Metal composite film and electrochemical device
By using an anti-corrosion layer containing nitrogen-containing polymers and acid-modified groups in the metal composite film of lithium-ion batteries, the problem of unsatisfactory anti-corrosion treatment effect is solved, the connection strength and corrosion resistance of the metal composite film are improved, and the production cost is reduced.
Patent Information
- Application Number
- CN202411054915.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
The corrosion protection effect of existing lithium-ion battery metal composite films is not ideal, which increases the risk of electrolyte leakage. Furthermore, the combination of different adhesive layers has a large difference in effect, affecting production efficiency and cost.
A nitrogen-containing polymer is used as the first anti-corrosion layer, combined with an adhesive layer containing acid-modified groups and isocyanate groups. The nitrogen atom content is controlled within the range of 0-20 At%. Covalent bonds are used to improve the connection strength and corrosion resistance between the intermediate metal layer and the hot-melt resin layer.
It improves the initial peel strength and corrosion resistance of the intermediate metal layer and the hot-melt resin layer of the metal composite film, reduces production costs, and enhances long-term stability and adaptability.
Smart Images

Figure CN118977480A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of metal-plastic films, and in particular to a metal composite film and an electrochemical device. Background Art
[0002] Currently, lithium-ion batteries are mainly divided into three categories: square, cylindrical, and soft-pack. The outer shells of square and cylindrical batteries are mainly made of hard shells such as aluminum alloy and stainless steel. The aluminum alloy outer shell can be made of aluminum, while the soft-pack outer shell made of metal and resin laminated uses a metal composite film, which greatly improves the problem of inflexible appearance design of hard-mounted batteries.
[0003] The metal composite film consists of an outer base resin layer, an intermediate metal layer, a first adhesive layer, and a heat-welding resin layer. As a battery packaging material, the metal composite film is required to be resistant to electrolyte corrosion, thereby preventing leakage of the battery shell and ensuring the battery life.
[0004] Generally, the metal in the metal composite film for lithium-ion battery outer packaging needs to be treated with corrosion protection. If the corrosion protection effect is not ideal, if water is mixed in the battery manufacturing process, it will react with the lithium salt in the electrolyte to generate corrosive hydrogen fluoride (HF). Hydrogen fluoride will pass through the heat-welding resin layer and the first adhesive layer to reach the surface of the intermediate metal layer, thereby corroding the metal and causing the intermediate metal layer to separate from the heat-welding resin layer. This increases the possibility of electrolyte leakage from the battery. Therefore, the corrosion protection treatment of the intermediate metal layer has a great influence on the metal composite film.
[0005] At present, the main components of the anti-corrosion treatment liquid of the metal composite film are trivalent chromium compounds, fluorides, aminophenol resins and phosphoric acid. After the intermediate metal layer is treated with this anti-corrosion liquid, the corrosion resistance of the metal composite film can be improved in some common electrolyte environments. However, the current common practice is to select different types of anti-corrosion treatment agents according to the type of the first adhesive layer. When the same anti-corrosion treatment agent is used with different types of first adhesive layers, the treatment effect varies greatly. When the treatment effect is poor, moisture may penetrate the outer packaging of the battery, causing the electrolyte to produce hydrogen fluoride (HF). The anti-corrosion treatment effect of this anti-corrosion liquid will be unsatisfactory, which can easily cause interlayer separation of the metal composite film for lithium-ion batteries, affecting the promotion and use of metal composite films in the field of lithium-ion batteries.
[0006] And assuming that, as shown in the present application, the anti-corrosion layer includes a nitrogen-containing polymer and the adhesive layer includes an acid-modified group and / or an isocyanate group, cracks are likely to form between the anti-corrosion layer and the inner adhesive layer after the reaction due to external forces. When the soft-packaged lithium battery is used for a long time, the intruding moisture will react with the electrolyte to generate hydrogen fluoride. Hydrogen fluoride is easy to invade from the cracks, resulting in a decrease in the peel strength between the anti-corrosion layer and the inner adhesive layer, and eventually delamination. Summary of the invention
[0007] The purpose of the present application is to overcome the deficiencies of the prior art and to provide a metal composite membrane and an electrochemical device.
[0008] The embodiment of the present application is implemented as follows:
[0009] In a first aspect, the present application provides a metal composite film, which includes a heat-melting resin layer, a first adhesive layer, a first anti-corrosion layer, an intermediate metal layer, and an outer substrate resin layer stacked in sequence;
[0010] Among them, the first adhesive layer includes acid-modified groups and / or isocyanate groups, the first anti-corrosion layer includes a nitrogen-containing polymer, the nitrogen-containing polymer has an amino group that reacts with the acid-modified groups and / or isocyanate groups, and the content of nitrogen atoms in the first anti-corrosion layer is greater than 0 and less than or equal to 20At%.
[0011] The metal composite film provided by the present application, by adding a nitrogen-containing polymer with a certain nitrogen atom content in the first anti-corrosion layer, can not only be compatible with different types of first adhesive layers, thereby reducing the preparation cost of the metal composite film and improving the preparation efficiency, but also the hardness between the intermediate metal layer and the hot-melt resin layer of the obtained metal composite film is reasonable, and it is not easily affected by external forces to generate cracks, and the initial peel strength between the intermediate metal layer and the hot-melt resin layer is good, and it has better long-term effectiveness, which is conducive to promoting the promotion and use of metal composite films in the field of lithium-ion batteries.
[0012] In a second aspect, the present application provides an electrochemical device using the metal composite membrane provided in the first aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0014] Figure 1 A schematic diagram of the structure of a metal composite film provided in some embodiments of the present application;
[0015] Figure 2 A schematic diagram of the structure of a metal composite film provided in some embodiments of the present application;
[0016] Figure 3 A schematic diagram of the structure of a metal composite film provided in some embodiments of the present application;
[0017] Figure 4 A schematic diagram of the structure of a metal composite film provided in some embodiments of the present application;
[0018] Figure 5 A schematic diagram of the structure of a metal composite film provided in some embodiments of the present application.
[0019] Icon: 1000 - metal composite film; 10 - hot-melt resin layer; 11 - first adhesive layer; 12 - first anti-corrosion layer; 13 - intermediate metal layer; 14 - second anti-corrosion layer; 15 - second adhesive layer; 16 - outer base material resin layer; 17 - coloring layer. DETAILED DESCRIPTION
[0020] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0021] The following is a detailed description of the metal composite film and electrochemical device according to the embodiment of the present application:
[0022] See also Figures 1 to 5 The present application provides a metal composite film 1000, which includes a heat-melting resin layer 10, a first adhesive layer 11, a first anti-corrosion layer 12, an intermediate metal layer 13 and an outer base resin layer 16 which are stacked in sequence.
[0023] Among them, the first adhesive layer 11 includes acid-modified groups and / or isocyanate groups, the first anti-corrosion layer 12 includes a nitrogen-containing polymer, the nitrogen-containing polymer has an amino group that reacts with the acid-modified groups and / or isocyanate groups, and the content of nitrogen atoms in the first anti-corrosion layer 12 is greater than 0 and less than or equal to 20At%.
[0024] The present application provides a first anti-corrosion layer 12 between the intermediate metal layer 13 and the first adhesive layer 11, which is beneficial for preventing corrosive hydrogen fluoride (HF) from reaching the surface of the intermediate metal layer 13 when it is generated in the battery, thereby inhibiting the detachment between the intermediate metal layer 13 and the heat-sealed resin layer 10.
[0025] The acid-modified groups that react with the amino groups include but are not limited to at least one of carboxyl, sulfonic acid, maleic acid, sulfinic acid, sulfenic acid, phosphoric acid, phosphonic acid, and the like.
[0026] The content of nitrogen atoms in the first anti-corrosion layer 12 refers to the element content deep in the first anti-corrosion layer 12 detected by the method described later (XPS-ESCA method), and the elements added to the first anti-corrosion layer 12 are uniformly dispersed in the first anti-corrosion layer 12 by default.
[0027] When the nitrogen atom content in the first anti-corrosion layer 12 is too high (greater than 20At%), the degree of bonding between the amino group (NH2) and the first adhesive layer 11 increases accordingly, resulting in an increase in the hardness between the first anti-corrosion layer 12 and the first adhesive layer 11 after the reaction, and cracks are easily generated under the influence of external forces. When the soft-packaged lithium battery is used for a long time, the intruded moisture will react with the electrolyte to generate hydrogen fluoride. Hydrogen fluoride easily invades from the cracks, resulting in a decrease in the peel strength between the first anti-corrosion layer 12 and the first adhesive layer 11, and eventually delamination. Therefore, controlling the content of nitrogen atoms in the first anti-corrosion layer 12 within the above range is beneficial to improving the peel strength between the first anti-corrosion layer 12 and the first adhesive layer 11.
[0028] Exemplarily, the content of nitrogen atoms in the first anti-corrosion layer 12 is any value of 0.1At%, 1At%, 3At%, 5At%, 8At%, 10At%, 13At%, 15At%, 18At%, 20At% or between any two values.
[0029] In summary, the present application uses the amino group of the nitrogen-containing polymer used in the first anti-corrosion layer 12 to react with the acid-modified group and / or isocyanate group in the first adhesive layer 11, and at the same time controls the content of nitrogen atoms in the first anti-corrosion layer, which not only allows the first anti-corrosion layer 12 to be bonded to the first adhesive layer 11 through a covalent bond, thereby effectively improving the adhesion between the two, and further makes the intermediate metal layer 13 and the hot-melt resin layer 10 firmly connected, thereby improving the initial peel strength between the intermediate metal layer 13 and the hot-melt resin layer 10 of the metal composite film 1000, and the corrosion resistance in anhydrous and aqueous electrolyte environments, which not only can achieve the long-term stability of the metal composite film 1000 when used as an outer packaging material for lithium-ion battery devices, but also the first anti-corrosion layer 12 can be adapted to different types of first adhesive layers, which is beneficial to improving the production efficiency of the metal composite film 1000 and reducing the production cost.
[0030] In some optional embodiments, see Figures 2 to 5 The metal composite film 1000 further includes a second adhesive layer 15 , and the second adhesive layer 15 is located between the outer base resin layer 16 and the intermediate metal layer 13 .
[0031] The introduction of the second adhesive layer is beneficial to improving the adhesion between the outer substrate resin layer 16 and the intermediate metal layer 13, thereby improving the initial peel strength between the intermediate metal layer 13 and the outer substrate resin layer 16, which is beneficial to improving the long-term stability of the metal composite film 1000 when used as an outer packaging material for lithium-ion battery devices.
[0032] In some optional embodiments, see Figures 3 to 5 The metal composite film 1000 further includes a second anti-corrosion layer 14 , and the second anti-corrosion layer 14 is located between the second adhesive layer 15 and the intermediate metal layer 13 .
[0033] The second anti-corrosion layer 14 is provided to further improve the corrosion resistance of the metal composite film 1000 when used as an outer packaging material for a lithium-ion battery device.
[0034] In some optional embodiments, see Figure 3 The metal composite film 1000 is composed of a heat-melting resin layer 10, a first adhesive layer 11, a first anti-corrosion layer 12, an intermediate metal layer 13, a second anti-corrosion layer 14, a second adhesive layer 15 and an outer base resin layer 16 which are stacked in sequence.
[0035] See also Figure 4 as well as Figure 5 In some optional embodiments, the metal composite film 1000 further includes a coloring layer 17, such as Figure 4 As shown, the colored layer 17 is set between the outer base resin layer 16 and the second adhesive layer 15, or as shown in Figure 5 As shown, the colored layer 17 is provided on the side of the outer base resin layer 16 facing away from the intermediate metal layer 13 .
[0036] By providing the coloring layer 17 , the metal composite film 1000 can meet different usage requirements.
[0037] In some optional embodiments, the second adhesive layer 15 contains a colorant. That is, by directly adding the colorant into the second adhesive layer 15, the coloring layer 17 is directly compounded with the second adhesive layer 15, thereby effectively reducing the preparation cost.
[0038] The following is a detailed description of each layer:
[0039] [Thermal fusion resin layer 10]
[0040] When the metal composite film 1000 is used as an outer packaging material for lithium ion batteries, the heat-welding resin layer 10 corresponds to the innermost layer and is a layer (heat-sealing layer) that seals the battery element by heat-welding the heat-welding resin layers when assembling the battery.
[0041] The resin constituting the heat-welding resin layer 10 is not particularly limited as long as it is heat-weldable, and is preferably a resin containing a polyolefin main chain such as polyolefin or acid-modified polyolefin.
[0042] As polyolefins, specifically, polyethylene ethylene-α-olefin copolymers such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene can be cited; polypropylene such as homopolypropylene, polypropylene block copolymers (such as block copolymers of propylene and ethylene), and random copolymers of polypropylene (such as random copolymers of propylene and ethylene); propylene-α-olefin copolymers; terpolymers of ethylene-butene-propylene, etc. Among them, polypropylene is preferred. The polyolefin resin used as a copolymer can be a block copolymer or a random copolymer. These polyolefin-based resins can be used alone or in combination of two or more.
[0043] Acid-modified polyolefin is a polymer modified by block polymerization or graft polymerization with an acid component and a polyolefin. As the acid-modified polyolefin, a copolymer formed by copolymerization of a polar molecule such as the above-mentioned polyacrylic acid or methacrylic acid with the above-mentioned polyolefin can also be used. In addition, as the acid component used in the acid modification, carboxylic acids or sulfonic acids such as maleic acid, acrylic acid, itaconic acid, crotonic acid, maleic anhydride, itaconic anhydride, and their anhydrides can be used, preferably acrylic acid or maleic acid and their anhydrides.
[0044] The heat-welding resin layer 10 may be composed of one resin alone or a combination of two or more resins. The heat-welding resin layer 10 may be composed of only one layer or two or more layers of the same or different resins.
[0045] The heat-welding resin layer 10 may also contain a lubricant as required. When the heat-welding resin layer 10 contains a lubricant, the moldability of the outer packaging material for lithium-ion batteries can be improved. The type of lubricant is not particularly limited and can be selected and used within a known range. One type of lubricant can be used alone or two or more types can be used in combination.
[0046] The lubricant is not particularly limited, but an amide lubricant is preferably used. The lubricant may be used alone or in combination of two or more. The amide lubricant is preferably used on the surface of the outer base resin layer 16 .
[0047] When a lubricant is present on the surface of the heat-welding resin layer 10, the content thereof is not particularly limited, but from the viewpoint of improving the moldability of the electronic packaging material, 10 to 50 mg / m2 is preferred, and 15 to 40 mg / m2 is more preferred.
[0048] The lubricant present on the surface of the heat-welding resin layer 10 may be a lubricant seeping out from the resin constituting the heat-welding resin layer 10 , or may be a lubricant coated on the surface of the heat-welding resin layer 10 .
[0049] There is no particular limitation on the thickness of the heat-welding resin layer 10 as long as the heat-welding resin layers can perform the function of sealing the battery element after heat-welding each other. The thickness can be about 100 μm or less, and more preferably about 25-80 μm.
[0050] The heat-welding resin layer 10 may also contain ingredients such as antioxidants as needed. The heat-welding resin layer 10 containing an antioxidant can suppress thermal degradation during the manufacturing process. The type of antioxidant is not particularly limited and can be selected and used within a known range. One antioxidant can be used alone or in combination of two or more.
[0051] The heat-melting resin in the present application is a single layer or a composite layer composed of one or a mixture of two or more of acid-modified polyolefin resin, homopolymer polypropylene resin, block copolymer polypropylene resin, random copolymer polypropylene resin, and polyethylene resin.
[0052] The resin used in the heat-welding resin layer 10 is a single layer or a composite layer composed of one or a mixture of two or more resins with a melting point of 120-162°C, more preferably 130-162°C, an MFR (230°C) of 2-15g / 10min, more preferably an MFR (230°C) of 3-12g / 10min, and a thickness of 20-120μm, more preferably 25-80μm. In addition, in the case where the inner welding resin layer is a composite layer, the thickness of the resin on the reverse side in contact with the intermediate metal layer 13 is more than 2μm and the melting point is 130-152°C. When the melting point is below 120°C, the fluidity is high when heated, and when pressurized heat sealing is performed, the thickness becomes thinner, and the adhesion to the intermediate metal layer 13 decreases. In addition, the pressurization causes the squeezed resin inside the battery to flow to the unsqueezed edge part, and the expansion and contraction of the battery and the external force of the bending process cause cracks. The electrolyte will penetrate into the intermediate metal layer 13 through the cracks, causing the insulation resistance of the heat-welded resin layer 10 to decrease, leakage occurs, and the battery life will be shortened. When the melting point exceeds 162°C, the crystallinity of the resin increases, making the fluidity during pressurized heat sealing relatively low, and the heat resistance is improved, but when the high-crystalline resin is heat-sealed, a hard and brittle resin layer is formed. Therefore, under the conditions of expansion and contraction of the battery and the external force of the bending process, the resin layer is prone to cracking, and long-term stable sealing cannot be obtained. When the MFR (230°C) of the resin is lower than 2g / 10min, the fluidity of the resin is low during pressurized heat sealing, and it is difficult to obtain stable sealing. When the MFR (230°C) of the resin exceeds 15g / 10min, the resin fluidity is too high during pressurized heat sealing, the resin thickness becomes seriously thin, and it is difficult to obtain stable sealing. In addition, the pressurization causes the squeezed resin inside the battery to flow to the unsqueezed edge portion, and the expansion and contraction of the battery and the external force of the bending process cause cracks. The electrolyte will penetrate into the intermediate metal layer 13 through the cracks, causing the insulation resistance of the heat-welding resin layer 10 to decrease, leakage occurs, and the battery life will be shortened. When the thickness of the heat-welding resin layer 10 is less than 20μm, it is difficult to obtain a uniform heat-welding portion, and it is even more difficult to obtain a stable seal because the thickness cannot fully cover the deviation of the mechanical processing size and conditions of the heat sealing device. In addition, the pressurization causes the squeezed resin inside the battery to flow to the unsqueezed edge portion, and the thickness of the heat-welding resin layer 10 becomes thinner. The expansion and contraction of the battery and the external force of the bending process easily cause cracks. The electrolyte will penetrate into the intermediate metal layer 13 through the cracks, causing the insulation resistance of the heat-welding resin layer 10 to decrease, leakage occurs, and the battery life will be shortened. When the thickness of the heat-melting resin layer 10 exceeds 120μm, the water vapor permeability will increase, the moisture inside the battery will increase, and it will react with the electrolyte to produce gas, which is prone to expansion, rupture, and leakage. The battery life is shortened, and excessive hydrogen fluoride corrodes the anti-corrosion treated metal layer, resulting in a decrease in the adhesion strength between the intermediate metal layer 13 and the heat-melting resin layer 10, which is prone to problems such as electrolyte leakage.
[0053] [First Adhesive Layer 11]
[0054] The first adhesive layer 11 is an intermediate layer provided to firmly bond the heat-welding resin layer 10 and the intermediate metal layer 13 .
[0055] The first adhesive layer 11 is formed of a resin capable of bonding the intermediate metal layer 13 and the hot-melt resin layer 10, and the first adhesive layer 11 includes an acid-modified group and / or an isocyanate group, and the acid-modified group includes but is not limited to at least one of a carboxyl group, a sulfonic acid group, a maleic acid group, a sulfinic acid group, a sulfenic acid group, a phosphoric acid group, a phosphonic acid group, and the like.
[0056] That is, the first adhesive layer 11 can use acid-modified polyolefin resins such as carboxylic acid-modified polyolefin, carboxylic acid-modified cyclic polyolefin, methacrylic acid-modified polyolefin, acrylic acid-modified polyolefin, and crotonic acid-modified polyolefin. From the viewpoint of improving the adhesion between the intermediate metal layer 13 and the inner heat-melting resin layer 10, as modified polyolefins, modified polyolefin resins such as acrylic acid, methacrylic acid, maleic acid, and anhydrous maleic anhydride are preferred. The resin constituting the first adhesive layer 11 may or may not contain a polyolefin main chain, preferably containing a polyolefin main chain. Whether the resin constituting the first adhesive layer 11 contains a polyolefin main chain can be analyzed by, for example, infrared spectroscopy, gas chromatography-mass spectrometry, etc., and the analysis method is not particularly limited. The polyolefin and its modified resin used in the first adhesive layer 11 can be the same as the resin used in the heat-melting resin layer 10, which is a polypropylene resin or a copolymer of propylene and ethylene.
[0057] From the viewpoint of long-term use stability of the lithium ion battery packaging material, the first adhesive layer 11 may be a resin composition containing an acid-modified polyolefin and a curing agent. The acid-modified polyolefin is particularly preferably a polyolefin modified with maleic anhydride or acrylic acid.
[0058] The curing agent is not particularly limited as long as it can cure the acid-modified polyolefin, and epoxy curing agents, polyfunctional isocyanate curing agents, carbodiimide curing agents, oxazoline curing agents, and the like can be used.
[0059] As epoxy curing agents, there are no particular limitations as long as they are compounds having at least one epoxy group. For example, epoxy resins such as bisphenol A diglycidyl ether, modified bisphenol A diglycidyl ether, novolac glycidyl ether, glycerol polyglycidyl ether, and polyglycerol polyglycidyl ether are used. As polyfunctional isocyanate curing agents, there are no particular limitations as long as they are compounds having two or more isocyanate groups in the molecule. For example, isophorone diisocyanate (PDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), and the components after polymerization or addition of the above substances, or the reaction products of such mixtures and other polymers are used. As carbodiimide curing agents, there are no particular limitations as long as they are compounds having at least one carbodiimide group (-N=C=N-) in the molecule. Polycarbodiimide compounds having at least two or more carbodiimide groups are preferred. The oxazoline-based curing agent is not particularly limited as long as it is a compound having an oxazoline skeleton.
[0060] From the viewpoint of improving the adhesion between the first adhesive layer 11 and the heat-sealing resin layer 10 , the curing agent may be composed of two or more compounds.
[0061] The thickness of the first adhesive layer 11 is not particularly limited as long as it can function as an adhesive layer, but is preferably about 1 to 80 μm, more preferably about 1 to 50 μm.
[0062] That is, when the intermediate metal layer 13 and the heat-welding resin layer 10 are compounded, the first adhesive layer 11 may be formed of a solution-type adhesive or a hot-melt-type adhesive.
[0063] In some optional embodiments, the first adhesive layer 11 is made of a solvent-based adhesive, and the first adhesive layer contains an isocyanate group and / or an acid-modified group.
[0064] Among them, the solution-type first adhesive layer 11 is mainly composed of acid-modified polyolefin resin as the main agent and one or more of isocyanate, epoxy resin or oxazoline as a hardener or amine compounds such as triethylamine and N,N-dimethylethanolamine as a curing agent. After being dissolved in at least one or more solvents such as water, ethanol, isopropanol, ethyl acetate, methyl ethyl ketone, toluene, methylcyclohexane, etc., it is evenly coated on the anti-corrosion treated metal surface, heated to evaporate the solvent, so that the thickness of the first adhesive layer 11 reaches the expected effect, for example, about 1 to 18 μm, preferably about 1 to 15 μm.
[0065] The melting point of the acid-modified polyolefin resin in the solution-type first adhesive layer 11 is 60-155°C, the weight average molecular weight is in the range of 10,000-150,000, and the acid value of the solvent-type adhesive is in the range of 0.5-200 mgKOH / g. When an amine compound is used as a curing agent, the solution-type first adhesive layer 11 is mainly composed of an acid-modified polyolefin resin and an amine compound, and the ratio of the acid-modified polyolefin to the amine compound is 10:1-125:1, preferably 15:1-50:1. The acid used for modifying the polyolefin is maleic acid, fumaric acid, methacrylic acid, etc., and the amine compound is at least one of triethylamine or N, N-2 methylethanolamine. The acid-modified polyolefin resin is a single layer or multiple layers composed of one or more blends of a block copolymer polypropylene resin (B-PP) with a melting point of more than 110°C and a polypropylene content of more than 50%, a random copolymer polypropylene resin (R-PP), and a homopolymer polypropylene resin (H-PP).
[0066] If the melting point is below 60°C, the heat resistance is low, and the intermediate metal layer 13 and the heat-melting resin layer 10 may peel off at high temperatures. In addition, if it exceeds 155°C, the heat resistance is good, but when reacting with the curing agent, a hard resin layer will be formed, and the bending property is poor. Therefore, the flexibility of the metal composite film 1000 decreases, or cracks are generated when bent, and there is a possibility of peeling of the intermediate metal layer 13 and the heat-melting resin layer 10. If the weight-average molecular weight is below 10,000, the resin fluidity is high when heated, and the thickness will be seriously thinned during heat sealing. The adhesion strength between the intermediate metal layer 13 and the heat-melting resin layer 10 (when the curing agent is added to react) will become low, and there will be sealing problems. If the weight average molecular weight exceeds 150,000, the intermediate metal layer 13 and the heat-melting resin layer 10 (when a curing agent is added to react) will form a hard resin layer, the bending resistance will deteriorate, the flexibility of the metal composite film 1000 will decrease, or cracks will occur when bent, and there is a case where the intermediate metal layer 13 and the heat-melting resin layer 10 are peeled off. If the acid value of the acid-modified polyolefin resin is less than 0.5 mgKOH / g, there are few curing reaction points with the curing agent, and the adhesion between the intermediate metal layer 13 and the heat-melting resin layer 10 is unstable. If the acid value exceeds 200 mgKOH / g, the curing reaction between the curing agent and the acid-modified polyolefin resin is too intense, a hard resin layer will be formed, the bending resistance will deteriorate, the flexibility of the metal composite film 1000 will decrease, or cracks will occur when bent, and there is a case where the intermediate metal layer 13 and the inner heat-melting resin layer 10 are peeled off.
[0067] In some optional embodiments, the first adhesive layer 11 is made of a hot-melt adhesive, and the first adhesive layer 11 contains an acid-modified group.
[0068] The resin used in the hot-melt first adhesive layer 11 is an acid-modified polyolefin resin with a melting point of 135 to 165°C and an MFR (230°C) of 3 to 15 g / 10 min. The thickness of the formed hot-melt first adhesive layer 11 is 2 to 80 μm, preferably 5 to 50 μm. The degree of modification of the acid-modified polyolefin resin used in the hot-melt first adhesive layer 11 is 1% to 15%, preferably 3% to 12%. When the melting point of the acid-modified polyolefin resin is below 135°C, heating will cause the resin fluidity to increase, and when pressurized heat sealing, the thickness will be seriously thinned, and the adhesion strength between the intermediate metal layer 13 and the heat-melting resin layer 10 will be reduced, resulting in sealing problems. When the melting point is above 165°C, the fluidity during pressurized heat sealing is relatively low, and the heat resistance is improved. However, when compounded with the intermediate metal layer 13, the amount of heat shrinkage increases, which increases the internal stress and reduces the adhesion between the hot melt type first adhesive layer 11 and the intermediate metal layer 13. Therefore, if it is stored for a long time, it may peel off from the intermediate metal layer 13. In addition, due to the heating during heat sealing, heat shrinkage will further occur, the adhesion between the intermediate metal layer 13 will decrease, the sealing strength will decrease, and the sealing will become a big problem. If the MFR (230°C) of the acid-modified polyolefin resin is lower than 3g / 10min, when it is extruded onto the intermediate metal layer 13 after hot melting and compounded, the extrusion film forming property is prone to instability. If the MFR (230°C) of the acid-modified polyolefin resin is higher than 15g / 10min, heating will cause the resin fluidity to increase, and the thickness will be seriously thinned during pressurized heat sealing. The adhesion strength between the intermediate metal layer 13 and the hot-melt resin layer 10 will decrease, and there will be sealing problems. When the thickness of the hot-melt type first adhesive layer 11 is less than 2 μm, the heat shrinkage cannot be absorbed when compounded with the intermediate metal layer 13 because the heat shrinkage is too much. Therefore, due to the increase in internal stress, the adhesion with the intermediate metal layer 13 is reduced. If it is stored for a long time, it may peel off from the intermediate metal layer 13. When the thickness of the hot-melt type first adhesive layer 11 exceeds 80 μm, there will be no physical property problems, but it will lead to an increase in production prices, so it is best to avoid using it. When the modification degree of the hot-melt type first adhesive layer 11 is less than 1%, the adhesion with the intermediate metal layer 13 will be unstable. If the modification degree exceeds 15%, although there will be no physical property problems, it will lead to an increase in production prices, so it is best to avoid this phenomenon.
[0069] [First anti-corrosion layer 12]
[0070] The first anti-corrosion layer 12 in the lithium-ion battery packaging material is used to prevent the hydrogen fluoride generated by the reaction of the electrolyte and moisture from corroding the surface of the intermediate metal layer 13, prevent the intermediate metal layer 13 from separating from the heat-melting resin layer 10, and at the same time maintain the uniformity of the surface of the intermediate metal layer 13 to minimize the change in adhesion (wettability), thereby preventing the intermediate metal layer 13 from stratifying from the heat-melting resin layer 10.
[0071] At present, the outer packaging materials for lithium-ion battery devices on the market select anti-corrosion liquids of different compositions according to the type of the first adhesive layer. This practice not only has low production efficiency but also high production costs.
[0072] In the present application, the first adhesive layer 11 includes acid-modified groups and / or isocyanate groups, and the first anti-corrosion layer 12 includes a nitrogen-containing polymer having an amino group that reacts with the acid-modified groups and / or isocyanate groups in the first adhesive layer 11. The content of nitrogen atoms in the first anti-corrosion layer 12 is greater than 0 and less than or equal to 20At%.
[0073] The nitrogen-containing polymer includes but is not limited to at least one of polyurethane, polyacrylamide, urea-formaldehyde resin, amino resin, melamine, etc., as long as it contains an amino group that can react with the acid-modified group. When the first adhesive layer 11 includes an isocyanate group, the amino group (NH2) in the nitrogen-containing polymer can react with the isocyanate group (NCO) in the first adhesive layer 11 to generate a urea group; when the first adhesive layer 11 includes an acid-modified group, the amino group (NH2) in the nitrogen-containing polymer can react with the acid-modified group in the first adhesive layer 11 to generate an amino compound. Both reactions have covalent bonding properties, thereby achieving a strong adhesive force.
[0074] The content of nitrogen atoms in the first anti-corrosion layer 12 refers to the element content deep in the first anti-corrosion layer 12 detected by the method described later (XPS-ESCA method), and the elements added to the first anti-corrosion layer 12 are uniformly dispersed in the first anti-corrosion layer 12 by default.
[0075] When the nitrogen atom content in the first anti-corrosion layer 12 is too high (greater than 20At%), the degree of bonding between the amino group (NH2) and the first adhesive layer 11 increases accordingly, resulting in an increase in the hardness between the first anti-corrosion layer 12 and the first adhesive layer 11 after the reaction, and cracks are easily generated under the influence of external forces. When the soft-packaged lithium battery is used for a long time, the intruded moisture will react with the electrolyte to generate hydrogen fluoride. Hydrogen fluoride easily invades from the cracks, resulting in a decrease in the peel strength between the first anti-corrosion layer 12 and the first adhesive layer 11, and eventually delamination. Therefore, controlling the content of nitrogen atoms in the first anti-corrosion layer 12 within the above range is beneficial to improving the peel strength between the first anti-corrosion layer 12 and the first adhesive layer 11.
[0076] Exemplarily, the content of nitrogen atoms in the first anti-corrosion layer 12 is any value of 0.1At%, 1At%, 3At%, 5At%, 8At%, 10At%, 13At%, 15At%, 18At%, 20At% or between any two values.
[0077] That is, the amino group of the nitrogen-containing polymer used in the first anti-corrosion layer 12 of the present application can react with the acid-modified group and / or isocyanate group in the first adhesive layer 11, and at the same time control the content of nitrogen atoms in the first anti-corrosion layer, which can not only make the first anti-corrosion layer 12 and the first adhesive layer 11 bonded by covalent bonds, thereby effectively improving the adhesion between the two, but also further make the intermediate metal layer 13 and the hot-melt resin layer 10 firmly connected, thereby improving the initial peel strength between the intermediate metal layer 13 and the hot-melt resin layer 10 of the metal composite film 1000, and the corrosion resistance in anhydrous and aqueous electrolyte environments, not only can the long-term stability of the metal composite film 1000 be achieved when it is used as an outer packaging material for lithium-ion battery devices, but also the first anti-corrosion layer 12 can be adapted to different types of first adhesive layers (solvent-based adhesives and hot-melt adhesives), which is beneficial to improving the production efficiency of the metal composite film 1000 and reducing the production cost.
[0078] In some optional embodiments, the content of nitrogen atoms in the first anti-corrosion layer 12 is 1At%-20At%.
[0079] Controlling the content of nitrogen atoms in the first anti-corrosion layer 12 within the above range is beneficial to improving the peel strength between the first anti-corrosion layer 12 and the first adhesive layer 11 .
[0080] Exemplarily, the content of nitrogen atoms in the first anti-corrosion layer 12 is any value of 1At%, 3At%, 5At%, 8At%, 10At%, 13At%, 15At%, 18At%, 20At% or between any two values.
[0081] In some optional embodiments, the first anti-corrosion layer is formed by coating and heat treating the anti-corrosion liquid; wherein the mass percentage of the nitrogen-containing polymer in the anti-corrosion liquid is 0.1%-3%.
[0082] By controlling the mass percentage of the nitrogen-containing polymer in the anti-corrosion liquid to 0.1%-3.0%, the first anti-corrosion layer can correspond to different types of first adhesive layers (solvent-based adhesives and hot-melt adhesives) and can be combined through covalent bonds, so that the intermediate metal layer 13 and the hot-melt resin layer 10 are firmly connected, effectively improving the peel strength and stability.
[0083] Exemplarily, the mass percentage of the nitrogen-containing polymer in the anti-corrosion liquid is any value of 0.1%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, or between any two values.
[0084] At present, the outer packaging materials for lithium-ion battery devices on the market will select anti-corrosion liquids of different components according to the type of the first adhesive layer. This practice not only has low production efficiency, but also high production costs. The nitrogen-containing polymer in the present application can react with the solution-type first adhesive and the hot-melt-type first adhesive to form a covalent bond, and the amount of the nitrogen-containing polymer added is within the above range, which is conducive to the first anti-corrosion layer being able to form a first adhesive layer with long-term stable composite properties, so that when the electrolyte penetrates, it is conducive to maintaining the stability of the peel strength.
[0085] In some optional embodiments, the anti-corrosion liquid also includes at least one of a carboxylic acid-containing polymer, a hydroxyl acrylic resin and a cross-linking agent, wherein the mass percentage of the carboxylic acid-containing polymer in the anti-corrosion liquid is 0.1%-2.0%, the mass percentage of the hydroxyl acrylic resin in the anti-corrosion liquid is 0.1%-2.0%, and the mass percentage of the cross-linking agent in the anti-corrosion liquid is 0.5%-5%.
[0086] Among them, nitrogen-containing polymers have higher activity, and the main chain is easy to break in a long period. The use of carboxylic acid-containing polymers can alleviate the failure of nitrogen in a long period, passivate nitrogen atoms, and inhibit the main chain of nitrogen-containing polymers from breaking in a long period, which is beneficial to improving the long-term effectiveness of the metal composite film.
[0087] The hydroxy acrylic resin can not only help improve the durability of the material, but also assist the nitrogen-containing polymer, so that the hydroxy acrylic resin can react with the cross-linking agent of the first anti-corrosion layer 12 itself and the first adhesive layer 11 formed by the solution-type adhesive, thereby improving the cross-linking density of the first anti-corrosion layer 12 and improving the overall long-term effectiveness.
[0088] By adding a cross-linking agent, the cross-linking density of the first anti-corrosion layer 12 can be increased, thereby stabilizing the tolerance of the first anti-corrosion layer 12 to the electrolyte as its content and the hydrogen fluoride produced by the reaction of the electrolyte and water. In addition, by controlling the upper limit of the addition of the cross-linking agent, it is possible to suppress the problem that the first anti-corrosion layer 12 is too hard due to excessive addition of the cross-linking agent, which makes it easy for the anti-corrosion layer to crack and peel off during the molding process, thereby reducing the corrosion resistance.
[0089] The present application helps to improve the overall long-term effectiveness by controlling the introduction and addition ratio of each component within the above-mentioned reasonable range.
[0090] Exemplarily, the mass percentage of the carboxylic acid-containing polymer in the anti-corrosion liquid is any value among 0.1%, 0.5%, 1.0%, 1.5%, 2.0%, or between any two values.
[0091] Exemplarily, the mass percentage of the hydroxy acrylic resin in the anti-corrosion liquid is any value among 0.1%, 0.5%, 1.0%, 1.5%, 2.0%, or between any two values.
[0092] Illustratively, the mass percentage of the cross-linking agent in the anti-corrosion liquid is any value of 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0% or between any two values.
[0093] Optionally, the anti-corrosion liquid includes a carboxylic acid polymer, a hydroxy acrylic resin and a cross-linking agent.
[0094] By simultaneously introducing the carboxylic acid-containing polymer, the hydroxyl acrylic resin and the crosslinking agent, it is beneficial to improve the direct bonding stability between the first adhesive layer 11 and the first anti-corrosion layer 12, so that when the electrolyte penetrates, the bonding force is suppressed from decreasing and the stability of the peel strength is ensured. In some optional embodiments, the carboxyl groups on the carbon chain of the carboxylic acid-containing polymer are spaced no more than 5 carbon atoms apart.
[0095] By controlling the distance between carboxyl groups on the carbon chain of the carboxylic acid-containing polymer to be no more than 5 carbon atoms, after the carboxyl groups are combined with the nitrogen-containing polymer, the carbon atom (C) cannot rotate freely due to the high density of carboxyl groups on the carbon chain, thereby relatively stabilizing the amino group in the nitrogen-containing polymer and making it difficult for the main chain to break over a long period of time, which is beneficial to improving the long-term effectiveness of the first anti-corrosion layer 12.
[0096] For example, the carboxylic acid-containing polymer having a carboxyl group interval of no more than 5 carbon atoms on the carbon chain includes but is not limited to polyacrylic acid and the like.
[0097] In some alternative embodiments, the carboxylic acid-containing polymer includes a phosphonocarboxylic acid copolymer.
[0098] The phosphonocarboxylic acid copolymer can not only be used as an amino protective agent, but also has excellent dispersibility, which can effectively improve the long-term effectiveness of the first anti-corrosion layer 12 .
[0099] In some optional embodiments, the cross-linking agent includes at least one of an epoxy compound, an oxazoline compound, and adipic acid dihydrazide compound.
[0100] By adding the crosslinking agent, the crosslinking density of the first anticorrosion layer 12 can be increased, and the resistance of the first anticorrosion layer 12 to the electrolyte as a content and hydrogen fluoride generated by the reaction between the electrolyte and water can be stabilized.
[0101] In some optional embodiments, the anti-corrosion liquid also includes a trivalent metal compound, an inorganic acid and an organic resin, wherein the trivalent metal compound is a trivalent chromium compound or a trivalent cerium compound, the mass percentage of the trivalent metal compound in the anti-corrosion liquid is 1.9%-6%, the mass percentage of the inorganic acid in the anti-corrosion liquid is 0.3%-6%, and the mass percentage of the organic resin in the anti-corrosion liquid is 0.6%-6%.
[0102] The organic resin is composed of polyacrylic acid resin and / or polyvinyl alcohol, and the polyacrylic acid resin is one or more of polyacrylic acid, polymethyl acrylate, copolymer of acrylic acid and maleic acid, copolymer of acrylic acid and styrene, and their sodium salt and ammonium salt derivatives.
[0103] Exemplarily, the organic resin is composed of at least one of acrylic resin, methacrylic resin, hydroxy acrylic resin, polyvinyl alcohol resin, olefin resin, and phenolic resin.
[0104] Among them, the trivalent chromium compound in the anti-corrosion liquid is composed of at least one of chromium nitrate, chromium phosphate, chromium chloride, and chromium fluoride; the trivalent cerium compound is composed of at least one of cerium nitrate, cerium phosphate, and cerium chloride; among them, the trivalent metal compound can react with the phosphonocarboxylic acid copolymer to form a stable complex, thereby improving the long-term effectiveness of the first anti-corrosion layer.
[0105] Optionally, the trivalent chromium compound is one of chromium nitrate and chromium fluoride. Chromium nitrate and chromium fluoride react with the resin, the intermediate metal layer and the inorganic acid in the first anti-corrosion layer. Chromium fluoride can improve the ability of the first anti-corrosion layer to resist hydrogen fluoride, and can ensure the stability of the peel strength of the heat-welded resin layer and the intermediate metal layer during long-term storage.
[0106] The inorganic acid is at least one of nitric acid and phosphoric acid. 21. The inorganic acid can remove the surface oxide film of the intermediate metal layer, so that the metal can quickly react with the components in the anti-corrosion layer to form a strong chromium reaction product. This can ensure the stability of the peel strength between the heat-welded resin layer and the intermediate metal layer when the composite film is stored for a long time.
[0107] Exemplarily, the mass percentage of the trivalent metal compound in the anti-corrosion liquid is any value of 1.9%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, 5.5%, 6.0% or between any two values.
[0108] Exemplarily, the mass percentage of the inorganic acid in the anti-corrosion liquid is any value of 0.3%, 1%, 2%, 3%, 4%, 5%, 6%, or between any two values.
[0109] Exemplarily, the mass percentage of the organic resin in the anti-corrosion liquid is any value of 0.6%, 1%, 2%, 3%, 4%, 5%, 6%, or between any two values.
[0110] In some optional embodiments, the anti-corrosion liquid includes a titanium compound or a zirconium compound, the mass percentage of the titanium compound in the anti-corrosion liquid is 0-0.6%, and the mass percentage of the zirconium compound in the anti-corrosion liquid is 0-2.8%.
[0111] The titanium compound or zirconium compound can improve the stability and uniformity of the reaction between chromium and resin, metal and inorganic acid. The titanium compound is at least one of titanium fluoride and titanium nitrate, and the zirconium compound is at least one of zirconium fluoride and zirconium nitrate.
[0112] Exemplarily, the mass percentage of the titanium compound in the anti-corrosion liquid is any value among 0%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6% or between any two values, and the mass percentage of the zirconium compound in the anti-corrosion liquid is any value among 0%, 0.1%, 0.3%, 0.5%, 0.8%, 1.0%, 1.3%, 1.5%, 1.7%, 2.0%, 2.3%, 2.5%, 2.8% or between any two values.
[0113] It is understandable that it should be noted that, in addition to the above-mentioned nitrogen-containing polymer, carboxylic acid-containing polymer, hydroxy acrylic resin, crosslinking agent and other components, the anticorrosion liquid also includes a solvent, wherein the mass percentage of each component and solvent is 100%. Among them, the solvent is an organic solvent, water, or a mixture of water and an organic solvent, that is, the organic solvent can be used alone as a solvent or added to water. The wettability of the anticorrosion liquid can be improved, and the reaction stability of the first anticorrosion layer and the intermediate metal layer can be improved. In addition, the surface tension of the anticorrosion liquid can be reduced, and the uniformity of the coating film can be improved. As an organic solvent, one can be selected from isopropyl alcohol, ethanol, and ethylene glycol butyl ether.
[0114] Exemplarily, the mass percentage of the solvent in the anti-corrosion liquid is 78.6-97.2%.
[0115] The coating method of the anti-corrosion liquid may include: first, using alkaline immersion method, electrolytic cleaning method, acid cleaning method, electrolytic acid cleaning method, oxygen activation method, heat treatment (annealing treatment) during calendering and other treatment methods to degrease at least the heat-welding resin layer of the intermediate metal layer. Secondly, the anti-corrosion liquid used is coated by rod coating method, roller coating method, gravure coating method, dipping method and other methods, and acts on the surface of the intermediate metal layer through high-temperature chemical reaction. The coating wet film amount of the anti-corrosion liquid on the intermediate metal layer 13 is in the range of 1.6-3.2g / m 2After applying the anti-corrosion liquid, heat treatment is performed at a high temperature of 130-200°C for 0.5-5 minutes to form an anti-corrosion layer.
[0116] The thickness of the first anticorrosion layer 12 is not particularly limited, but is preferably 1 nm to 3.0 μm, more preferably 1 nm to 1.5 μm, from the viewpoint of adhesion between the intermediate metal layer 13 and the heat-welding resin layer.
[0117]
Middle metal layer 13
[0118] The intermediate metal layer 13 in the metal composite film 1000 serves as a barrier layer capable of at least suppressing the intrusion of moisture during use.
[0119] Specifically, the metal material used for the intermediate metal layer 13 may be aluminum alloy, stainless steel, titanium steel, nickel-plated steel plate, or the like.
[0120] In some optional embodiments, the intermediate metal layer 13 is a nickel-plated steel plate. When the intermediate metal layer 13 is a nickel-plated steel plate, the nickel-plated layer has anti-corrosion effects such as rust prevention, and also has the effect of improving surface cleanliness. By forming the anti-corrosion layer described later on the nickel-plated surface, the electrolyte resistance is greatly improved through the anti-corrosion property of the nickel-plated layer and the synergistic effect with the anti-corrosion layer. The thickness of the nickel-plated layer can be less than 20μm. Preferably, it is more than 1μm and less than 5μm. When it exceeds 20μm, although the anti-corrosion performance is improved, cracks are easily generated due to external pressure loads such as molding.
[0121] In addition, the surface cleanliness of the intermediate metal layer 13 has a great influence on the anti-corrosion effect, so the management of the surface cleanliness of the intermediate metal layer 13 becomes very important. Surface cleanliness can be managed by a method using a wetting reagent to test wettability as an indicator or a method using a contact angle as an indicator. As an indicator of wettability, it is D grade and above, preferably B grade. In addition, as an indicator of the contact angle, when tested with pure water, the contact angle is below 25°, preferably below 20°, and more preferably below 15°. When the wettability is lower than Class D, or the contact angle exceeds 25°, the reactivity or initial adhesion with the anti-corrosion layer described later will deteriorate. If the reactivity deteriorates, the reaction of the first anti-corrosion layer 12 / the second anti-corrosion layer 14 and the intermediate metal layer 13 becomes insufficient, and the resistance to the penetration of the electrolyte as the battery contents and the resistance to hydrogen fluoride produced in the reaction of the electrolyte and water will decrease. As time goes by, the adhesion of the first anticorrosion layer 12 / second anticorrosion layer 14 to the intermediate metal layer 13 decreases, the first anticorrosion layer 12 / second anticorrosion layer 14 dissolves, and the intermediate metal layer 13 and the first / second anticorrosion layer 14 may peel off, thereby shortening the life of the battery. In addition, the same situation will occur when the initial adhesion between the first anticorrosion layer 12 / second anticorrosion layer 14 and the intermediate metal layer 13 deteriorates.
[0122] The surface wettability test method of the intermediate metal layer 13 may adopt "National Standard of the People's Republic of China GB / T225638.5-2016, Metal Test Methods, Part 5: Wettability Detection". The contact angle test method of the intermediate metal layer 13 may adopt "National Standard of the People's Republic of China GB / T22638.9-2008, Metal Test Methods Part 9: Determination of Hydrophilicity".
[0123] [Second anti-corrosion layer 14]
[0124] The second anti-corrosion layer 14 is located between the second adhesive layer 15 and the intermediate metal layer 13, and is used to prevent the intermediate metal layer 13 from being separated from the external resin layer.
[0125] It should be noted that the composition of the second anti-corrosion layer 14 may be the same as or different from that of the first anti-corrosion layer 12 . Preferably, the composition of the second anti-corrosion layer 14 may be the same as that of the first anti-corrosion layer 12 .
[0126] The thickness of the second anti-corrosion layer 14 may be the same as or different from the thickness of the first anti-corrosion layer 12 , and those skilled in the art may set the thickness according to actual needs.
[0127] [Second Adhesive Layer 15]
[0128] The second adhesive layer 15 is a layer formed for the purpose of improving the adhesion between the outer base resin layer 16 and the intermediate metal layer 13 .
[0129] The second adhesive layer 15 is formed by an adhesive capable of bonding the outer base resin layer 16 and the intermediate metal layer 13. The adhesive used to form the second adhesive layer 15 is not limited, and it can be, for example, a two-component curing adhesive (two-component adhesive), or a one-component curing adhesive (one-component adhesive). The adhesive used to form the second adhesive layer 15 can be any of a chemical reaction type, a solvent volatilization type, a hot melt type, a hot pressing type, etc. In addition, the second adhesive layer 15 can be a single layer or a multilayer.
[0130] The composition of the second adhesive layer 15 can be the same as or different from that of the first adhesive layer 11. Usually, the second adhesive layer 15 is a two-component polyurethane adhesive formed by using polyester polyol and polyol modified with polyol as diol main agent and aromatic or aliphatic isocyanate as curing agent. The curing agent can be selected according to the functional groups of the adhesive components, such as multifunctional epoxy resin, polymer containing methanesulfonic acid, polyamine resin, inorganic acid, etc. In addition, the main agent used in the outer adhesive layer includes polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyethylene isophthalate, and copolymerized polyester; polyether resin; polyurethane resin; epoxy resin; phenolic resin; polyamide resins such as nylon 6, nylon 66, nylon 12, and copolymerized polyamide; polyolefin resins such as polyolefin, cyclic polyolefin, acid-modified polyolefin, and acid-modified cyclic polyolefin; polyvinyl acetate; cellulose; (meth) acrylic resin; polyimide resin; polycarbonate; amino resins such as urea resin and melamine resin; rubbers such as chloroprene rubber, nitrile rubber, and styrene-butadiene rubber; silicone resin, etc. These adhesive components can be used alone or in combination of two or more.
[0131] The preferred combination of the second adhesive layer 15 in the present application is a combination of a binary or multi-component polyester, one or two of a polyurethane-modified polyester and an isocyanate. Isocyanates are not particularly limited to compounds having two or more isocyanate groups in the molecule. For example, isophorone diisocyanate (IPDI), toluene diisocyanate (TDI), diphenylmethane-4,4-diisocyanate (DDI), and polyisocyanate. , -diisocyanate (MDI), hexamethylene diisocyanate (HDI) and other polymers, or a mixture of two or more thereof.
[0132] In some optional embodiments, the second anti-corrosion layer 14 includes a nitrogen-containing polymer having an amine group, and the second adhesive layer 15 includes an acid-modified group and / or an isocyanate group that reacts with the amine group.
[0133] The specific composition of the second anticorrosion layer 14 can refer to the configuration of the first anticorrosion layer 12, and will not be described in detail here. The acid-modified group includes but is not limited to at least one of carboxyl, sulfonic acid, maleic acid, sulfinic acid, sulfenic acid, phosphoric acid, phosphonic acid, etc.
[0134] The second adhesive layer 15 may contain other components as long as they do not impair the adhesiveness, and may contain a colorant, a thermoplastic elastomer, a tackifier, a filler, and the like.
[0135] In some optional embodiments, the second adhesive layer 15 contains a colorant. The second adhesive layer 15 contains a colorant, so that the lithium ion battery packaging material can be colored. As the colorant, a colorant such as a pigment or a dye can be used. In addition, the colorant can be used alone or in combination of two or more.
[0136] The type of pigment is not particularly limited as long as it does not impair the adhesiveness of the second adhesive layer 15. As organic pigments, for example, azo, phthalocyanine, quinacridone, anthraquinone, dioxazine, indigothioindigo, perylene, isoindoline and the like pigments can be used; as inorganic pigments, carbon black, titanium oxide, cadmium, lead, isoindoline and the like pigments can be used.
[0137] Among the colorants, carbon black is preferred in order to make the appearance of the lithium ion battery packaging material black, for example.
[0138] The average particle size of the pigment is not particularly limited, and can be selected from about 0.05 to 5 μm, preferably about 0.08 to 2 μm. The average particle size of the pigment is a median particle size measured by a laser diffraction / scattering particle size distribution measuring device.
[0139] The content of the pigment in the second adhesive layer 15 is not particularly limited as long as the lithium ion battery packaging material is colored, but is preferably about 5 to 60%, more preferably 10 to 40%.
[0140] The thickness of the second adhesive layer 15 is not particularly limited as long as the outer base resin layer 16 and the intermediate metal layer 13 can be bonded to each other. The preferred range is about 1 to 10 μm, and more preferably about 2 to 5 μm.
[0141] [Outer base resin layer 16]
[0142] When the metal composite film 1000 is used as a lithium ion battery packaging material, the outer base resin layer 16 is located on the outer layer side of the lithium ion battery packaging material. The outer base resin layer 16 is provided to enable the film to function as a base material of the lithium ion battery packaging material.
[0143] The material for forming the outer base resin layer 16 is not particularly limited as long as it has at least insulating properties.
[0144] There are many methods for making the outer substrate resin layer 16. For example, it can be a resin film directly formed from a resin, or it can be a coated resin product. As a resin film, it can be an unstretched film or a stretched film. As a stretched film, it can be a uniaxial stretched film or a biaxial stretched film, preferably a biaxial stretched film. As a method for making a biaxial stretched film, for example, a step-by-step biaxial stretching method, a blown film method, and a synchronous stretching method. As a resin coating method, for example, a roll coating method, a micro-concave coating method, an extrusion coating method, etc.
[0145] The resin forming the outer base resin layer 16 may be, for example, polyester, polyamide, polyolefin, epoxy resin, acrylic resin, fluororesin, polyurethane, silicone resin, phenolic resin or modified products of these resins. In addition, the resin forming the outer base resin layer 16 may be a copolymer of these resins, a modified product of the copolymer, or a mixture of these resins, preferably a single layer or multiple layers.
[0146] As the resin forming the outer base resin layer 16, polyester and polyamide are preferably mentioned above.
[0147] As polyester, specifically, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyethylene isophthalate, copolyester, etc. can be cited. In addition, as copolyester, copolyester with ethylene terephthalate as the main body of repeating unit can be cited. Specifically, copolymer polyester (hereinafter referred to as copolyester (terephthalate / isophthalate)) formed by polymerizing ethylene terephthalate as the main body of repeating unit with ethylene isophthalate, copolyester (terephthalate / adipate), copolyester (terephthalate / sodium isophthalate), copolyester (terephthalate / phenyl-dicarboxylate), copolyester (terephthalate / decane dicarboxylate), etc. These polyesters can be used alone or in combination of two or more.
[0148] In addition, specific examples of polyamides include aliphatic polyamides such as nylon 6, nylon 66, nylon 610, nylon 12, nylon 46, and copolymers of nylon 6 and nylon 66; aromatic polyamides such as hexamethylenediamine-isophthalic acid-terephthalic acid copolymer polyamides such as nylon 6I, nylon 6T, nylon 6IT, and nylon 6I6T (I represents isophthalic acid, and t represents terephthalic acid) containing structural units derived from terephthalic acid and / or isophthalic acid, and polyamide MXD6 (polyamide PACM6 (polybis(4-aminocyclohexyl)methaneazideamide). These polyamides may be used alone or in combination of two or more.
[0149] The outer substrate resin layer 16 preferably contains at least one of a polyester film, a polyamide film and a polyolefin film; preferably contains at least one of a stretched polyester film, a stretched polyamide film and a stretched polyolefin film; further preferably contains at least one of a stretched polyethylene terephthalate film, a stretched polybutylene terephthalate film, a stretched nylon film and a stretched polypropylene film; further preferably contains at least one of a biaxially stretched polyethylene terephthalate film, a biaxially stretched polybutylene terephthalate film, a biaxially stretched nylon film and a biaxially stretched polypropylene film.
[0150] The outer base resin layer 16 may be a single layer or may be composed of two or more layers. When the outer base resin layer 16 is composed of two or more layers, the outer base resin layer 16 may be a composite film formed by the action of an adhesive, or may be a resin composite film formed by co-extruding resins to form two or more layers. In addition, the outer base resin layer 16 may be a resin composite film formed by co-extruding resins to form two or more layers in an unstretched state, or may be a resin composite film formed by uniaxial stretching or biaxial stretching.
[0151] In the outer substrate resin layer 16, as specific examples of a laminate of two or more layers of resin films, a composite film of a polyester film and a nylon film, a composite film of two or more layers of nylon, a composite film of two or more layers of polyester, etc. can be cited. Preferred are a laminate of a stretched nylon film and a stretched polyester film, a stretched nylon composite film of two or more layers, and a stretched polyester composite film of two or more layers. For example, when the outer substrate resin layer 16 is a two-layer resin composite film, a composite film of a polyester resin film and a polyester resin film, a composite film of a polyamide resin film and a polyamide resin film, or a composite film of a polyester resin film and a polyamide resin film is preferred, and a composite film of a polyethylene terephthalate film and a polyethylene terephthalate film, a composite film of a polybutylene terephthalate film and a polybutylene terephthalate film, a composite film of a nylon film and a nylon film, or a composite film of a polyethylene terephthalate film and a nylon film is more preferred. In addition, polyester resin is unlikely to change color when an electrolyte adheres to the surface. Therefore, when the outer base resin layer 16 is a resin composite film of two or more layers, the polyester resin film is preferably located at the outermost layer of the outer base resin layer 16 .
[0152] When the outer substrate resin layer 16 is a resin composite film of more than two layers, the two or more resin films can also be composited by an adhesive. As a preferred adhesive, a glue solution with the same composition as the outer layer adhesive can be used. In addition, as a method for composite two or more layers of resin films, there is no particular limitation, and dry composite method, sandwich composite method, extrusion composite method, thermal composite method, etc. can be used, preferably dry composite method. When composited by dry composite method, a reactive polyurethane adhesive is preferably used as the reactive adhesive of the outer layer. At this time, the thickness of the adhesive layer can be about 2 to 5 μm. When the outer substrate resin layer 16 is formed by a resin coating method, the resin can be first dissolved in an organic solvent, and the outer substrate resin layer 16 can be formed by coating. The coating resin can use polyamide resin, polyimide resin, polyurethane resin, epoxy resin, acrylic resin, polyester resin, polyamide resin, polyimide resin, fluorine copolymer resin, polyester resin and other phenolic resins, polyester resin, polycarbonate resin, urea resin and melamine resin and other amino resins.
[0153] Furthermore, one or more additives such as lubricants, flame retardants, anti-blocking agents, antioxidants, light stabilizers, tackifiers, and antistatic agents may be added to the surface and interior of the outer base resin layer 16 .
[0154] From the viewpoint of improving the formability of the packaging material for lithium ion batteries, it is preferred to form a layer composed of a lubricant on the surface of the outer substrate resin layer 16. As a lubricant, there is no particular restriction, and an amide-based lubricant is preferred. Amide lubricants include saturated fatty acid amides, unsaturated fatty acid amides, substituted amides, hydroxymethylamides, saturated fatty acid bisamides, unsaturated fatty acid bisamides, fatty acid amides and aromatic bisamides, etc. Taking saturated fatty acid amides as an example, lauric acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, hydroxystearic acid amide, etc. can be used. Taking unsaturated fatty acid amides as an example, oleic acid amide, erucic acid amide, etc. can be cited. Substituted amides include N-oleopalmitic acid amide, N-stearic acid amide, N-stearic acid amide, N-oleostearic acid amide and N-stearic acid amide. In addition, hydroxymethylamide includes hydroxymethylstearic acid amide, etc. Saturated fatty acid bisamides include methylene bis stearic acid amide, ethylene bis caprylic acid amide, ethylene bis lauric acid amide, ethylene bis stearic acid amide, ethylene bis hydroxy stearic acid amide, ethylene bis behenic acid amide and hexamethylene bis stearic acid hexamethylene bis behenic acid amide, hexamethylene hydroxy stearic acid amide, n, n , - Distearyl adipamide, n, n , - Distearyl sebacic acid amide, etc. Unsaturated fatty acid bisamides include ethylene bisoleic acid amide, ethylene biserucic acid amide, hexamethylene bisoleic acid amide, n, n , -Dioleyl adipamide and n, n ,-Dioleyl sebacic acid amide. Fatty acid ester amides include stearylamide ethyl stearate, etc. In addition, aromatic bisamides include m-xylyl diisocyanate bis-stearic acid amide, m-xylyl diisocyanate bis-hydroxy stearic acid amide, n, n , - Distearyl isophthalic acid amide, etc. The lubricant may be used alone or in combination of two or more.
[0155] When a lubricant is present on the surface of the outer base resin layer 16, the amount of lubricant applied is not particularly limited, but is preferably about 3 mg / m 2 More preferably, 4 to 30 mg / m 2 about.
[0156] The lubricant present on the surface of the outer base resin layer 16 may be the lubricant seeping out of the base resin layer containing the lubricant, or the lubricant may be applied on the surface of the outer base resin layer 16 .
[0157] The thickness of the outer base resin layer 16 is not particularly limited as long as it functions as a base. When the outer base resin layer 16 is a composite resin film of two or more layers, the thickness of each resin film constituting the layer is preferably about 2 to 30 μm.
[0158] In the present application, the outer substrate resin layer 16 can be a single layer or a composite film of more than two layers formed by one or more materials of polymer materials such as blown film nylon, synchronous or asynchronous biaxially stretched nylon, synchronous or asynchronous biaxially stretched polyethylene terephthalate (PET), synchronous or asynchronous biaxially stretched polybutylene terephthalate (PBT), polyimide (PI), etc. The outer substrate resin layer 16 can be bonded to the intermediate metal layer 13 by one or a combination of extrusion, coating, compounding and thermal bonding. The total thickness of the outer substrate resin layer 16 is 5 to 35 μm. When the thickness is less than 5 μm, the formability and insulation are relatively poor. In addition, if it exceeds 35 μm, the total thickness of the metal composite film 1000 is too thick, and the advantage of the metal composite film 1000, that is, the softness, will deteriorate.
[0159] [Colorant layer 17]
[0160] The colored layer 17 is provided between the outer base resin layer 16 and the second adhesive layer 15 as required, or the colored layer 17 is provided on the side of the outer base resin layer 16 away from the intermediate metal layer 13, so that the appearance of the metal composite film 1000 is a layer of a preset color.
[0161] The coloring layer 17 contains a colorant, and the colorant may be a pigment, a dye, or the like. The colorant may be used alone or in combination of two or more.
[0162] The average particle size of the pigment is not particularly limited, and can be selected to be about 0.05-5 μm, preferably about 0.08-2 μm. The average particle size of the pigment is the median particle size measured by a laser diffraction / scattering particle size distribution measuring device.
[0163] As a specific example of the colorant contained in the colored layer 17 , the example of the second adhesive layer 15 can be referred to.
[0164]
Metal Composite Film 1000 Composite Process
[0165] 1. Degreasing treatment of the intermediate metal layer 13:
[0166] The surface wettability of the intermediate metal layer 13 is 65 dyn / cm, preferably 70 dyn / cm or more, or the contact angle of distilled water is 15 degrees or less, preferably 10 degrees or less. If the wettability of the intermediate metal layer 13 or the surface water contact angle exceeds the given range, it means that the rolling oil in the manufacturing stage may still remain on the metal, so the adhesion of the interface formed between the first anti-corrosion layer 12, the intermediate metal layer 13 and the heat-welding resin layer 10 becomes poor. During the long-term storage of the battery, there is a risk of the intermediate metal layer 13 and the heat-welding resin layer 10 falling off, and the battery is prone to leakage. As a preventive measure, an annealing treatment of more than 150°C can be performed, and degreasing can also be performed by plasma, corona method, or alkali solution. The alkali degreasing method is to immerse the metal in an alkali solution at 50-65°C, and after a certain period of treatment, wash it twice with deionized water, and then dry it to obtain a deoiled metal.
[0167] 2. Formation of the first / second anti-corrosion layer 14 on the intermediate metal layer 13:
[0168] After the anti-corrosion liquid is coated on the surface of the intermediate metal layer 13, it is heat treated at a high temperature for a period of time to form the first / second anti-corrosion layer 14.
[0169] 3. Formation and compounding of the second adhesive layer 15:
[0170] A polyurethane adhesive dissolved in an organic solvent is applied between the intermediate metal layer 13 and the outer base resin layer 16, and heated at a certain temperature for a certain time to volatilize the organic solvent to form a second adhesive layer 15. The outer base resin layer 16, the second adhesive layer 15, and the intermediate metal layer 13 are further compounded at a certain temperature and pressure, and after being stored at a certain temperature for a certain time, the second adhesive layer 15 is cured to obtain a composite resin layer composed of the outer base resin layer 16, the second adhesive layer 15, and the intermediate metal layer 13. When the outer base resin layer 16 and the intermediate metal layer 13 are compounded without using the second adhesive, the intermediate metal layer 13 and the outer base resin layer 16 are compounded by heating and pressurizing, and the outer base resin layer 16 is subjected to heating treatment, ultraviolet treatment, and electron beam treatment to make it film-like, so as to obtain a composite resin layer composed of the outer base resin layer 16 and the intermediate metal layer 13.
[0171] 4. Composite of the heat-melting resin layer 10: The composite film composed of the outer base resin layer 16 and the intermediate metal layer 13 can be appropriately selected and composited with the heat-melting resin layer 10 in different composite methods, as shown below:
[0172] a. Dry composite method: A solution-type first adhesive layer composed of a main agent, a curing agent and an organic solvent is applied to the anti-corrosion surface of the intermediate metal layer 13 of the composite film composed of the outer substrate resin layer 16 and the intermediate metal layer 13, and the solution-type first adhesive is dried to form the first adhesive layer 11, and is thermally composited with the bonding surface of the hot-melt resin layer 10 at a certain temperature and pressure, and then subjected to a aging treatment to form a composite product of the outer substrate resin layer 16 / intermediate metal layer 13 / first adhesive layer 11 / hot-melt resin layer 10. Preferably, the bonding surface of the hot-melt resin layer 10 in contact with the first adhesive layer 11 is pre-corona treated. In addition, an aging treatment not exceeding 60°C of the melting point temperature of the first adhesive layer 11 may be performed;
[0173] b. Melt extrusion method: The hot melt type first adhesive layer resin is melt extruded to form a hot melt type first adhesive layer 11 of a certain thickness on the anti-corrosion surface of the intermediate metal layer 13. In addition, the surface of the first adhesive layer 11 and the bonding surface of the hot melt resin layer 10 are thermally composited to form a composite product of the outer base resin layer 16 / intermediate metal layer 13 / first adhesive layer 11 / hot melt resin layer 10. In order to improve the peeling force between the intermediate metal layer 13 and the hot melt resin layer 10, a heat treatment of not more than 60°C of the melting point temperature of the first adhesive layer 11 can be performed;
[0174] c. Melt extrusion method: The hot melt type first adhesive layer 11 and the hot melt resin layer 10 are co-extruded to form a composite product of the outer base resin layer 16 / intermediate metal layer 13 / first adhesive layer 11 / hot melt resin layer 10. After the surface of the intermediate metal layer 13 in contact with the first adhesive layer 11 is subjected to anti-corrosion treatment, in order to improve the peeling force between the intermediate metal layer 13 and the hot melt resin layer 10, a heat treatment of not more than 60°C of the melting point of the first adhesive layer 11 can be performed;
[0175] d. Thermal bonding method: Dissolve a resin main agent and a curing agent with a melting point above 100°C in an aqueous or organic solvent to form an aqueous solution type first adhesive. Apply it to the anti-corrosion treated surface of the metal layer of the composite layer composed of the outer substrate resin layer 16 and the intermediate metal layer 13, and dry the solution type first adhesive to form the first adhesive layer 11. Under a certain temperature and pressure, thermally composite with the bonding surface of the hot melt resin layer 10 to form a composite product of the outer substrate resin layer 16 / intermediate metal layer 13 / first adhesive layer 11 / hot melt resin layer 10. In order to improve the peeling force between the intermediate metal layer 13 and the hot melt resin layer 10, a heat treatment of not more than 60°C of the melting point of the first adhesive layer 11 can be performed. The hot melt resin layer 10 can also be formed by extrusion, or a film can be used. When a film is used, it is preferred that the bonding surface of the hot melt resin layer 10 in contact with the first adhesive layer 11 is pre-corona treated.
[0176] The present application also provides an electrochemical device, which uses the above-mentioned metal composite film.
[0177] Electrochemical devices include but are not limited to batteries, and batteries include but are not limited to lithium ion batteries, sodium ion batteries, etc. That is, the above-mentioned metal composite film can be used as a battery outer packaging material in electrochemical devices.
[0178] The present application will be described in detail below through examples.
[0179] 1. Parameter determination
[0180] (1) Water contact angle measurement
[0181] The water contact angle of the surface of the metal intermediate layer was measured using a German KRUSSDSA25 contact angle meter. The metal intermediate layer was placed flat on the instrument workbench, the water output of the syringe was controlled at 2 μml each time, and the liquid addition speed was 2.67 μmL / s. The contact angle value of the water drop just dripping onto the surface of the metal intermediate layer was recorded.
[0182] (2) Determination of dyne value
[0183] Use the German Arcotest dyne pen to draw two 10cm long straight lines on the surface of the metal intermediate layer. If the straight line shrinks by more than 10% within 3 seconds, it means that the surface dyne value of the metal intermediate layer does not reach the dyne value of the dyne pen at this time. Select a dyne pen with a lower dyne value for re-measurement.
[0184] (3) Determination of elements in the anti-corrosion layer
[0185] XPS (AXIS supra, Shimadzu, UK) was used to determine the element distribution of the first / second anti-corrosion layer depth on the metal intermediate layer surface by the ESCA method. The metal surface of the sample was sputtered by Ar ions, with an ion beam diameter of 800 μm, a voltage of 15 KV, an ion beam sputtering depth of 5 nm, a sputtering rate of 3 nm / min, 7 sputtering times, a signal source detection depth of 5 nm, a detection limit of 1‰, and 8 detection times.
[0186] 2. The peel strength test between the intermediate metal layer and the heat-welded resin layer of the finished metal composite film is as follows.
[0187] (1) Initial peel strength test
[0188] The finished metal composite film is prepared into a straight strip with a strip size of 100*15mm. The peeling test between the intermediate metal layer and the hot-melt resin layer is performed using a tensile test device. The peeled hot-melt resin layer film is placed in the upper clamping plate of the telescopic test device, and the intermediate metal layer is placed in the lower clamping plate. Then, at a telescopic speed of 50mm / min, a T-shaped peeling with a peeling surface of 180° is performed to start measuring the peel strength between the intermediate metal layer and the hot-melt resin layer. The peel strength is read in the manner that the moving distance of the hot-melt resin layer and the intermediate metal layer is 50mm, and the average value of the peel strength between the moving distance of 10mm and 40mm is selected. 5 pieces / group are tested in parallel.
[0189] (2) Anhydrous electrolyte resistance test of finished metal composite membranes
[0190] The finished metal composite film specimens were directly immersed in a mixed solvent of dimethyl carbonate (DMC): diethyl carbonate (DEC): ethylene carbonate (EC) with a molar ratio of 1:1:1 containing 1 mol / L LiPF6. After immersion at 85°C for 7 days, they were taken out and washed with water for 15 minutes. The moisture on the surface of the specimens was wiped dry, and the peel strength between the intermediate metal layer and the hot-melt resin layer was measured according to the initial peel strength test method.
[0191] (3) Aqueous electrolyte resistance test of finished metal composite membranes
[0192] After the intermediate metal layer and the heat-melting resin composite layer of the finished metal composite film sample are peeled off by 20mm, they are immersed in a mixed solution of dimethyl carbonate (DMC): diethyl carbonate (DEC): ethylene carbonate (EC) with a molar ratio of 1:1:1 containing 1mol / L LiPF6, and then 1000PPM of water accounting for the total mass of the electrolyte is added to the mixed solvent. After soaking at a temperature of 85℃ for 7 days, take it out, wash it with water for 15min, and do not wipe off the water. The peel strength between the intermediate metal layer and the heat-melting resin layer is measured according to the initial peel strength test method. This test method is to peel it off in the state where there is residual water between the metal layer and the heat-melting resin layer, and measure the peel strength between the intermediate metal layer and the heat-melting resin layer from the pre-peeled part.
[0193] Examples 1-12 and Comparative Examples 1-2
[0194] like Figure 3 As shown, the metal composite film 1000 provided in Examples 1-12 and Comparative Examples 1-2 is composed of an outer substrate resin layer 16 / a second adhesive layer 15 / a second anti-corrosion layer 14 / an intermediate metal layer 13 / a first anti-corrosion layer 12 / a first adhesive layer 11 / a hot melt resin layer 10.
[0195] The stacking method is as follows:
[0196] (1) Obtaining an intermediate metal layer 13, wherein the difference between the intermediate metal layer 13 in Examples 1-12 and Comparative Examples 1-2 is shown in Table 1:
[0197] The intermediate metal layer 13 of Examples 1-12 and Comparative Examples 1-2 is a nickel-plated stainless steel plate with a total thickness of 45 μm, and the specific differences are as follows:
[0198] In Example 1, the surface dyne value of the intermediate metal layer 13 is 68 dyn / cm, and the thickness of the nickel plating layer on one side is 2 μm.
[0199] In Example 2, the water contact angle of the intermediate metal layer 13 is 10°, and the thickness of the nickel plating layer on one side is 2 μm.
[0200] The surface dyne value of the intermediate metal layer 13 in Examples 3, 11 and Comparative Example 2 was 75 dyn / cm, and the thickness of the nickel plating layer on one side was 2 μm.
[0201] In Examples 4 and 12, the water contact angle of the intermediate metal layer 13 is 15°, and the thickness of the nickel plating layer on one side is 2 μm.
[0202] In Example 5, the water contact angle of the intermediate metal layer 13 is 20°, and the thickness of the nickel plating layer on one side is 12 μm.
[0203] In Example 6, the water contact angle of the intermediate metal layer 13 is 17°, and the thickness of the nickel plating layer on one side is 20 μm.
[0204] The water contact angle of the intermediate metal layer 13 in Examples 7, 8 and Comparative Example 1 was 2°, and the thickness of the nickel plating layer on one side was 15 μm.
[0205] The surface dyne value of the intermediate metal layer 13 of Examples 9-10 was 75 dyn / cm, and the thickness of the nickel plating layer on one side was 0.2 μm.
[0206] (2) Both surfaces of the intermediate metal layer 13 are subjected to anti-corrosion treatment using an anti-corrosion liquid in advance, that is, the first anti-corrosion layer 12 and the second anti-corrosion layer 14 are formed on both surfaces of the intermediate metal foil, respectively.
[0207] Among them, in Example 1, the anti-corrosion liquid includes, by mass percentage: 0.1% polyacrylamide, 1.1% phosphonocarboxylic acid copolymer, 1.2% hydroxy acrylic resin, 1.9% oxazoline compound, 2.0% chromium fluoride, 0.3% hydrofluoric acid, 1.2% polyvinyl alcohol resin, 0.4% zirconium fluoride, and 91.8% solvent, wherein the solvent is a mixture of water and ethylene glycol butyl ether in a ratio of 97:3.
[0208] In Example 2, the anti-corrosion liquid includes, by mass percentage: 0.2% polyacrylamide, 0.9% phosphonocarboxylic acid copolymer, 0.8% hydroxy acrylic resin, 2.1% oxazoline compound, 3.5% chromium nitrate, 5% phosphoric acid, 2.5% acrylic resin, and 85% solvent, wherein the solvent is a mixture of water and ethylene glycol butyl ether in a ratio of 97:3.
[0209] In Example 3, the anti-corrosion liquid includes, by mass percentage: 0.5% polyacrylamide, 0.2% phosphonocarboxylic acid copolymer, 0.3% hydroxy acrylic resin, 0.9% oxazoline compound, 3.5% chromium nitrate, 5% phosphoric acid, 2.5% acrylic resin, and 87.1% solvent, wherein the solvent is a mixture of water and ethylene glycol butyl ether in a ratio of 97:3.
[0210] In Example 4, the anti-corrosion liquid includes, by mass percentage, 0.6% polyacrylamide, 0.3% phosphonocarboxylic acid copolymer, 0.4% hydroxy acrylic resin, 1.3% oxazoline compound, 2.0% chromium fluoride, 0.3% hydrofluoric acid, 1.2% polyvinyl alcohol resin, 0.4% zirconium fluoride, and 93.5% solvent, wherein the solvent is a mixture of water and ethylene glycol butyl ether in a ratio of 97:3.
[0211] In Example 5, the anti-corrosion liquid includes, by mass percentage: 1.2% polyacrylamide, 1.3% phosphonocarboxylic acid copolymer, 0.6% hydroxy acrylic resin, 2.4% oxazoline compound, 2.0% chromium fluoride, 0.3% hydrofluoric acid, 1.2% polyvinyl alcohol resin, 0.4% zirconium fluoride, and 90.6% solvent, wherein the solvent is a mixture of water and ethylene glycol butyl ether in a ratio of 97:3.
[0212] In Example 6, the anti-corrosion liquid includes, by mass percentage: 1.4% polyacrylamide, 1.4% phosphonocarboxylic acid copolymer, 0.8% hydroxy acrylic resin, 2.8% oxazoline compound, 2.0% chromium fluoride, 0.3% hydrofluoric acid, 1.2% polyvinyl alcohol resin, 0.4% zirconium fluoride, and 89.7% solvent, wherein the solvent is a mixture of water and ethylene glycol butyl ether in a ratio of 97:3.
[0213] In Example 7, the anti-corrosion liquid includes, by mass percentage: 2.5% polyacrylamide, 1.6% phosphonocarboxylic acid copolymer, 1.4% hydroxy acrylic resin, 3.8% oxazoline compound, 2.0% chromium fluoride, 0.3% hydrofluoric acid, 1.2% polyvinyl alcohol resin, 0.4% zirconium fluoride, and 86.8% solvent, wherein the solvent is a mixture of water and ethylene glycol butyl ether in a ratio of 97:3.
[0214] In Example 8, the anti-corrosion liquid includes, by mass percentage: 3% polyacrylamide, 2% phosphonocarboxylic acid copolymer, 2% hydroxy acrylic resin, 4.9% oxazoline compound, 2.5% chromium nitrate, 4% phosphoric acid, 2.5% acrylic resin, and 79.1% solvent, wherein the solvent is a mixture of water and ethylene glycol butyl ether in a ratio of 97:3.
[0215] In Example 9, the anti-corrosion liquid includes, by mass percentage: 2.2% polyacrylamide, 1% phosphonocarboxylic acid copolymer, 1.6% hydroxy acrylic resin, 2.6% oxazoline compound, 6% chromium fluoride, 0.3% hydrofluoric acid, 1.5% polyvinyl alcohol resin, and 84.8% solvent, wherein the solvent is a mixture of water and ethylene glycol butyl ether in a ratio of 97:3.
[0216] In Example 10, the anti-corrosion liquid includes, by mass percentage: 2.7% polyacrylamide, 0.5% hydroxy acrylic resin, 2.3% oxazoline compound, 6% chromium nitrate, 0.3% phosphoric acid, 1.5% acrylic resin, and 86.7% solvent, wherein the solvent is a mixture of water and ethylene glycol butyl ether in a ratio of 97:3.
[0217] In Example 11, the anti-corrosion liquid includes, by mass percentage, 0.8% polyacrylamide, 1.8% phosphonocarboxylic acid copolymer, 3.7% oxazoline compound, 1.9% chromium nitrate, 4% phosphoric acid, 2.5% acrylic resin, and 85.3% solvent, wherein the solvent is a mixture of water and ethylene glycol butyl ether in a ratio of 97:3.
[0218] In Example 12, the anti-corrosion liquid includes, by mass percentage, 1.9% polyacrylamide, 0.7% phosphonocarboxylic acid copolymer, 1.1% hydroxy acrylic resin, 6% chromium fluoride, 0.3% hydrofluoric acid, 1.5% polyvinyl alcohol resin, and 88.5% solvent, wherein the solvent is a mixture of water and ethylene glycol butyl ether in a ratio of 97:3.
[0219] In Comparative Example 1, the anti-corrosion liquid includes, by mass percentage: 1.2% of phosphonocarboxylic acid copolymer, 0.9% of hydroxy acrylic resin, 3% of oxazoline compound, 6% of chromium nitrate, 0.3% of phosphoric acid, 1.5% of acrylic resin, and 87.1% of solvent, wherein the solvent is a mixture of water and ethylene glycol butyl ether in a ratio of 97:3.
[0220] In comparative example 2, the anticorrosion liquid includes, by mass percentage: 4.2% polyacrylamide, 1.1% phosphonocarboxylic acid copolymer, 0.7% hydroxy acrylic resin, 3.2% oxazoline compound, 2.0% chromium fluoride, 4% hydrofluoric acid, 2.5% polyvinyl alcohol resin, and 82.3% solvent, wherein the solvent is a mixture of water and ethylene glycol butyl ether in a ratio of 97:3. The main differences between the anticorrosion agents used in Examples 1-12 and Comparative Examples 1-2 are shown in Table 1. The anticorrosion liquid used in Examples 1-9 and Comparative Examples 1-2 is evenly coated on both sides of the intermediate metal by a coating roller, and the coating wet film amount of the anticorrosion layer treatment liquid is 5g / m 2 , and then heat-baked at 190° C. for 2 minutes to form a first anti-corrosion layer and a second anti-corrosion layer 14.
[0221] The anti-corrosion liquid used in Examples 10-12 is evenly coated on both sides of the intermediate metal by a coating roller, and the coating wet film amount of the anti-corrosion layer treatment liquid is 5g / m 2 , and then heat-baked at 100° C. for 2 minutes to form a first anti-corrosion layer and a second anti-corrosion layer 14.
[0222] (3) The outer base resin layer 16 film in contact with the second adhesive layer 15 is subjected to a corona treatment.
[0223] A non-crystalline polyester polyol with a weight average molecular weight of 5000, a Tg of 50°C and a hydroxyl value of 25 mg KOH / g is mixed with a non-crystalline polyester polyol with a weight average molecular weight of 20000, a Tg of -17°C and a hydroxyl value of 8 mg KOH / g in a weight ratio of 3:2, and toluene diisocyanate (TDI) is added to form a second adhesive liquid with an NCO / OH ratio of 6.2. The second adhesive liquid is applied on the second anti-corrosion layer 14 to form a 3 μm second adhesive layer. The intermediate metal foil is thermally compounded with the second adhesive layer 15 and the outer substrate resin layer 16 film, and then aged at 80°C for 3 days to form a semi-finished product of outer substrate resin layer 16 / second adhesive layer 15 (3 μm) / second anti-corrosion layer 14 / intermediate metal layer 13.
[0224] (4) Compounding the first adhesive layer 11 and the hot-melt resin layer 10 on the surface of the first anti-corrosion layer 12 of the semi-finished product. The first adhesive layer 11 includes a hot-melt first adhesive layer B-1 and a solution-type first adhesive layer B-2, and the compounding methods of the two are as follows:
[0225] A. Hot-melt first adhesive layer B-1 composite method: The hot-melt resin used in the first adhesive layer 11 is anhydrous maleic anhydride modified polypropylene. On the surface of the first anticorrosion layer 12 of the intermediate metal layer 13 in contact with the hot-melt resin layer 10, a first adhesive layer with a thickness of 15 μm is formed, and further, it is composited with a hot-melt resin with a thickness of 30 μm. The first adhesive layer 11 and the hot-melt resin layer 10 are composited to the first anticorrosion layer in contact with the hot-melt resin layer 10 by melt co-extrusion. The first adhesive layer 11 used is 60% (by weight) of anhydrous maleic anhydride modified random copolymer polypropylene with a melting point of 140°C and an MFR (230°C) of 5g / 10min. The modification degree of anhydrous maleic anhydride on random copolymer polypropylene is 10%, the melting point is 160°C, the MFR (230°C) is 2.6g / 10min, and the density is 0.87g / cm 3 24% (by weight) of copolymer elastomer of propylene and butene, melting point 130°C, MFR (230°C) 9.5g / 10min, density 0.91g / cm 3 A mixture of 8% (by weight) of a crystalline copolymer elastomer of ethylene and propylene and 8% (by weight) of a low-density polyethylene having a melting point of 105°C and an MFR (230°C) of 12 g / 10min.
[0226] The heat-welding resin layer 10 consists of two layers, and its structure is as follows:
[0227] The resin layer A in contact with the first adhesive layer 11 is a mixture layer of 62% by weight of random copolymer polypropylene with a melting point of 155°C and an MFR (230°C) of 4 g / 10 min, 33% of a non-crystalline propylene elastomer and 5% of a low-density polyethylene with a melting point of 110°C and an MFR (230°C) of 7.5 g / 10 min;
[0228] Innermost resin layer B (resin layer on the side away from the first adhesive layer 11): a layer composed of random copolymer polypropylene with a melting point of 155°C and an MFR (230°C) of 15 g / 10 min;
[0229] The thickness ratio of the resin layer A in contact with the first adhesive layer 11 to the innermost resin layer B is 8:2.
[0230] After the intermediate metal layer 13 is compounded with the first adhesive layer 11 and the heat-melting resin layer 10, a heat treatment is performed at a temperature of 180°C for 2 seconds. In this way, a composite product of the outer base resin layer 16 / the second adhesive layer 15 (3 μm) / the second anti-corrosion layer 14 / the intermediate metal layer 13 / the first anti-corrosion layer 12 / the first adhesive layer 11 (15 μm) / the heat-melting resin layer 10 (30 μm) is formed.
[0231] B. Solution-type first adhesive layer B-2 composite method: a weight average molecular weight of 80,000, a melting point of 80°C, and an acid value of 2 mg A solution type mixture of KOH / g anhydrous maleic anhydride modified polypropylene solution and aromatic isocyanate (HDI series, hexamethylene diisocyanate) solution in a solid ratio of 20:1 is coated on the intermediate metal surface (that is, the surface of the first anti-corrosion layer 12) of the composite film that has been composited with the outer substrate resin layer 16 and has been subjected to anti-corrosion treatment and is in contact with the hot melt resin layer 10. After drying, a first adhesive layer B-2 with a thickness of 4 μm is formed, and then it is thermally composited with the bonding surface of 25 μm hot melt resin at a temperature of 80°C, and then aged at a temperature of 60°C for 7 days to form a composite product of outer substrate resin layer 16 / second adhesive layer 15 (3 μm) / second anti-corrosion layer 14 / intermediate metal layer 13 / first anti-corrosion layer 12 / first adhesive layer 11-2 (4 μm) / hot melt resin layer 10 (25 μm). The adhesive surface of the three-layer heat-welding resin layer 10 in contact with the first adhesive layer 11 - 2 is previously subjected to corona treatment.
[0232] The three-layer structure of the hot-melt resin is:
[0233] The resin layer in contact with the first adhesive layer 11: a layer composed of random copolymer polypropylene with a melting point of 145°C and an MFR (230°C) of 7.5 g / 10 min;
[0234] Middle resin layer: by weight, 40% of block copolymer polypropylene with a melting point of 162°C and an MFR (230°C) of 2g / 10min, 40% of block copolymer polypropylene with a melting point of 160°C and an MFR (230°C) of 5g / 10min, and 20% of a melting point of 130°C, an MFR (230°C) of 9.5g / 10min, and a density of 0.91g / cm 3 A mixture layer formed of a crystalline polymer elastomer composed of ethylene and propylene;
[0235] Innermost resin layer: a layer composed of random copolymer polypropylene with a melting point of 145°C and an MFR (230°C) of 7.5 g / 10 min;
[0236] In the heat-welding resin layer 10 , the thickness ratio of the three layers of resin from the layer in contact with the first adhesive layer 11 to the innermost layer is 1:8:1.
[0237] The compounding methods corresponding to the embodiments and comparative examples are shown in Table 1.
[0238] The peel strength test of the metal composite film product prepared above was carried out, and the results are shown in Table 1.
[0239] Table 1 Distinguishing parameters and test results of Examples 1-8
[0240]
[0241]
[0242] Table 2 Parameters and test results of Examples 9-12 and Comparative Examples 1-2
[0243]
[0244] It should be noted that in Table 1 and Table 2, the maintenance rate refers to the ratio of the peel strength between the intermediate metal layer and the heat-welding resin layer measured with or without water-resistant electrolyte to the initial peel strength. CAS number of hydroxy acrylic resin: 37956-57-3.
[0245] It can be seen from Tables 1 and 2 that the maintenance rates of the metal composite films provided in the present application in the anhydrous electrolyte resistance test are greater than those of comparative examples 1-2. At the same time, in the aqueous electrolyte resistance test, examples 1-12 are greater than comparative example 1, and examples 1-9 and 11-12 are greater than comparative example 2, indicating that the metal composite films provided in the present application have excellent peel strength and excellent maintenance rate, and are long-lasting.
[0246] In Examples 1-8, the initial peel strength of the metal composite film is above 10.0 N / 15 mm, and the peel strength maintenance rates after being placed in anhydrous and aqueous electrolyte environments for 14 days are above 80% and 60%, respectively.
[0247] The number of carbon atoms (C) between the carboxyl groups on the carbon chain of the carboxylic acid copolymer in the anticorrosive solution of Example 9 is 7. As a result, the initial peel strength between the intermediate metal layer and the heat-welding resin layer in Example 9 is 14.6N / 15mm, and the maintenance rate of the electrolyte resistance test is 67% without adding water and 48% with adding water, which are lower than those of Examples 1-8. Although the initial bonding force is fully exerted, the number of carbon atoms (C) between the carboxyl groups in the anticorrosive solution is 7, and the ability to passivate nitrogen atoms (N) is low, resulting in a low maintenance rate and poor long-term effectiveness.
[0248] The content of the phosphonocarboxylic acid copolymer in the anticorrosion liquid forming the anticorrosion layer in Example 10 is 0%. As a result, the initial peel strength between the intermediate metal layer and the heat-welding resin layer in Example 10 is 14N / 15mm, and the maintenance rate of the electrolyte resistance test is: 91% under the condition of no water addition and 45% under the condition of water addition, which are lower values compared with Examples 1-8. Although the maintenance rate is higher under the condition of no water addition, since the phosphonocarboxylic acid copolymer is not added to the anticorrosion liquid, the amino group fails in the long term, and the maintenance rate is low under the condition of water addition.
[0249] No hydroxy acrylic resin was added to the anticorrosion liquid forming the anticorrosion layer in Example 11. As a result, the initial peel strength between the intermediate metal layer and the heat-welded resin layer in Example 11 was 14.3N / 15mm, and the maintenance rate of the electrolyte resistance test was 88% without adding water and 54% with adding water, both of which were lower than those of Examples 1-8.
[0250] No crosslinking agent was added to the anticorrosion liquid forming the anticorrosion layer in Example 12. As a result, the initial peel strength between the intermediate metal layer and the heat-melting resin layer in Example 13 was 13.7N / 15mm, and the maintenance rate of the electrolyte resistance test was 75% under the condition of no water addition and 48% under the condition of water addition. Although the initial bonding force was fully exerted, due to the absence of a crosslinking agent, the first anticorrosion layer and the first adhesive layer could not be crosslinked and cured, and could not resist the corrosion of hydrogen fluoride, so the long-term effect was poor, and compared with Examples 1-8, they all showed low values.
[0251] The anti-corrosion liquid used in Comparative Example 1 does not contain any nitrogen-containing polymer. Therefore, the nitrogen atom (N) content is 1.0% 100 nm from the surface of the first anti-corrosion layer to the inside. At this time, the first anti-corrosion liquid cannot react with the first adhesive layer, resulting in the metal composite film of Comparative Example 1 having an initial peel strength of 14.4 N / 15 mm. The maintenance rate of the electrolyte resistance test is 58% without adding water and 33% with adding water, which are both low values compared with Examples 1-12.
[0252] The mass content of nitrogen-containing polymer in the anticorrosion liquid used in Comparative Example 2 is 4.2%, resulting in a nitrogen atom (N) content of 31% at 100nm from the surface of the first anticorrosion layer to the inside. At this time, the degree of reaction and curing between the anticorrosion layer and the first adhesive layer is too high, causing the bonding layer to become brittle and prone to cracks. At this time, although the initial strength is as high as 15.3N / 15mm, the maintenance rate of the electrolyte resistance test is only 61% without adding water and 47% under the condition of adding water, which shows low values compared with Examples 1-9 and 11-12, but is better than Comparative Example 1. Among them, it can also be seen from Example 10 and Comparative Example 2 that the phosphonocarboxylic acid copolymer is beneficial to improving the retention rate of the peel strength between the intermediate metal layer and the thermally welded resin layer in the aqueous electrolyte resistance test.
[0253] It can be seen from Examples 1-12 that the addition of nitrogen-containing polymers to the antiseptic liquid makes it compatible not only with the hot-melt first adhesive layer B-1, but also with the solution-type first adhesive layer B-2, thereby reducing the preparation cost of the metal composite film and improving the preparation efficiency.
[0254] In summary, the metal composite film provided by the present application adds nitrogen-containing polymers to the anti-corrosion liquid and controls the content of nitrogen atoms in the first anti-corrosion layer. This is not only beneficial to improving the initial peel strength between the intermediate metal layer and the hot-melt resin layer of the obtained metal composite film, making it have better long-term effectiveness, but also can be adapted to different types of first adhesive layers, thereby reducing the preparation cost of the metal composite film and improving the preparation efficiency, which is beneficial to promoting the promotion and use of metal composite films in the field of lithium-ion batteries.
[0255] The above are only specific embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A metal composite film, It is characterized in that It includes a heat-melting resin layer, a first adhesive layer, a first anti-corrosion layer, an intermediate metal layer and an outer base material resin layer which are sequentially stacked; Wherein, the first adhesive layer includes acid-modified groups and / or isocyanate groups, the first anti-corrosion layer includes a nitrogen-containing polymer, the nitrogen-containing polymer has an amino group that reacts with the acid-modified groups and / or the isocyanate groups, and the content of nitrogen atoms in the first anti-corrosion layer is greater than 0 and less than or equal to 20At%.
2. The metal composite film according to claim 1, It is characterized in that The content of nitrogen atoms in the first anti-corrosion layer is 1At%-20At%.
3. The metal composite film according to claim 1, It is characterized in that The first anti-corrosion layer is formed by coating and heat treating the anti-corrosion liquid; Wherein, the mass percentage of the nitrogen-containing polymer in the anti-corrosion liquid is 0.1%-3%.
4. The metal composite film according to claim 3, It is characterized in that The anti-corrosion liquid also includes at least one of a carboxylic acid-containing polymer, a hydroxylated acrylic resin and a cross-linking agent, wherein the mass percentage of the carboxylic acid-containing polymer in the anti-corrosion liquid is 0.1%-2.0%, the mass percentage of the hydroxylated acrylic resin in the anti-corrosion liquid is 0.1%-2.0%, and the mass percentage of the cross-linking agent in the anti-corrosion liquid is 0.5%-5%.
5. The metal composite film according to claim 4, It is characterized in that The carboxyl groups on the carbon chain of the carboxylic acid-containing polymer are spaced no more than 5 carbon atoms apart.
6. The metal composite film according to claim 4, It is characterized in that The carboxylic acid-containing polymer includes a phosphonocarboxylic acid copolymer.
7. The metal composite film according to claim 4, It is characterized in that The cross-linking agent includes at least one of an epoxy compound, an oxazoline compound, and adipic acid dihydrazide compound.
8. The metal composite film according to claim 3, It is characterized in that The anti-corrosion liquid further comprises a trivalent metal compound, an inorganic acid and an organic resin, wherein the trivalent metal compound is a trivalent chromium compound or a trivalent cerium compound, the mass percentage of the trivalent metal compound in the anti-corrosion liquid is 1.9%-6%, the mass percentage of the inorganic acid in the anti-corrosion liquid is 0.3%-6%, and the mass percentage of the organic resin in the anti-corrosion liquid is 0.6%-6%; The organic resin is composed of polyacrylic acid resin and / or polyvinyl alcohol, and the polyacrylic acid resin is one or more of polyacrylic acid, polymethyl acrylate, copolymer of acrylic acid and maleic acid, copolymer of acrylic acid and styrene, and sodium salt and ammonium salt derivatives thereof.
9. The metal composite film according to claim 3, It is characterized in that The anti-corrosion liquid comprises a titanium compound or a zirconium compound, wherein the mass percentage of the titanium compound in the anti-corrosion liquid is 0-0.6%, and the mass percentage of the zirconium compound in the anti-corrosion liquid is 0-2.8%.
10. The metal composite film according to any one of claims 1 to 9, It is characterized in that The first adhesive layer is made of a solvent-based adhesive, and the first adhesive layer contains an isocyanate group and / or an acid-modified group; or, The first adhesive layer is made of a hot-melt adhesive and contains an acid-modified group.
11. The metal composite film according to any one of claims 1 to 9, It is characterized in that The metal composite film further includes a second adhesive layer, and the second adhesive layer is located between the outer base resin layer and the intermediate metal layer.
12. The metal composite film according to claim 11, It is characterized in that The metal composite film further includes a second anti-corrosion layer, and the second anti-corrosion layer is located between the second adhesive layer and the intermediate metal layer.
13. The metal composite film according to claim 12, It is characterized in that The second anticorrosion layer includes a nitrogen-containing polymer having an amine group, and the second adhesive layer includes an acid-modified group and / or an isocyanate group that reacts with the amine group.
14. The metal composite film according to claim 11, It is characterized in that The metal composite film further includes a colored layer, and the colored layer is disposed between the outer base resin layer and the second adhesive layer, or the colored layer is disposed on a side of the outer base resin layer away from the intermediate metal layer.
15. The metal composite film according to claim 11, It is characterized in that The second adhesive layer contains a colorant.
16. The metal composite film according to any one of claims 1 to 9, It is characterized in that The thickness of the first anti-corrosion layer is 1 nm-3.0 μm.
17. The metal composite film according to any one of claims 1 to 9, It is characterized in that The intermediate metal layer is made of nickel-plated steel plate.
18. An electrochemical device, It is characterized in that Use the metal composite film as described in any one of claims 1 to 17.
Citation Information
Patent Citations
Soft package membrane for lithium battery
CN104485430A
Metal composite film and electrochemical device
CN112563632A
Exterior material for power storage device, method for manufacturing exterior material for power storage device, and power storage device
CN113329876A
Resin coated metal laminate, method for producing resin coated metal laminate, battery outer packaging material, and battery
CN113442542A
Metal composite film of outer packing material for lithium ion battery device