Efficient and rapid graphite oxide preparation method

By adding interlayer dispersant and potassium ferrate to graphite and oxidation treatment under specific conditions, the problem of slow diffusion of oxidants is solved, and efficient and rapid graphene oxide preparation is achieved, which improves the oxidation rate and safety, and reduces the production costs.

CN118978155APending Publication Date: 2024-11-19HUBEI HUAEN NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411048181.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the existing graphite oxide preparation methods, the oxidant diffuses slowly between graphite layers, resulting in a long oxidation reaction time and safety hazards, making it difficult to achieve efficient and rapid graphene oxide preparation.

Method used

By adding interlayer dispersant and potassium ferrate to graphite, curing at specific temperatures and pressures, and then stirring reactions in a mixed environment of concentrated sulfuric acid and nitric acid, the oxidant entry is improved by using water bath conditions and deionized water treatment. The rate of graphite layer and the oxidation rate.

Benefits of technology

The rate of oxidant entering the graphite layer is significantly improved, the oxidation reaction time is shortened, the production cost is reduced, the corrosion to the equipment is reduced, and the graphite oxidation rate and safety is improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the field of graphite oxide material preparation, and discloses an efficient and rapid graphite oxide preparation method which comprises the following steps: S1, grinding dry graphite powder to 250-300 meshes; s2, adding an interlayer dispersant into the graphite in the step S1, then adding potassium ferrate, and maintaining for 0.5-1 hour; s3, adding the graphite prepared in the step S2 into a reactor, adding concentrated sulfuric acid into the reactor, uniformly stirring, and stirring to react for 1-2 hours under a water bath condition; s4, adding nitric acid into the graphite reactor in the step S3, and stirring to react at the temperature of 30-35 DEG C; and S5, slowly pouring reactants in the reactor in the step S4 into deionized water with the temperature of 30-60 DEG C, controlling the reaction temperature to be 20-60 DEG C, carrying out stirring reaction for 20-30 minutes, introducing 35% hydrogen peroxide into the deionized solution, and carrying out water washing, centrifugation and drying treatment to obtain the graphite oxide. The method has the advantages and effects of increasing the rate of the oxidant entering the graphite layer, improving the oxidation rate and reducing the production cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of graphite oxide preparation, and in particular to an efficient and rapid method for preparing graphite oxide. Background Art

[0002] Graphite oxide and its exfoliated product, graphene oxide, as key precursors for large-scale preparation of graphene, play an important role in many fields. Currently, in scientific research and industrial preparation, graphite is chemically oxidized in a concentrated sulfuric acid system using a strong oxidant based on the Hummers method, and further exfoliated to obtain graphene oxide.

[0003] Graphene oxide is mainly prepared by exfoliating graphite oxide. The preparation of graphite oxide is based on the reaction of graphite with a large amount of concentrated nitric acid, concentrated sulfuric acid, potassium permanganate and other composite strong oxidants. The most commonly used Hummers method is that the oxidant is composed of concentrated sulfuric acid and potassium permanganate. However, because the oxidant diffuses slowly between graphite layers, there are problems such as long oxidation reaction time and great safety hazards in the preparation process of graphite oxide. Therefore, the invention of an efficient and fast graphene oxide preparation technology is of great significance to the large-scale safe production of graphite oxide. Summary of the invention

[0004] The purpose of the present invention is to provide an efficient and rapid method for preparing graphite oxide, which has the effects of increasing the rate at which an oxidant enters a graphite layer, improving the oxidation rate and reducing production costs.

[0005] The above technical objectives of the present invention are achieved through the following technical solutions: an efficient and rapid method for preparing graphite oxide, comprising the following steps: S1, grinding dry graphite powder to 250-300 mesh;

[0006] S2, adding an interlayer dispersant to the graphite in step S1, then adding potassium ferrate, and curing for 0.5-1h;

[0007] S3, adding the graphite prepared in step S2 into the reactor, adding concentrated sulfuric acid into the reactor, stirring evenly, and stirring the reaction in a water bath for 1-2h;

[0008] S4, adding nitric acid to the graphite reactor in step S3, stirring and reacting at 30-35°C;

[0009] S5. Slowly pour the reactants in the reactor of step S4 into deionized water at a temperature of 30-60° C., control the reaction temperature to 20-60° C., stir the reaction for 20-30 minutes, pass 35% hydrogen peroxide into the deionized solution, and obtain graphite oxide after washing, centrifugation and drying.

[0010] The present invention is further configured as follows: the interlayer dispersant in step S2 is composed of sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide and benzoyl peroxide, and the ratio thereof is (2-4):(1-2):1.

[0011] The present invention is further configured as follows: the content of the interlayer dispersant in step S2 is 0.5-3% of the mass of the graphite, and the content of potassium ferrate is 15-20% of the mass of the graphite.

[0012] The present invention is further configured as follows: the curing temperature in step S2 is 30-40°C.

[0013] The present invention is further configured as follows: the curing pressure in step S2 is 0.5-1.0 MPa.

[0014] The present invention is further configured as follows: the ratio of sulfuric acid to nitric acid is 4:1.

[0015] The present invention is further configured as follows: the stirring time in step S4 is 10-20 minutes.

[0016] The beneficial effects of the present invention are:

[0017] 1. The interlayer dispersant of the present invention can effectively change the interaction between the interface of graphite and the oxidized intercalant; the positively charged anions carried by the interlayer dispersant are neutralized with the negative charges carried by the micro-oxidized graphite. Under the action of high temperature and pressure, the interlayer dispersant moves and diffuses rapidly in the solution into the graphite layer, reducing the interlayer repulsion, increasing the distance between the graphite layers by more than 35%, increasing the rate at which the oxidant enters the graphite layer, and improving the oxidation rate.

[0018] 2. The present invention uses potassium ferrate as an oxidant to nurture graphite. By controlling the temperature at 30-40°C and the pressure at 0.5-1.0MPa, the dispersing ability of the interlayer dispersant and the diffusion speed of ions are increased, the dispersion rate and oxidation efficiency of potassium ferrate between graphite layers are improved, and the oxidation reaction time of graphite in concentrated sulfuric acid is reduced.

[0019] 3. The present invention re-oxidizes graphite based on a mixture of concentrated sulfuric acid and nitric acid, which further reduces the oxidation time in a concentrated acid environment, reduces corrosion to production equipment, and reduces production costs. DETAILED DESCRIPTION

[0020] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Example 1

[0022] S1. Grind the dry graphite powder to 250 mesh;

[0023] S2, adding an interlayer dispersant with a content of 0.5% of the mass of graphite to the graphite in step S1, the interlayer dispersant is composed of sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, and benzoyl peroxide, and the ratio is 2:1:1, and then adding potassium ferrate with a content of 15% of the mass of graphite, and curing at 40°C and a pressure of 0.9MPa for 1h;

[0024] S3. Add the graphite prepared in step S2 into the reactor, add concentrated sulfuric acid into the reactor, stir evenly, and stir the reaction in a water bath for 1 hour.

[0025] S4. Add nitric acid into the graphite reactor in step S3, and stir the reaction at 30° C. for 10 min.

[0026] S5. Slowly pour the reactants in the reactor of step S4 into deionized water at a temperature of 30-60° C., control the reaction temperature to 20-60° C., stir the reaction for 20-30 minutes, pass 35% hydrogen peroxide into the deionized solution, and obtain graphite oxide after washing, centrifugation and drying.

[0027] Wherein, the ratio of sulfuric acid to nitric acid added in steps S3 and S4 is 4:1.

[0028] The prepared graphite oxide was subjected to elemental analysis to determine the contents of carbon, hydrogen and oxygen therein. Then, based on the measured content ratios of carbon, hydrogen and oxygen, the graphite oxidation rate was calculated to be 95.2%.

[0029] Example 2

[0030] S1. Grind the dry graphite powder to 300 mesh.

[0031] S2. Add an interlayer dispersant with a content of 3% of the mass of graphite to the graphite in step S1, wherein the interlayer dispersant is composed of sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, and benzoyl peroxide in a ratio of 4:1:1, and then add potassium ferrate with a content of 20% of the mass of graphite, and cure at 30° C. and a pressure of 0.5 MPa for 0.5 h.

[0032] S3. Add the graphite prepared in step S2 into the reactor, add concentrated sulfuric acid into the reactor, stir evenly, and stir the reaction in a water bath for 1 hour.

[0033] S4. Add nitric acid into the graphite reactor in step S3 and stir the reaction at 35° C. for 20 min.

[0034] S5. Slowly pour the reactants in the reactor of step S4 into deionized water at a temperature of 30-60° C., control the reaction temperature to 20-60° C., stir the reaction for 20-30 minutes, pass 35% hydrogen peroxide into the deionized solution, and obtain graphite oxide after washing, centrifugation and drying.

[0035] Wherein, the ratio of sulfuric acid to nitric acid added in steps S3 and S4 is 4:1.

[0036] The element analysis of the graphite oxide was carried out to determine the contents of carbon, hydrogen and oxygen elements therein. Then, based on the measured content ratios of carbon, hydrogen and oxygen elements, the graphite oxidation rate was calculated to be 81.5%.

[0037] Example 3

[0038] S1. Grind the dry graphite powder to 300 mesh.

[0039] S2. Add an interlayer dispersant with a content of 2% of the mass of graphite to the graphite in step S1, wherein the interlayer dispersant is composed of sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, and benzoyl peroxide in a ratio of 4:2:1, and then add potassium ferrate with a content of 18% of the mass of graphite, and cure at 35°C and a pressure of 1.0 MPa for 0.6 h.

[0040] S3. Add the graphite prepared in step S2 into the reactor, add concentrated sulfuric acid into the reactor, stir evenly, and stir the reaction in a water bath for 1.5 hours.

[0041] S4. Add nitric acid into the graphite reactor in step S3, and stir the reaction at 35° C. for 15 min.

[0042] S5. Slowly pour the reactants in the reactor of step S4 into deionized water at a temperature of 30-60° C., control the reaction temperature to 20-60° C., stir the reaction for 20-30 minutes, pass 35% hydrogen peroxide into the deionized solution, and obtain graphite oxide after washing, centrifugation and drying.

[0043] Wherein, the ratio of sulfuric acid to nitric acid added in steps S3 and S4 is 4:1.

[0044] The prepared graphite oxide was subjected to elemental analysis to determine the contents of carbon, hydrogen and oxygen therein, and then, based on the measured content ratios of carbon, hydrogen and oxygen, the graphite oxidation rate was calculated to be 92.4%.

[0045] Comparative Example: The conditions of the comparative example are the same as those of Example 2, except that no interlayer dispersant and potassium ferrate are added, and the calculated graphite oxidation rate is 71.8%.

[0046] It can be seen from Comparative Example 1 and Example 2 that under the same time conditions, the graphite oxidation rate is significantly improved.

Claims

1. An efficient and rapid method for preparing graphite oxide, characterized in that: The steps include: S1. Grind the dry graphite powder to 250-300 mesh; S2, adding an interlayer dispersant to the graphite in step S1, then adding potassium ferrate, and curing for 0.5-1h; S3, adding the graphite prepared in step S2 into the reactor, adding concentrated sulfuric acid into the reactor, stirring evenly, and stirring the reaction in a water bath for 1-2h; S4, adding nitric acid to the graphite reactor in step S3, stirring and reacting at 30-35°C; S5. Slowly pour the reactants in the reactor of step S4 into deionized water at a temperature of 30-60° C., control the reaction temperature to 20-60° C., stir the reaction for 20-30 minutes, pass 35% hydrogen peroxide into the deionized solution, and obtain graphite oxide after washing, centrifugation and drying.

2. An efficient and rapid method for preparing graphite oxide according to claim 1, characterized in that: The interlayer dispersant in step S2 is composed of sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide and benzoyl peroxide, and the ratio is (2-4):(1-2):

1.

3. The method for preparing graphite oxide efficiently and quickly according to claim 1, characterized in that: In step S2, the content of the interlayer dispersant is 0.5-3% of the mass of the graphite, and the content of potassium ferrate is 15-20% of the mass of the graphite.

4. The method for preparing graphite oxide efficiently and quickly according to claim 1, characterized in that: The curing temperature in step S2 is 30-40°C.

5. The method for preparing graphite oxide efficiently and quickly according to claim 1, characterized in that: The curing pressure in step S2 is 0.5-1.0 MPa.

6. The method for preparing graphite oxide efficiently and quickly according to claim 1, characterized in that: The ratio of sulfuric acid to nitric acid is 4:

1.