Method for rapidly preparing coal-based homologous carbon material and application
The microwave method is used to treat coal and metal catalysts, and combine coal pyrolysis products to combine them to prepare high-efficiency and low-cost coal-based homologous carbon materials, which solves the problem of insufficient negative performance of coal-based carbon materials and improves the electrode materials of sodium ion batteries performance.
Patent Information
- Application Number
- CN202411051649.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-01
AI Technical Summary
The coal-based carbon material negative electrode has problems in sodium ion batteries with low first desodium capacity, low first Coulomb efficiency, and complex and high cost.
The coal and metal catalyst were mixed with the microwave method and treated with an oxidative atmosphere to obtain a solid and liquid precursor, and then heat treatment was performed under an inert atmosphere, combined with the coal pyrolytic product composite, and coal-based homologous carbon material was prepared by microwave treatment.
It realizes rapid, low-cost and environmentally friendly preparation of coal-based homologous carbon materials, improves the specific capacity and Coulomb efficiency of the material, simplifies the process flow, and provides excellent electrode material performance for sodium ion batteries.
Smart Images

Figure CN118978144A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of material preparation, and in particular relates to a method for rapidly preparing a coal-based homologous carbon material and an application thereof. Background Art
[0002] In electrochemical energy storage, lithium-ion batteries and lead-acid batteries currently occupy an important position. Among them, lithium-ion batteries have a higher energy density and a longer cycle life, but the cost remains high, and there is a shortage of lithium resources. The outstanding advantages of lead-acid batteries are low cost and high recovery rate, but low energy density and poor cycle life. Therefore, it is urgent to develop a low-cost, resource-rich electrochemical energy storage system. Through continuous exploration in recent years, sodium-ion batteries can solve the above problems well. In sodium-ion batteries, the positive and negative electrode materials determine their performance. For negative electrode materials, carbon materials have commercial prospects. Among the raw materials of carbon materials, only coal has both low cost and abundant reserves. However, the negative electrode of coal-based carbon materials has the problems of low first sodium removal capacity and low first coulomb efficiency. The current modification method is relatively cumbersome and costly. Summary of the invention
[0003] The purpose of the present invention is to solve the problems of low first sodium removal capacity, low first coulombic efficiency, and complex modification method in the negative electrode of coal-based carbon materials, and to provide a method and application for rapidly preparing coal-based homologous carbon materials. The present invention uses cheap and readily available coal as raw material, and through a rapid preparation microwave method, it is compounded with liquid organic matter produced by the pyrolysis of the coal itself. The operation is simple, environmentally friendly and efficient.
[0004] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0005] A method for rapidly preparing coal-based homologous carbon materials, the method comprising:
[0006] Step 1: Mixing the coal raw material and the metal catalyst and subjecting the mixture to microwave treatment in an oxidizing atmosphere, wherein the obtained solid product is solid precursor 1 and the obtained liquid product is liquid precursor 1;
[0007] Step 2: Liquid precursor 2 is obtained by removing water from liquid precursor 1, and solid precursor 2 is obtained by deashing solid precursor 1; solid precursor 2, liquid precursor 2 and an auxiliary agent are added into a reaction container, and heat-treated under an inert atmosphere to obtain a solid product, which is solid precursor 3;
[0008] Step 3: The solid precursor 3 is subjected to microwave treatment under an inert atmosphere to obtain a coal-based homologous carbon material.
[0009] Furthermore, in step one, the coal raw material is one or more of peat, lignite, bituminous coal or anthracite; the metal catalyst is one or more of ferric chloride, ferrous chloride, ferric oxide, ferrous oxide, ferric oxide, aluminum chloride, aluminum oxide, zinc chloride, zinc oxide, potassium chloride, potassium oxide, sodium chloride and sodium oxide; and the mass ratio of the coal raw material to the metal catalyst is 100:1 to 50.
[0010] Furthermore, in step one, the oxidizing atmosphere is one or more of air, oxygen, carbon dioxide and water vapor; and the flow rate of the oxidizing atmosphere is 0.01 to 100 L / min.
[0011] Furthermore, in step 2, the mass ratio of the solid precursor 2 to the liquid precursor 2 is 20:1-40, and the mass ratio of the solid precursor 2 to the auxiliary agent is 50:1-50.
[0012] Furthermore, in step 2, the auxiliary agent includes one or more of amino, carboxyl, hydroxyl, anhydride, halogen, and sulfonate functional groups contained in organic matter.
[0013] Furthermore, in step 2, the heat treatment time is 0.5 to 30 hours, the temperature is 50 to 400° C., and the pressure is 10 to 1000 kPa.
[0014] Furthermore, in step 1 and step 3, the power of the microwave is 100-5000W, and the time is 0.5-200min.
[0015] Furthermore, in step 2 and step 3, the inert gas is one or more of nitrogen, argon and helium, and the flow rate of the inert gas is 0.1 to 50 L / min.
[0016] A coal-based homologous carbon material prepared by the above method.
[0017] A coal-based homologous carbon material prepared by the above method is used in electrode materials of sodium ion batteries, lithium ion batteries and potassium ion batteries.
[0018] Compared with the prior art, the beneficial effects of the present invention are: first, the present invention provides a high value-added utilization method of coal, the preparation method is short in time, environmentally friendly, simple to operate, low in production cost and high in yield; second, the microwave treatment in step one provides abundant storage sites for subsequent sodium ion storage and improves the specific capacity of the material; finally, in step two, the coal pyrolysis product is compounded to reduce the surface defects of the material particles and improve the coulombic efficiency of the material during the charging and discharging process, while forming closed pores to provide sites for sodium ion storage, further improving the specific capacity of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 XRD spectra of samples YY-1 and Y-1.
[0020] Figure 2 The charge and discharge curves of samples YY-1 and Y-1. DETAILED DESCRIPTION
[0021] The present invention is described in detail below with reference to the embodiments, but the embodiments of the present invention are not limited thereto. Obviously, the embodiments described below are only partial embodiments of the present invention. For those skilled in the art, other similar embodiments obtained without creative labor all fall within the protection scope of the present invention.
[0022] Example 1
[0023] After mixing 20g of peat with 5g of zinc chloride, put it into a microwave reactor, treat it for 200min under a carbon dioxide atmosphere with a flow rate of 0.01L / min and a microwave power of 100W, deash the obtained solid product, and dehydrate the obtained liquid product. Take 5g of deashed solid, 0.25g of dehydrated liquid and 5g of ethylenediamine and transfer them to a reaction vessel, and treat them at 150°C for 6h under a nitrogen atmosphere of 0.5L / min and a pressure of 500kPa. Take 5g of the obtained solid and put it into a microwave reactor, treat it for 60min under a 1L / min argon atmosphere and a microwave power of 2000W to obtain a coal-based homologous carbon material, which is recorded as NY-1.
[0024] Example 2
[0025] 20g lignite was mixed with 10g ferric oxide, and then placed in a microwave reactor. The mixture was treated for 30min at a flow rate of 100L / min in an air atmosphere and a microwave power of 1000W. The obtained solid product was deashed and the obtained liquid product was dehydrated. 5g of deashed solid, 10g of dehydrated liquid and 0.5g of terephthalic acid were mixed and transferred to a reaction vessel. The mixture was treated at 400°C for 30min at a nitrogen atmosphere of 10L / min and a pressure of 1000kPa. 5g of the obtained solid was placed in a microwave reactor and treated for 0.5min at a nitrogen atmosphere of 50L / min and a microwave power of 5000W to obtain a coal-based homologous carbon material, which was recorded as HY-1.
[0026] Example 3
[0027] 20g of bituminous coal was mixed with 2g of potassium oxide, and then placed in a microwave reactor. The mixture was treated for 60min under an oxygen atmosphere with a flow rate of 1L / min and a microwave power of 500W. The obtained solid product was deashed and the obtained liquid product was dehydrated. 5g of deashed solid, 2g of dehydrated liquid and 2g of phthalic anhydride were mixed and transferred to a reaction vessel, and treated at 300°C for 60min under a nitrogen atmosphere of 1L / min and a pressure of 800kPa. 5g of the obtained solid was placed in a microwave reactor, and treated for 5min under a nitrogen atmosphere of 1L / min and a microwave power of 3000W to obtain a coal-based homologous carbon material, which was recorded as YY-1.
[0028] Example 4
[0029] After mixing 20g of anthracite with 0.2g of aluminum chloride, put it into a microwave reactor, treat it for 60min under a water vapor atmosphere with a flow rate of 15L / min and a microwave power of 1000W, deash the obtained solid product, and dehydrate the obtained liquid product. Take 5g of deashed solid, 0.25g of dehydrated liquid and 0.1g of ethylene glycol and transfer them to a reaction vessel, and treat them at 50°C for 30h under a 10L / min nitrogen atmosphere and a pressure of 10kPa. Take 5g of the obtained solid and put it into a microwave reactor, treat it for 30min under a 10L / min nitrogen atmosphere and a microwave power of 1000W to obtain a coal-based homologous carbon material, which is recorded as WY-1.
[0030] Comparative Example 1
[0031] 20g of bituminous coal and 2g of potassium oxide were mixed and placed in a microwave reactor. The mixture was treated for 60min in an oxygen atmosphere with a flow rate of 1L / min and a microwave power of 500W. The obtained solid product was deashed and the obtained liquid product was dehydrated. 5g of the deashed solid was placed in a microwave reactor and treated for 5min in a nitrogen atmosphere with a flow rate of 1L / min and a microwave power of 3000W to obtain a carbon material, which was recorded as Y-1.
[0032] The carbon materials obtained in Example 3 and Comparative Example 1 were subjected to XRD test. Figure 1 As shown, through XRD testing, it can be seen that the peaks of the spectra of YY-1 and Y-1 at 2θ of about 23° and 44° correspond to the 002 diffraction peak and 100 diffraction peak, respectively, indicating that it is a typical amorphous carbon. From the position of the 002 peak in the figure, it can be seen that YY-1 tends to be at a high angle, indicating that its structure is more ordered. The coal-based homologous carbon materials prepared in Example 3 and Comparative Example 1 were used as sodium ion battery electrode materials for electrochemical testing. The assembly and testing methods were carried out in accordance with the reference [Energy & Fuels [J]. 2021, 35 (10): 9029-9037]. The electrochemical test results are shown in Figure 2 As shown, the experiment shows that step two can effectively improve the battery's first coulombic efficiency, specific capacity and rate performance. At a current density of 0.03A / g, the specific capacity can reach 302.4mAh / g and the first coulombic efficiency is 94%.
[0033] Table 1 Electrochemical test results of samples prepared in Examples 1-4 and Comparative Example 1
[0034] Sample name First cycle sodium removal capacity (mAh / g) First coulombic efficiency (%) NY-1 281.7 85.2 HY-1 275.9 86.0 YY-1 302.4 93.7 WY-1 286.8 83.2 Y-1 268.2 88.3
[0035] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for rapidly preparing coal-based homologous carbon materials, characterized in that: The method is: Step 1: Mix the coal raw material and the metal catalyst and then perform microwave treatment in an oxidizing atmosphere, so that the obtained solid product is solid precursor 1, and the obtained liquid product is liquid precursor 1; Step 2: Liquid precursor 2 is obtained by removing water from liquid precursor 1, and solid precursor 2 is obtained by deashing solid precursor 1; solid precursor 2, liquid precursor 2 and an auxiliary agent are added into a reaction container, and heat-treated under an inert atmosphere to obtain a solid product, which is solid precursor 3; Step 3: The solid precursor 3 is subjected to microwave treatment under an inert atmosphere to obtain a coal-based homologous carbon material.
2. A method for rapidly preparing coal-based homologous carbon materials according to claim 1, characterized in that: In step one, the coal raw material is one or more of peat, lignite, bituminous coal or anthracite; the metal catalyst is one or more of ferric chloride, ferrous chloride, ferric oxide, ferrous oxide, ferric oxide, aluminum chloride, aluminum oxide, zinc chloride, zinc oxide, potassium chloride, potassium oxide, sodium chloride and sodium oxide; the mass ratio of the coal raw material to the metal catalyst is 100:1 to 50.
3. The method for rapidly preparing coal-based homologous carbon materials according to claim 1, characterized in that: In step 1, the oxidizing atmosphere is one or more of air, oxygen, carbon dioxide and water vapor; the flow rate of the oxidizing atmosphere is 0.01 to 100 L / min.
4. The method for rapidly preparing coal-based homologous carbon materials according to claim 1, characterized in that: In step 2, the mass ratio of the solid precursor 2 to the liquid precursor 2 is 20:1-40, and the mass ratio of the solid precursor 2 to the auxiliary agent is 50:1-50.
5. The method for rapidly preparing coal-based homologous carbon materials according to claim 1, characterized in that: In step 2, the auxiliary agent includes one or more of amino, carboxyl, hydroxyl, anhydride, halogen, and sulfonate functional groups in organic matter.
6. The method for rapidly preparing coal-based homologous carbon materials according to claim 1, characterized in that: In step 2, the heat treatment time is 0.5 to 30 hours, the temperature is 50-400° C., and the pressure is 10 to 1000 kPa.
7. The method for rapidly preparing coal-based homologous carbon materials according to claim 1, characterized in that: In step 1 and step 3, the power of the microwave is 100-5000W, and the time is 0.5-200min.
8. The method for rapidly preparing coal-based homologous carbon materials according to claim 1, characterized in that: In step 2 and step 3, the inert gas is one or more of nitrogen, argon and helium, and the flow rate of the inert gas is 0.1 to 50 L / min.
9. A coal-based homologous carbon material prepared by the method according to any one of claims 1 to 8.
10. A coal-based homologous carbon material prepared by the method according to any one of claims 1 to 8, which is used as an electrode material for sodium ion batteries, lithium ion batteries and potassium ion batteries.
Citation Information
Patent Citations
Preparation method of lignite-derived carbon, lignite-derived carbon and sodium ion battery
CN117049506A
Porous carbon material and the manufacturing method making the same
TW202426391A