mentioned that a plurality of through holes 31 distributed in an array are provided on the aluminum foil layer 3. The corresponding parts of the adhesive layer 2 and the broken adhesive layer 4 pass through the through holes 31 and are crosslinked and cured with the corresponding broken adhesive layer 4 and the adhesive layer 2. In the embodiment of the present application, the polyurethane surface layer 1 includes 50-80 parts by weight of polyurethane resin, 0.1-3 parts of antioxidant, 0.1-5 parts of curing agent and 0-3 parts of color paste. The adhesive layer 2 includes 60-100 parts by weight of polyester polyol, 30-50 parts of diphenylmethane diisocyanate, 17-30 parts of phthalic anhydride, 10-20 parts of ethylene glycol, 1-3 parts of epoxy resin, 0.1-1 parts of methanol, 0.1-3 parts of polycarbonate diol and 0.01-3 parts of zinc oxide. The crushing layer is formed by mixing and curing a glue solution which comprises 16-24 parts by weight of vinyl acetate, 22-28 parts by weight of butyl rubber, 7-12 parts by weight of polyethylene, 0.01-2 parts by weight of graphene, 0.01-1 parts by weight of antioxidant, 0.5-1 parts by weight of epoxy resin and 0.5-1 parts by weight of calcium carbonate.
[0028] The antioxidant used in the embodiment of the present application is antioxidant V76-P, the curing agent is polyisocyanate trimer HTBL-175S purchased from Wanhua, the polyethylene is linear low-density polyethylene, and the antioxidant is phenol-free phosphite antioxidant 3010. The semi-cured adhesive layer is formed by curing the light / heat curing adhesive.
[0029] It should be noted that the light / heat curing adhesive includes a binary or multi-polymer of ethylene and propylene, butene, pentene, hexene, octene, butadiene, 1,4-pentadiene, isoprene, ethylidene norbornene, dicyclopentadiene, 1,4-hexadiene containing an active group as a base resin, ethylene glycol, a silane coupling agent, tert-butyl peroxyisopropyl carbonate and N,N-dimethylcyclohexylamine, and the weight ratio is 70-98:0.05-10:0.01-2:0.01-2:0.01-2. The active group is an isocyanate group or an acyl chloride group.
[0030] A method for preparing lightweight and high-density leather for labor protection shoes comprises the following steps:
[0031] Step 1, coating the polyurethane surface layer 1 slurry on the release paper, controlling the coating thickness to be 0.05-0.2 mm, and obtaining the polyurethane surface layer 1 after drying;
[0032] Step 2, evenly coating the adhesive on the polyurethane surface layer 1, controlling the coating thickness to be 0.1-0.2 mm, and obtaining the adhesive surface layer after drying by 20-80%;
[0033] Step 3: attach the laminated substrate to the adhesive surface layer, perform infrared or high temperature treatment, and peel off the release paper after drying to obtain a lightweight and high-density leather for labor protection shoes.
[0034] With respect to the laminating substrate in step 3, the laminating substrate in the embodiment of the present application is composed of an aluminum foil layer 3, a crushing layer, a semi-cured adhesive layer and a bottom base fabric. The bottom base fabric used is a fiber woven cloth or a non-woven fabric. The thickness of the aluminum foil layer 3 is 0.05-0.1 mm, and it is laser-perforated to achieve the effect of crushing the crushing layer and impacting into the semi-cured adhesive layer. The crushing layer is formed by mixing and curing a glue solution including 16-24 parts of vinyl acetate, 22-28 parts of butyl rubber, 7-12 parts of polyethylene, 0.01-2 parts of graphene, 0.01-1 parts of antioxidants, 0.5-1 parts of epoxy resins and 0.5-1 parts of calcium carbonate by weight.
[0035] The application of a lightweight and high-density leather for labor protection shoes in the labor protection shoe upper plays a role in significantly improving the service life of the labor protection shoe upper and effectively avoiding cracking and powdering.
[0036] Embodiment 1
[0037] like Figure 1As shown, a lightweight and high-density leather for labor protection shoes includes a polyurethane surface layer 1, an adhesive layer 2, an aluminum foil layer 3, a crushable adhesive layer 4 and a bottom base 5. The crushable adhesive layer 4 is composed of a crushable layer dispersed in a semi-cured adhesive layer. The crushable layer has adhesive force and has the effect of connecting the aluminum foil layer 3 and the semi-cured adhesive layer when it is not crushed, and forms a combined structure combined with the semi-cured adhesive layer during the processing of the aluminum foil layer 3, and is used to form the crushable adhesive layer 4 after being fully cured.
[0038] It should be mentioned that a plurality of through holes 31 distributed in an array are provided on the aluminum foil layer 3. The corresponding parts of the adhesive layer 2 and the broken adhesive layer 4 pass through the through holes 31 and are cross-linked and cured with the corresponding broken adhesive layer 4 and the adhesive layer 2. In the embodiment of the present application, the polyurethane surface layer 1 includes 50 parts by weight of polyurethane resin, 0.1 parts of antioxidant and 0.1 parts of curing agent. The adhesive layer 2 includes 60 parts by weight of polyester polyol, 30 parts of diphenylmethane diisocyanate, 17 parts of phthalic anhydride, 10 parts of ethylene glycol, 1 part of epoxy resin, 0.1 parts of methanol, 0.1 parts of polycarbonate diol and 0.01 parts of zinc oxide. The crushing layer is formed by mixing and curing a glue solution including 16 parts by weight of vinyl acetate, 22 parts of butyl rubber, 7 parts of polyethylene, 0.01 parts of graphene, 0.01 parts of antioxidant, 0.5 parts of epoxy resin and 0.5 parts of calcium carbonate.
[0039] The antioxidant used in the embodiment of the present application is antioxidant V76-P, the curing agent is polyisocyanate trimer HTBL-175S purchased from Wanhua, the polyethylene is linear low-density polyethylene, and the antioxidant is phenol-free phosphite antioxidant 3010. The semi-cured adhesive layer is formed by curing the light / heat curing adhesive.
[0040] It should be noted that the light / heat curing adhesive comprises a multi-polymer of ethylene, propylene and butylene containing active groups as a base resin, ethylene glycol, a silane coupling agent, tert-butyl peroxyisopropyl carbonate and N,N-dimethylcyclohexylamine, and the weight ratio is 70:0.05:0.01:0.01:0.01. The active group is an isocyanate group.
[0041] A method for preparing lightweight and high-density leather for labor protection shoes comprises the following steps:
[0042] Step 1, coating the polyurethane surface layer 1 slurry on the release paper, controlling the coating thickness to be 0.05 mm, and obtaining the polyurethane surface layer 1 after drying;
[0043] Step 2, evenly coating the adhesive on the polyurethane surface layer 1, controlling the coating thickness to be 0.1 mm, and obtaining an adhesive surface layer after preliminary drying;
[0044] Step 3: attach the laminated substrate to the adhesive surface layer, perform infrared or high temperature treatment, and peel off the release paper after drying to obtain a lightweight and high-density leather for labor protection shoes.
[0045] Regarding the bonding substrate in step 3, the bonding substrate in the embodiment of the present application is composed of an aluminum foil layer 3, a crushing layer, a semi-cured adhesive layer and a bottom base fabric. The bottom base fabric used is a fiber woven cloth. The thickness of the aluminum foil layer 3 is 0.05mm, and it is laser-perforated to achieve the effect of crushing the crushing layer and impacting into the semi-cured adhesive layer. The laser opening spacing can be 0.05mm-0.2mm, and the speed, Q frequency and other parameters are set according to demand, which will not be repeated here. And in Example 1 of the present application, 0.05mm spacing, 600mm / s marking speed, 20KHzQ frequency and 40% power are mainly used.
[0046] At the same time, the present application also discloses the application of a lightweight and high-density leather for labor protection shoes in the labor protection shoe upper, which plays a role in significantly improving the service life of the labor protection shoe upper and effectively avoiding cracking and powdering.
[0047] Embodiment 2
[0048] like Figure 1 As shown, a lightweight and high-density leather for labor protection shoes includes a polyurethane surface layer 1, an adhesive layer 2, an aluminum foil layer 3, a crushable adhesive layer 4 and a bottom base 5. The crushable adhesive layer 4 is composed of a crushable layer dispersed in a semi-cured adhesive layer. The crushable layer has adhesive force and has the effect of connecting the aluminum foil layer 3 and the semi-cured adhesive layer when it is not crushed, and forms a combined structure combined with the semi-cured adhesive layer during the processing of the aluminum foil layer 3, and is used to form the crushable adhesive layer 4 after being fully cured.
[0049] It should be mentioned that a plurality of through holes 31 distributed in an array are provided on the aluminum foil layer 3. The corresponding parts of the adhesive layer 2 and the broken adhesive layer 4 pass through the through holes 31 and are crosslinked and cured with the corresponding broken adhesive layer 4 and the adhesive layer 2. In the embodiment of the present application, the polyurethane surface layer 1 includes 70 parts by weight of polyurethane resin, 1 part of antioxidant, 2 parts of curing agent and 1 part of color paste. The adhesive layer 2 includes 80 parts by weight of polyester polyol, 40 parts of diphenylmethane diisocyanate, 20 parts of phthalic anhydride, 15 parts of ethylene glycol, 2 parts of epoxy resin, 0.4 parts of methanol, 0.8 parts of polycarbonate diol and 1 part of zinc oxide. The crushing layer is formed by mixing and curing a glue solution including 22 parts by weight of vinyl acetate, 25 parts of butyl rubber, 10 parts of polyethylene, 1 part of graphene, 0.3 parts of antioxidant, 0.7 parts of epoxy resin and 0.6 parts of calcium carbonate.
[0050] The antioxidant used in the embodiment of the present application is antioxidant V76-P, the curing agent is polyisocyanate trimer HTBL-175S purchased from Wanhua, the polyethylene is linear low-density polyethylene, and the antioxidant is phenol-free phosphite antioxidant 3010. The semi-cured adhesive layer is formed by curing the light / heat curing adhesive.
[0051] It should be noted that the light / heat curing adhesive comprises a binary copolymer of ethylene and octene, butadiene, and isoprene containing an active group as a base resin, ethylene glycol, a silane coupling agent, tert-butyl peroxyisopropyl carbonate, and N,N-dimethylcyclohexylamine, and the weight ratio is 78:3:1:0.8:1.4. The active group is an acyl chloride group.
[0052] A method for preparing lightweight and high-density leather for labor protection shoes comprises the following steps:
[0053] Step 1, coating the polyurethane surface layer 1 slurry on the release paper, controlling the coating thickness to be 0.1 mm, and obtaining the polyurethane surface layer 1 after drying;
[0054] Step 2, evenly coating the adhesive on the polyurethane surface layer 1, controlling the coating thickness to be 0.15 mm, and obtaining an adhesive surface layer after preliminary drying;
[0055] Step 3: attach the laminated substrate to the adhesive surface layer, perform infrared or high temperature treatment, and peel off the release paper after drying to obtain a lightweight and high-density leather for labor protection shoes.
[0056] Regarding the bonding substrate in step 3, the bonding substrate in the embodiment of the present application is composed of an aluminum foil layer 3, a crushing layer, a semi-cured adhesive layer and a bottom base fabric. The bottom base fabric used is a non-woven fabric. The thickness of the aluminum foil layer 3 is 0.08mm, and it is laser-perforated to achieve the effect of crushing the crushing layer and impacting into the semi-cured adhesive layer. The laser opening spacing can be 0.05mm-0.2mm, and the speed, Q frequency and other parameters are set according to demand, which will not be repeated here. And in Example 2 of the present application, 0.1mm spacing, 600mm / s marking speed, 20KHzQ frequency and 37% power are mainly used.
[0057] At the same time, the present application also discloses the application of a lightweight and high-density leather for labor protection shoes in the labor protection shoe upper, which plays a role in significantly improving the service life of the labor protection shoe upper and effectively avoiding cracking and powdering.
[0058] Embodiment 3
[0059] like Figure 1As shown, a lightweight and high-density leather for labor protection shoes includes a polyurethane surface layer 1, an adhesive layer 2, an aluminum foil layer 3, a crushable adhesive layer 4 and a bottom base 5. The crushable adhesive layer 4 is composed of a crushable layer dispersed in a semi-cured adhesive layer. The crushable layer has adhesive force and has the effect of connecting the aluminum foil layer 3 and the semi-cured adhesive layer when it is not crushed, and forms a combined structure combined with the semi-cured adhesive layer during the processing of the aluminum foil layer 3, and is used to form the crushable adhesive layer 4 after being fully cured.
[0060] It should be mentioned that a plurality of through holes 31 distributed in an array are provided on the aluminum foil layer 3. Among them, the corresponding parts of the adhesive layer 2 and the broken adhesive layer 4 pass through the through hole 31 and are cross-linked and cured with the corresponding broken adhesive layer 4 and the adhesive layer 2. In the embodiment of the present application, the polyurethane surface layer 1 includes 80 parts of polyurethane resin, 3 parts of antioxidant, 5 parts of curing agent and 3 parts of color paste by weight. The adhesive layer 2 includes 100 parts of polyester polyol, 50 parts of diphenylmethane diisocyanate, 30 parts of phthalic anhydride, 20 parts of ethylene glycol, 3 parts of epoxy resin, 1 part of methanol, 3 parts of polycarbonate diol and 3 parts of zinc oxide by weight. The broken layer is formed by mixing and curing a glue solution including 24 parts of vinyl acetate, 28 parts of butyl rubber, 12 parts of polyethylene, 2 parts of graphene, 1 part of antioxidant, 1 part of epoxy resin and 1 part of calcium carbonate by weight.
[0061] The antioxidant used in the embodiment of the present application is antioxidant V76-P, the curing agent is polyisocyanate trimer HTBL-175S purchased from Wanhua, the polyethylene is linear low-density polyethylene, and the antioxidant is phenol-free phosphite antioxidant 3010. The semi-cured adhesive layer is formed by curing the light / heat curing adhesive.
[0062] It should be noted that the light / heat curing adhesive comprises a multi-polymer of ethylene and 1,4-hexadiene containing an active group as a base resin, ethylene glycol, a silane coupling agent, tert-butyl peroxyisopropyl carbonate and N,N-dimethylcyclohexylamine, and the weight ratio is 98:10:2:2:2. The active group is an isocyanate group.
[0063] A method for preparing lightweight and high-density leather for labor protection shoes comprises the following steps:
[0064] Step 1, coating the polyurethane surface layer 1 slurry on the release paper, controlling the coating thickness to be 0.2 mm, and obtaining the polyurethane surface layer 1 after drying;
[0065] Step 2, evenly coating the adhesive on the polyurethane surface layer 1, controlling the coating thickness to be 0.2 mm, and obtaining an adhesive surface layer after preliminary drying;
[0066] Step 3: attach the laminated substrate to the adhesive surface layer, perform infrared or high temperature treatment, and peel off the release paper after drying to obtain a lightweight and high-density leather for labor protection shoes.
[0067] Regarding the bonding substrate in step 3, the bonding substrate in the embodiment of the present application is composed of an aluminum foil layer 3, a crushing layer, a semi-cured adhesive layer and a bottom base fabric. The bottom base fabric used is a fiber woven cloth or a non-woven fabric. The thickness of the aluminum foil layer 3 is 0.1 mm, and it is laser-perforated to achieve the effect of crushing the crushing layer and impacting into the semi-cured adhesive layer. The laser opening spacing can be 0.05 mm-0.2 mm, and the speed, Q frequency and other parameters are set according to demand, which will not be repeated here. And in Example 3 of the present application, 0.2 mm spacing, 800 mm / s marking speed, 20 KHz Q frequency and 38% power are mainly used.
[0068] At the same time, the present application also discloses the application of a lightweight and high-density leather for labor protection shoes in the labor protection shoe upper, which plays a role in significantly improving the service life of the labor protection shoe upper and effectively avoiding cracking and powdering.
[0069] Embodiment 4
[0070] The difference between Example 4 and Example 2 is that the graphene used in the crushing layer in Example 4 is activated graphene treated with sodium hydroxide solution with a pH of 2-3.
[0071] Comparative Example 1
[0072] The difference between the comparative example 1 and the embodiment 2 is that the lightweight high-density leather for labor protection shoes in the comparative example 1 comprises a polyurethane surface layer 1, an adhesive layer 2, a crushable adhesive layer 4 and a bottom base 5.
[0073] Comparative Example 2
[0074] The difference between Comparative Example 2 and Example 2 is that the aluminum foil layer 3 in Comparative Example 2 does not have a through hole 31 .
[0075] Comparative Example 3
[0076] The difference between the comparative example 3 and the embodiment 2 is that the broken adhesive layer 4 in the comparative example 3 is formed by directly curing the semi-cured adhesive layer.
[0077] Comparative Example 4
[0078] The difference between Comparative Example 4 and Example 2 is that the semi-cured adhesive layer in Comparative Example 4 is a double-sided adhesive without a substrate.
[0079] Comparative Example 5
[0080] The difference between Comparative Example 5 and Example 2 is that the crushing layer in Comparative Example 5 does not have graphene.
[0081] Performance Test:
[0082] 1. Mechanical strength: breaking strength, peel strength and warp tear strength
[0083] 2. Hydrolysis resistance: Tested at 70°C and 95%RH for 5 weeks.
[0084] The performance test results are shown in Table 1 below:
[0085] Table 1 Performance test results of Examples 1 to 4 and Comparative Examples 1 to 5
[0086]
[0087]
[0088] It can be seen from Table 1 above that the lightweight high-density leather for labor protection shoes of the present application is resistant to alcohol and hydrolysis, with a peel strength greater than 45N / 3cm, a breaking strength greater than 600N / cm, and a warp tear strength greater than 100N. Compared with existing materials, the mechanical properties are significantly improved and the requirements for hydrolysis resistance are met.
[0089] In addition, compared with Comparative Examples 1 to 5, the lightweight and high-density leather for labor protection shoes in the embodiment of the present application has a five-layer structure consisting of a polyurethane surface layer, an adhesive layer, an aluminum foil layer, a crushable adhesive layer and a bottom base. While the aluminum foil layer plays an effective supporting role, the crushable layer is crushed and combined with the semi-cured adhesive layer when a through hole is opened on the aluminum foil layer, so as to form a crushed adhesive layer with significantly improved structural strength after complete curing, thereby achieving the purpose of improving peel strength and mechanical strength.
[0090] In summary, the present application provides a lightweight, high-density leather for labor protection shoes, and a preparation method and application thereof. The lightweight, high-density leather for labor protection shoes realizes the connection and support of the polyurethane surface layer and the bottom base through aluminum foil, an adhesive layer and a broken adhesive layer. The adhesive layer and the broken adhesive layer intersecting through the through holes form a high-density polymer cross-linked network structure, so that the wear resistance and hydrolysis resistance are significantly improved through the improvement of composite performance, thereby achieving the purpose of improving structural strength and extending service life. The preparation method of the lightweight, high-density leather for labor protection shoes has the function of effectively obtaining a broken adhesive layer composed of a broken layer dispersed in a semi-cured adhesive layer, and cross-linking and curing the broken adhesive layer with the adhesive layer to achieve the purpose of effectively improving structural strength.
[0091] The "first", "second", "third", "fourth", etc. (if any) referred to in this application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments described herein can be implemented in an order other than that illustrated or described herein. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods or devices.
[0092] It should be noted that the descriptions involving "first", "second", etc. in this application are only for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in this field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by this application.
[0093] Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for those skilled in the art, according to the idea of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A lightweight and high-density leather for labor protection shoes. Features: The invention comprises a polyurethane surface layer, an adhesive layer, an aluminum foil layer, a crushable adhesive layer and a bottom base; the aluminum foil layer is provided with a plurality of through holes distributed in an array, and the adhesive layer or a corresponding part of the crushable adhesive layer passes through the through holes; the adhesive layer comprises 60-100 parts by weight of polyester polyol, 30-50 parts by weight of diphenylmethane diisocyanate, 17-30 parts by weight of phthalic anhydride, 10-20 parts by weight of ethylene glycol, 1-3 parts by weight of epoxy resin, 0.1-1 parts by weight of methanol, 0.1-3 parts by weight of polycarbonate diol and 0.01-3 parts by weight of zinc oxide; the crushable adhesive layer is composed of a crushable layer dispersed in a semi-cured adhesive layer.
2. A lightweight and high-density leather for labor protection shoes according to claim 1, Features: The polyurethane surface layer comprises 50-80 parts of polyurethane resin, 0.1-3 parts of antioxidant, 0.1-5 parts of curing agent and 0-3 parts of color paste by weight.
3. A lightweight and high-density leather for labor protection shoes according to claim 2, Features: The antioxidant is antioxidant V76-P, and the curing agent is polyisocyanate trimer HTBL-175S purchased from Wanhua.
4. The lightweight and high-density leather for labor protection shoes according to claim 1, Features: The crushing layer is formed by mixing and curing a glue solution comprising 16-24 parts by weight of vinyl acetate, 22-28 parts by weight of butyl rubber, 7-12 parts by weight of polyethylene, 0.01-2 parts by weight of graphene, 0.01-1 parts by weight of antioxidant, 0.5-1 parts by weight of epoxy resin and 0.5-1 parts by weight of calcium carbonate.
5. A lightweight and high-density leather for labor protection shoes according to claim 4, Features: The polyethylene is a linear low-density polyethylene, and the antioxidant is a phenol-free phosphite antioxidant YIPHOS® 3010.
6. The lightweight and high-density leather for labor protection shoes according to claim 1, Features: The semi-cured adhesive layer is formed by curing a light / heat curing adhesive.
7. The lightweight and high-density leather for labor protection shoes according to claim 6, Features: The light / heat curing adhesive comprises a binary or multi-component copolymer of ethylene and propylene, butene, pentene, hexene, octene, butadiene, 1,4-pentadiene, isoprene, ethylidene norbornene, dicyclopentadiene, and 1,4-hexadiene containing active groups as a base resin, ethylene glycol, a silane coupling agent, tert-butyl peroxyisopropyl carbonate, and N,N-dimethylcyclohexylamine, and the weight ratio is 70-98:0.05-10:0.01-2:0.01-2:0.01-2.
8. A method for preparing a lightweight and high-density leather for labor protection shoes according to any one of claims 1 to 7, It is characterized in that The steps include: Step 1, coating the polyurethane surface layer slurry on the release paper, controlling the coating thickness to be 0.05-0.2 mm, and obtaining the polyurethane surface layer after drying; Step 2, evenly coating the adhesive on the polyurethane surface layer, controlling the coating thickness to be 0.1-0.2 mm, and obtaining the adhesive surface layer after drying by 20-80%; Step 3: attach the laminated substrate to the adhesive surface layer, peel off the release paper after drying, and obtain a lightweight and high-density leather for labor protection shoes.
9. The lightweight and high-density leather for labor protection shoes according to claim 8, Features: In step 3, the laminating substrate is composed of an aluminum foil layer, a crushing layer, a semi-cured adhesive layer and a bottom base fabric; the bottom base fabric is a fiber woven fabric or a non-woven fabric; the thickness of the aluminum foil layer is 0.05-0.1 mm and is laser-perforated; the crushing layer is formed by mixing and curing a glue solution including 16-24 parts by weight of vinyl acetate, 22-28 parts of butyl rubber, 7-12 parts of polyethylene, 0.01-2 parts of graphene, 0.01-1 parts of antioxidants, 0.5-1 parts of epoxy resins and 0.5-1 parts of calcium carbonate; the semi-cured adhesive layer is formed by curing a light / heat curing adhesive.
10. Use of the lightweight and high-density leather for labor protection shoes according to any one of claims 1 to 7 in labor protection shoe uppers.
Citation Information
Patent Citations
Multi-layer composite materials comprising a plastic or metal foil, corresponding method of production and use thereof
CN101959681A
High-heat-conduction graphene modified EVA foaming material and preparation method thereof
CN109438821A
Packaging material, related coating and preparation method thereof, and photovoltaic module
CN111675971A
Material for environment-friendly regenerated leather sports shoes and preparation process of material
CN117087256A
Low-VOC (volatile organic compound) polyurethane interior material for automobile seat and preparation method of low-VOC polyurethane interior material
CN118048791A