Degradable high-toughness high-barrier film

Through the double-layer film composite structure, combined with vacuum sputtering and silanization modification technology, the problem of degradable film materials between mechanical properties and gas barrier properties is solved, and a fully degraded, high-strength and high-barrier film material is achieved. Meets the needs of food and drug packaging and other fields.

CN118977485AActive Publication Date: 2024-11-19XIAN HUAQI ZHONGXIN TECH DEV CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411169711.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-25
Publication Date
2024-11-19
Estimated Expiration
2044-08-25

AI Technical Summary

Technical Problem

Existing degradable membrane materials are difficult to achieve good oxygen and carbon dioxide barrier properties while ensuring mechanical properties. In addition to traditional methods, nanoparticles or high-barrier polymers will deviate from the original intention of fully degradable, and lack the ability to meet both toughness and high gases. Barrier material.

Method used

Using a double-layer film composite structure, the bottom layer is P3H4B-PBAT film layer and the upper layer is a hydrophobic modified cellulose film layer. The silicon oxide layer is covered with vacuum sputtering and silanization modification treatment, combined with hot pressing technology, a high-strength full degradation is formed. Tough high barrier membrane.

Benefits of technology

It achieves good mechanical properties and gas barrier properties, while ensuring the full degradation of the material, improving the comprehensive performance and industrial prospects of the membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118977485A_ABST
    Figure CN118977485A_ABST
Patent Text Reader

Abstract

The invention relates to a degradable high-toughness high-barrier film which is formed by compounding two layers and comprises a P3H4B-PBAT film on the bottom layer and a hydrophobic modified cellulose film layer on the upper layer, wherein the upper surface of the P3H4B-PBAT film on the bottom layer is subjected to plasma treatment and then is covered with the silicon oxide film layer through vacuum sputtering; silanization modification is carried out on the lower surface of the hydrophobic modified cellulose membrane layer, and then the P3H4B-PBAT membrane subjected to surface modification and the hydrophobic modified cellulose membrane layer are compounded through hot pressing; the composite film has good mechanical properties, also has good oxygen and carbon dioxide barrier properties, and can be applied to the packaging fields of food, medicines and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a film, and in particular to a degradable film material with high strength and high gas barrier properties. Background Art

[0002] In packaging products, especially in the field of packaging films, plastic materials are still widely used, such as PE, PP, and PET films, which are still the mainstream of packaging films. The above petroleum-based plastic materials have excellent processability and good mechanical properties. Some materials, such as PET, also have excellent barrier properties. Despite the excellent performance, its non-degradability has also brought a series of environmental problems. Finding packaging materials with excellent performance and full degradability is still the direction of people's efforts.

[0003] In the field of food and drug packaging, the requirements for film materials are very high. For example, while ensuring mechanical properties, they must also have special functionality. For example, due to the requirement of shelf life, the film must have good oxygen barrier properties. For some packaging that directly contacts food, it is best to have certain antibacterial properties. However, it is very difficult to achieve the above characteristics while ensuring degradability. For example, film materials directly prepared from degradable materials often cannot achieve good barrier properties due to their structural characteristics. For example, polylactic acid films, polylactic acid / PBAT films, PVA films, etc., due to their own structural limitations, cannot achieve the required oxygen permeability and carbon dioxide barrier properties. Although a large number of studies have been devoted to the barrier properties of degradable film materials, such as adding nucleating agents to polylactic acid to increase the crystallinity of polylactic acid, thereby improving the gas barrier properties of the film; adding nanoparticles such as nano-montmorillonite and other lamellar structures to polylactic acid and polycaprolactone to extend the path for gas passage; adding barrier resins such as EVOH to bio-polyester, on the one hand, adding nanoparticles cannot truly achieve high gas barrier properties, and adding high-barrier polymers deviates from the original intention of full degradability. Obviously, only the development of truly fully degradable materials that can simultaneously meet the requirements of toughness and barrier properties will have practical significance and industrial prospects.

[0004] In response to the above problems, this patent aims to develop a fully degradable film material with good gas barrier properties, and coordinate the functions of different functional layers through a special multi-layer composite method to achieve the goal of balanced comprehensive performance. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of poor barrier properties and mechanical properties of degradable materials and to develop a film material with good mechanical properties and gas barrier properties.

[0006] The objective of the present invention is achieved through the following technical solutions: A biodegradable high-strength and high-barrier membrane is composited by a double-layer membrane, including a bottom P3H4B (polyhydroxyalkanoate)-PBAT (butylene adipate-butylene terephthalate copolymer) membrane layer and an upper hydrophobic modified cellulose membrane layer; wherein the bottom P3H4B-PBAT membrane layer is formed by melt extrusion casting, and the upper hydrophobic modified cellulose membrane layer is formed by solution casting; the upper surface of the P3H4B-PBAT membrane layer is covered with a silicon oxide layer by vacuum sputtering, and the lower surface of the hydrophobic modified cellulose membrane layer is silanized, and the treated double-layer membrane layer is composited by hot pressing.

[0007] Furthermore, the thickness of the P3H4B-PBAT film is between 0.15-0.35 mm, the thickness of the silicon oxide layer is between 0.05-0.08 mm, and the thickness of the hydrophobically modified cellulose film layer is between 0.08-0.16 mm.

[0008] Furthermore, the P3H4B-PBAT film is made of P3H4B and PBAT as main raw materials, and is melt-extruded into a film after adding a biomass compatibilizer, a biomass plasticizer, and an antioxidant to compound; wherein the mass ratio of P3H4B (poly 3-hydroxybutyric acid-co-4-hydroxybutyrate) and PBAT is between 80:20-50:50; the amount of the biomass compatibilizer and the biomass plasticizer is between 2-4% of the mass of the main material, and the amount of the antioxidant is between 0.5-1.2% of the mass of the main material.

[0009] Further, the molecular structure of the P34HB is as follows: ; Among them, n=100-150, m=200-280.

[0010] Furthermore, the molecular weight of the PBAT is between 20,000 and 60,000.

[0011] Furthermore, the biomass compatibilizer is a biopolyester graft, including one of polylactic acid grafted with maleic anhydride, polycaprolactone grafted with maleic anhydride, and polylactic acid grafted with β-hydroxyethyl acrylate; the molecular weight of the biopolyester used is between 20,000-50,000, preferably between 20,000-35,000.

[0012] Furthermore, the biomass plasticizer is tributyl citrate, triethyl citrate, epoxidized soybean oil bioplasticizer, and commercial SOY-CIZER TM BP series bio-based plasticizers.

[0013] Furthermore, the process conditions for melt extrusion film formation are as follows: the main material and the auxiliary material are uniformly mixed in a high-speed mixer, and then put into a twin-screw extruder casting machine at 180-220 oMelt extrusion casting under C conditions.

[0014] Furthermore, the hydrophobically modified cellulose film layer is made of long carbon chain hydrophobically modified hydroxyethyl cellulose as a main raw material, with auxiliary agents such as defoaming agent, leveling agent, plasticizer, etc. added, dissolved in a solvent and then formed into a film by casting.

[0015] Furthermore, the solvent used needs to be selected according to the modification and solubility of the raw materials.

[0016] Furthermore, the long carbon chain hydrophobic modified hydroxyethyl cellulose is prepared by using hydroxyethyl cellulose as a starting material and a halogenated alkane as a modifier, wherein the hydroxyl groups are etherified to obtain a modified hydroxyethyl cellulose having a long carbon chain structure. The length and content of the hydrophobic chain can be controlled by changing the type of the halogenated alkane, such as dodecane bromide and octadecane bromide, and the amount used.

[0017] Furthermore, the mass of the long carbon chain hydrophobically modified hydroxyethyl cellulose inserted is between 10-20% based on the mass of the hydroxyethyl cellulose.

[0018] Furthermore, the plasticizer of the hydrophobically modified cellulose film layer is preferably epoxy fatty acid ester or epoxy soybean oil.

[0019] Furthermore, the silanization modification process of the lower surface of the hydrophobically modified cellulose membrane layer is: dissolving the silane coupling agent in ethanol to form a solution with a mass fraction of 3-6%, spraying the solution evenly on the membrane surface, and obtaining a modified membrane after drying; the silane coupling agent can be one of KH540, KH550, KH560, KH792, Si-563, and A-171 coupling agents, which can effectively ensure the bonding between the hydrophobically modified cellulose membrane layer and the silicon oxide membrane layer.

[0020] Furthermore, the basic mechanical properties of the P3H4B-PBAT film layer are as follows: the tensile strength and the elongation at break are between 30.6-52.4 MPa and 89.2-152.6%, respectively, and the tear strength is between 126.2N-198.4N; the basic mechanical properties of the hydrophobically modified cellulose film layer are as follows: the tensile strength and the elongation at break are between 22.5-38.2 MPa and 58.5-124.3%, and the tear strength is between 54.5N-92.1N.

[0021] Further, the composite of the P3H4B-PBAT membrane layer and the hydrophobically modified cellulose membrane layer is performed by setting one or more groups of temperatures at 60-85 o The double rollers between C are hot pressed for 1-2 minutes and the pressure is between 0.5-2MPa to achieve close bonding between the two layers.

[0022] Furthermore, the beneficial effects of the present invention are: a fully degradable double-layer structure is adopted, in which the bottom P3H4B-PBAT film ensures good basic mechanical strength and tensile properties, the attached silicon oxide layer can provide sufficient gas barrier properties, and the outer hydrophobic modified cellulose film layer not only plays a role in further coordinating mechanical properties such as stretching and tearing, but also helps to improve gas barrier properties and provide surface hydrophobicity. The special treatment between the two layers will also greatly enhance the bonding between the modified cellulose film layer and the silicon oxide film layer, thereby synergistically improving performance.

[0023] Further, the membrane of the present invention is tested in the following manner: The tensile strength and elongation at break of the membrane are tested according to GB / T 1040.3-2006 standard; The tear strength of the film is tested according to GB / T 16578.3-2008 standard; The impact strength of the film is tested according to GB / T 9639.1-2008 standard; The puncture resistance of the membrane is tested according to GB / T 37841-2019 standard; The oxygen barrier properties of the film are tested according to GB / T 18454-2019 standard; The carbon dioxide barrier properties of the film are tested according to GB / T 1038.1-2022 standard. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Schematic diagram of the multilayer structure of the film prepared in Example 1. DETAILED DESCRIPTION

[0025] The exemplary implementation methods of the present invention will be described in detail below, but these implementation methods are for exemplary purposes only and the present invention is not limited thereto.

[0026] Example 1 like Figure 1 As shown, a degradable high-strength and high-barrier membrane is composited by a double-layer membrane, including a bottom P3H4B-PBAT membrane layer 1-1 and an outer hydrophobic modified cellulose membrane layer 2-1; wherein the upper surface of the bottom P3H4B-PBAT membrane layer 1-1 is plasma treated and then covered with a silicon oxide layer 1-2 by vacuum sputtering; the lower surface of the hydrophobic modified cellulose membrane layer 2-1 is silanized and modified to cover the silane modified layer 2-2, and then the double layers are composited by hot pressing.

[0027] The thickness of the P3H4B-PBAT film layer is 0.26 mm, the thickness of the silicon oxide layer is 0.06 mm, and the thickness of the hydrophobically modified cellulose film layer is 0.1 mm.

[0028] The P3H4B-PBAT film layer is made of P3H4B and PBAT as main raw materials, and polylactic acid grafted maleic anhydride, tributyl citrate and antioxidant 1020 are added to form a film after melt extrusion; the mass ratio of P3H4B to PBAT is 70:30; the amount of polylactic acid grafted maleic anhydride and tributyl citrate is 3.5% and 2.5% of the main material mass respectively, and the amount of antioxidant 1020 is 0.7% of the main material.

[0029] The molecular structure of the P34HB is as follows: ; Among them, n=120, m=250.

[0030] The molecular weight of the PBAT is 35,000.

[0031] The molecular weight of the polylactic acid grafted with maleic anhydride is 32,000.

[0032] The process conditions of melt extrusion film forming are as follows: the main material and the auxiliary material are mixed evenly in a high-speed mixer, and then put into a twin-screw extruder casting machine at 190-220 o C conditions to form a melt extrusion cast film.

[0033] The hydrophobically modified cellulose film layer is prepared by solvent casting using octadecane hydrophobically modified hydroxyethyl cellulose as raw material, adding 0.5% by weight of defoamer, 0.5% by weight of leveling agent, and 1.5% by weight of epoxy soybean oil, and using DMSO as solvent.

[0034] The mass of the long carbon chain hydrophobic modified hydroxyethyl cellulose is calculated based on the mass of the hydroxyethyl cellulose, and the mass of the connected long carbon chain is 14%.

[0035] The silanization modification of the lower surface of the hydrophobically modified cellulose membrane layer is performed by dissolving Si-563 coupling agent in ethanol to form a solution with a mass fraction of 5%, spraying the solution evenly on the membrane surface, and obtaining a modified membrane after drying.

[0036] The bottom P3H4B-PBAT film layer and the outer hydrophobic modified cellulose film layer are composited by two groups of temperatures of 60 o C. 70 o The roller of C has a rolling time of 1.5min and a pressure of 1MPa for each group to achieve a close bond between the two layers.

[0037] The properties of the prepared membrane materials are shown in Table 1.

[0038] Example 2 A degradable high-strength and high-barrier membrane is composited by a double-layer membrane, including a bottom P3H4B-PBAT membrane layer and an outer hydrophobic modified cellulose membrane layer; wherein the upper surface of the bottom P3H4B-PBAT membrane layer is plasma treated and then covered with a silicon oxide layer by vacuum sputtering; the lower surface of the hydrophobic modified cellulose membrane layer is silanized and covered with a silane modified layer, and then the double layers are composited by hot pressing.

[0039] The thickness of the P3H4B-PBAT film layer is 0.18 mm, the thickness of the silicon oxide layer is 0.08 mm, and the thickness of the hydrophobically modified cellulose film layer is 0.14 mm.

[0040] The P3H4B-PBAT film layer is made of P3H4B and PBAT as main raw materials, and polycaprolactone grafted maleic anhydride, triethyl citrate and antioxidant 1020 are added and then melt-extruded into a film; the mass ratio of P3H4B to PBAT is 75:25; the amount of polylactic acid grafted maleic anhydride and tributyl citrate is 3% and 2.8% of the mass of the main materials respectively, and the amount of antioxidant 1020 is 1% of the main material.

[0041] The molecular structure of the P34HB is as follows: ; Among them, n=150, m=260.

[0042] The molecular weight of the PBAT is 42,000.

[0043] The molecular weight of the polylactic acid grafted with maleic anhydride is 38,000.

[0044] The process conditions of melt extrusion film forming are as follows: the main material and the auxiliary material are mixed evenly in a high-speed mixer, and then put into a twin-screw extruder casting machine at 190-220 o C conditions to form a melt extrusion cast film.

[0045] The hydrophobically modified cellulose film layer is prepared by solvent casting using dodecane hydrophobically modified hydroxyethyl cellulose as raw material, adding 0.8% by weight of defoamer, 0.8% by weight of leveling agent, and 2.2% by weight of epoxy soybean oil, and using DMSO as solvent.

[0046] The mass of the long carbon chain hydrophobic modified hydroxyethyl cellulose is calculated based on the mass of the hydroxyethyl cellulose, and the mass of the connected long carbon chain is 16%.

[0047] The silanization modification of the lower surface of the hydrophobically modified cellulose membrane layer is performed by dissolving the KH792 coupling agent in ethanol to form a solution with a mass fraction of 4%, spraying the solution evenly on the membrane surface, and obtaining a modified membrane after drying.

[0048] The bottom P3H4B-PBAT film layer and the outer hydrophobically modified cellulose film layer are composited by two groups of temperatures of 65 o C. 75 o The roller of C achieves a close bond between the two layers through each set of rolling with a pressing time of 2 minutes and a pressure of 1.2 MPa.

[0049] The properties of the prepared membrane materials are shown in Table 1.

[0050] Example 3 A degradable high-strength and high-barrier membrane is composited by a double-layer membrane, including a bottom P3H4B-PBAT membrane layer and an outer hydrophobic modified cellulose membrane layer; wherein the upper surface of the bottom P3H4B-PBAT membrane layer is plasma treated and then covered with a silicon oxide layer by vacuum sputtering; the lower surface of the hydrophobic modified cellulose membrane layer is silanized and covered with a silane modified layer, and then the double layers are composited by hot pressing.

[0051] The thickness of the P3H4B-PBAT film is 0.33 mm, the thickness of the silicon oxide layer is 0.07 mm, and the thickness of the hydrophobically modified cellulose film layer is 0.15 mm.

[0052] The P3H4B-PBAT membrane is made of P3H4B and PBAT as main raw materials, and polycaprolactone grafted maleic anhydride and SOY-CIZER TM BP series bio-based plasticizer and antioxidant 1020 are compounded and melt-extruded into films; the mass ratio of P3H4B to PBAT is 75:25; the dosage of polylactic acid grafted maleic anhydride and tributyl citrate is 3% and 2.8% of the main material mass respectively, and the dosage of antioxidant T501 is 1% of the main material.

[0053] The molecular structure of the P34HB is as follows: ; Among them, n=110, m=270.

[0054] The molecular weight of the PBAT is 48,000.

[0055] The molecular weight of the polycaprolactone grafted maleic anhydride is 38,000.

[0056] The process conditions of melt extrusion film forming are as follows: the main material and the auxiliary material are mixed evenly in a high-speed mixer, and then put into a twin-screw extruder casting machine at 190-220 o C conditions to form a melt extrusion cast film.

[0057] The main raw material of the hydrophobically modified cellulose film layer is octadecane hydrophobically modified hydroxyethyl cellulose as the raw material, 0.6% of defoamer, 0.6% of leveling agent, and 2.6% of epoxy fatty acid methyl ester are added, and ethyl acetate is used as the solvent to obtain the film layer through solvent casting.

[0058] The long carbon chain hydrophobic modified hydroxyethyl cellulose is calculated based on the mass of the hydroxyethyl cellulose, and the mass of the connected long carbon chain is 18%.

[0059] The silanization modification of the lower surface of the hydrophobically modified cellulose membrane layer is performed by dissolving the KH550 coupling agent in ethanol to form a solution with a mass fraction of 5%, spraying the solution evenly on the membrane surface, and obtaining a modified membrane after drying.

[0060] The bottom P3H4B-PBAT film layer and the outer hydrophobically modified cellulose film layer are composited by two groups of temperatures of 65 o C. 75 o The roller of C achieves a close bond between the two layers through each set of rolling with a time of 1.5 min and a pressure of 1.5 MPa.

[0061] The properties of the prepared membrane materials are shown in Table 1.

[0062] Example 4 A degradable high-strength and high-barrier membrane is composited by a double-layer membrane, including a bottom P3H4B-PBAT membrane layer and an outer hydrophobic modified cellulose membrane layer; wherein the upper surface of the bottom P3H4B-PBAT membrane layer is plasma treated and then covered with a silicon oxide layer by vacuum sputtering; the lower surface of the hydrophobic modified cellulose membrane layer is silanized and covered with a silane modified layer, and then the double layers are composited by hot pressing.

[0063] The thickness of the P3H4B-PBAT film layer is 0.16 mm, the thickness of the silicon oxide layer is 0.07 mm, and the thickness of the hydrophobically modified cellulose film layer is 0.09 mm.

[0064] The P3H4B-PBAT film layer is made of P3H4B and PBAT as main raw materials, and polycaprolactone grafted maleic anhydride and SOY-CIZER TM BP series bio-based plasticizer and antioxidant 1020 are compounded and melt-extruded into films; the mass ratio of P3H4B to PBAT is 75:25; the dosage of polylactic acid grafted β-hydroxyethyl acrylate and epoxy soybean oil is 3% and 2.8% of the main material mass respectively, and the dosage of antioxidant T501 is 1% of the main material.

[0065] The molecular structure of the P34HB is as follows: ; Among them, n=140, m=210.

[0066] The molecular weight of the PBAT is 48,000.

[0067] The molecular weight of the polycaprolactone grafted maleic anhydride is 28,000.

[0068] The process conditions of melt extrusion film forming are as follows: the main material and the auxiliary material are mixed evenly in a high-speed mixer, and then put into a twin-screw extruder casting machine at 190-220 o Melt extrusion casting under C conditions.

[0069] The hydrophobically modified cellulose film layer is prepared by solvent casting using dodecane hydrophobically modified hydroxyethyl cellulose as raw material, adding 0.6% by weight of defoamer, 0.6% by weight of leveling agent, and 2.2% by weight of epoxy soybean oil, and using DMSO as solvent.

[0070] The mass of the long carbon chain hydrophobic modified hydroxyethyl cellulose is calculated based on the mass of the hydroxyethyl cellulose, and the mass of the connected long carbon chain is 14%.

[0071] The silanization modification of the lower surface of the hydrophobically modified cellulose membrane layer is carried out by dissolving KH540 in ethanol to form a solution with a mass fraction of 4.5%, spraying the solution evenly on the membrane surface, and obtaining a modified membrane after drying.

[0072] The bottom P3H4B-PBAT film layer and the outer hydrophobic modified cellulose film layer are composited by two groups of temperatures of 60 o C. 80 o C's rollers are used, and each set of rolling time is 1.5 minutes to achieve a close bond between the two layers.

[0073] The properties of the prepared membrane materials are shown in Table 1.

[0074] Comparative Example 1 Compared with Example 1, the comparative example does not have the upper hydrophobic modified cellulose film layer, and other formulas and processes are completely the same.

[0075] The properties of the prepared membrane are shown in Table 1: It can be seen from Table 1 that when the hydrophobically modified cellulose film layer on the surface is removed, the tensile strength, elongation at break and tear strength are slightly reduced. This is because the lower P3H4B-PBAT film has no synergy and partial force dispersion; at the same time, the gas barrier property is also slightly reduced, indicating that the upper hydrophobically modified cellulose film layer also plays a certain gas barrier synergy.

[0076] Comparative Example 2 Compared with Example 2, the comparative example does not have a silicon oxide layer on the surface of the P3H4B-PBAT film layer, and other formulas and processes are completely the same.

[0077] The properties of the prepared membrane are shown in Table 1: As can be seen from Table 1, when the middle silicon oxide layer is removed, the mechanical properties of the film are slightly reduced, while the gas barrier property is greatly reduced. This shows that the silicon oxide layer still plays the main barrier role in the film.

[0078] Comparative Example 3 Compared with Example 1, the comparative example changes the P3H4B-PBAT film layer to a PLA film layer, and the other formulas and processes are completely the same.

[0079] Among them, the PLA film layer uses PLA as the main material, and is melt-extruded into a film by adding plasticizers, toughening agents, and nucleating agents. The basic mechanical properties of the film alone are: tensile strength and elongation at break are 36.7MPa and 24.6%, and transverse and longitudinal tear strengths are 104.6N and 67.9N.

[0080] The properties of the prepared membrane are shown in Table 1: As can be seen from Table 1, the toughness and tear strength of the overall film are greatly reduced, and the barrier property is also reduced to a certain extent, indicating that the performance of the base film has an important influence on the overall film and also affects the overall gas barrier effect.

[0081] Comparative Example 4 Compared with Example 1, the comparative example changes the hydrophobically modified cellulose membrane layer into a cellulose acetate membrane layer, and the other formulas and processes are completely the same.

[0082] Among them, the cellulose acetate film layer is dissolved in 60% ethanol solvent and then cast into a film. The thickness of the film is 0.08mm. The basic mechanical properties of the single film are: tensile strength and elongation at break are 21.6MPa and 57.4%, and transverse and longitudinal tear strengths are 27.6N and 22.4N.

[0083] The properties of the prepared membrane are shown in Table 1: As can be seen from Table 1, the strength, toughness and tear strength of the overall film all decreased to a certain extent, and the barrier property also decreased to a certain extent, indicating that the upper film also played a synergistic role in the overall performance and barrier property of the film.

[0084] Table 1. Performance of membrane materials prepared in Examples and Comparative Examples Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Tensile strength (MPa) 46.4 42.9 56.5 55.9 37.6 39.7 35.8 42.3 Elongation at break (%) 104.5 88.1 128.9 132.8 114.5 83.8 25.8 83.4 Tear strength (longitudinal) / (transverse) (MPa) 204.6 / 182.4 173.9 / 142.8 231.7 / 187.6 142.6 / 93.8 134.4 / 131.7 201.3 / 171.5 109.3 / 87.6 165.5 / 127.4 Puncture resistance (N) 13.5 11.7 16.8 14.3 11.4 10.8 12.4 13.7 <![CDATA[O2 permeation rate cm 3 / (m 3 ·24hr·MPa)]]> 82.3 42.1 56.7 76.5 104.6 672.9 173.8 127.6 <![CDATA[CO2 permeability cm 3 / (m 3 ·24hr·MPa)]]> 93.7 35.4 51.2 69.8 133.5 629.3 196.9 169.5

Claims

1. A degradable high-strength and high-barrier membrane, which is composed of a double-layer membrane, including a bottom P3H4B-PBAT membrane layer and an upper hydrophobic modified cellulose membrane layer; wherein: The bottom P3H4B-PBAT film layer is formed by melt extrusion casting, and the upper hydrophobic modified cellulose film layer is formed by solution casting; the upper surface of the P3H4B-PBAT film layer is covered with a silicon oxide layer by vacuum sputtering, and the lower surface of the hydrophobic modified cellulose film layer is silanized, and the treated double-layer film layer is composited by hot pressing; the thickness of the P3H4B-PBAT film layer is between 0.15-0.35 mm, the thickness of the silicon oxide layer is between 0.05-0.08 mm, and the thickness of the hydrophobic modified cellulose film layer is between 0.08-0.16 mm.

2. The degradable high-strength and high-barrier film according to claim 1, characterized in that: The P3H4B-PBAT film layer is made of P3H4B and PBAT as main raw materials, and is melt-extruded into a film after adding a biomass compatibilizer, a biomass plasticizer and an antioxidant to compound; wherein the mass ratio of P3H4B to PBAT is between 80:20 and 50:50; the amount of the biomass compatibilizer and the biomass plasticizer is between 2% and 4% of the mass of the main material, and the amount of the antioxidant is between 0.5% and 1.2% of the mass of the main material.

3. The degradable high-strength and high-barrier film according to claim 1, characterized in that: The biomass compatibilizer is a biopolyester graft, which can be selected from one of polylactic acid grafted with maleic anhydride, polycaprolactone grafted with maleic anhydride, and polylactic acid grafted with β-hydroxyethyl acrylate.

4. The degradable high-strength and high-barrier film according to claim 1, characterized in that: The biomass plasticizers are tributyl citrate, triethyl citrate, epoxidized soybean oil bioplasticizer, and commercial SOY-CIZER TM BP series bio-based plasticizers.

5. The degradable high-strength and high-barrier film according to claim 1, characterized in that: The hydrophobically modified cellulose film layer is made of long carbon chain hydrophobically modified hydroxyethyl cellulose as the main raw material, with auxiliary agents such as defoamer, leveling agent, plasticizer, etc. added, dissolved in a solvent and then formed into a film by casting.

6. The degradable high-strength and high-barrier film according to claim 1, characterized in that: The silanization modification process of the lower surface of the hydrophobically modified cellulose membrane layer is as follows: dissolving a silane coupling agent in ethanol to form a solution with a mass fraction of 3-6%, spraying the solution evenly on the membrane surface, and obtaining a modified membrane after natural drying; the silane coupling agent can be one of KH540, KH550, KH560, KH792, Si-563, and A-171 coupling agents.

7. The degradable high-strength and high-barrier film according to claim 1, characterized in that: The basic mechanical properties of the P3H4B-PBAT film layer are as follows: the tensile strength and the elongation at break are between 30.6-52.4 MPa and 89.2-152.6% respectively, and the tear strength is between 126.2N-198.4N; the basic mechanical properties of the hydrophobically modified cellulose film layer are as follows: the tensile strength and the elongation at break are between 22.5-38.2 MPa and 58.5-124.3% respectively, and the tear strength is between 54.5N-92.1N.

8. The degradable high barrier antibacterial film according to claim 1, characterized in that: The P3H4B-PBAT membrane layer and the hydrophobically modified cellulose membrane layer are composited by setting one or more groups of temperatures at 60-85 o The double rollers between C are hot pressed for 1-2 minutes and the pressure is between 0.5-2MPa to achieve close bonding between the two layers.

Citation Information

Patent Citations

  • Full-degradable mulching film and preparation method thereof

    CN110483961A

  • Biodegradable Film and Laminate

    US20150337094A1

  • Deep eutectic solvent for the modification of nanocellulose film

    WO2020044210A1

  • Silicon dioxide coated polyhydroxyalkanoates for packaging

    WO2024119002A1