Silicon negative electrode material with improved cycle performance and preparation method thereof
By preparing mesoporous SiO2 and forming a double carbon cladding layer on its surface, the volume expansion problem of silicon negative electrode material caused by lithium ion deintercalation in lithium ion batteries is solved, and the cycle stability and capacity retention rate are significantly improved, and the cycle stability and capacity retention rate are achieved. Commercial application of silicon anode materials.
Patent Information
- Application Number
- CN202411009162.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-19
AI Technical Summary
The volume expansion effect of silicon anode material caused by lithium ion deintercalation in lithium-ion batteries hinders its commercial application, resulting in poor circulation performance.
By preparing mesoporous SiO2 and forming a double carbon cladding layer on its surface, stress expansion is relieved by using mesoporous SiO2, and volume changes are buffered by the carbon layer to improve the cyclic stability and rate performance of the silicon negative electrode material.
It effectively slows down the volume expansion effect of silicon negative electrode materials during the lithiation/dehydrogenation process, inhibits powdering, improves cycle stability and battery circulation performance, and significantly improves capacity retention.
Smart Images

Figure CN118978161A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a silicon negative electrode material with improved cycle performance and a preparation method thereof. Background Art
[0002] Silicon anode material has a high theoretical specific capacity (4200mAh / g), which is the preferred anode material for the next generation of high energy density batteries. Currently, the development of silicon anode material is in full swing, and it has a bright future in the field of lithium-ion batteries. Silicon anode material has a natural advantage in capacity, but the expansion effect caused by lithium ion deintercalation has hindered the commercial application process.
[0003] Relevant modifications to silicon negative electrode materials can inhibit the volume expansion effect of silicon materials during the cycle, improve the cycle of silicon negative electrode materials, and promote the commercialization of silicon negative electrode materials. Summary of the invention
[0004] Based on the technical problems existing in the background technology, the present invention proposes a silicon negative electrode material with improved cycle performance and a preparation method thereof.
[0005] The present invention provides a method for preparing a silicon negative electrode material with improved cycle performance, comprising the following steps:
[0006] S1. Preparation of mesoporous SiO2: dissolving a pH regulator in water to adjust the pH, sequentially adding an organic solvent and a silicon source and stirring evenly to obtain a mixed solution, subjecting the mixed solution to hydrothermal crystallization, suction filtration, drying, and calcination to obtain mesoporous SiO2;
[0007] S2. Preparation of C / rGO double carbon coating layer: graphene oxide is dispersed in water, mesoporous SiO2 is added for hydrothermal treatment, centrifugation, washing, and freeze-drying to obtain SiO2 / rGO, and SiO2 / rGO is calcined in an inert gas flow containing organic vapor to obtain a silicon negative electrode material SiO2@C / rGO with improved cycle performance.
[0008] The present invention obtains a silicon negative electrode material with improved cycle performance through a two-step method. First, the prepared mesoporous SiO2 is used to alleviate the stress expansion of the silicon material during the cycle. Secondly, the mesoporous SiO2 is coated with a double carbon shell to further buffer the expansion and contraction of the volume of the mesoporous SiO2, thereby improving the overall cycle stability and rate performance of the silicon negative electrode material.
[0009] Preferably, in S1, the pH regulator is urea.
[0010] The role of urea is to adjust the pH to a weak base, and secondly to form an oil-in-water emulsion system, allowing the silicon source and surfactant to adhere to the small droplets, reducing the surface activation energy of the particles. In the subsequent drying stage, due to the low melting point of urea (32.7 degrees), it will decompose into carbon dioxide and ammonia, making SiO2 form a mesoporous state.
[0011] Preferably, in S1, the pH is adjusted to 7.5-8.5.
[0012] Preferably, in said S1, the organic solvent is an anionic or cationic surfactant.
[0013] More preferably, in the S1, the organic solvent is selected from one or more of CTAB, SDS, and F127.
[0014] Anionic and cationic surfactants act as templates in the preparation of mesoporous SiO2; they can form micelle structures in solution, and under alkaline conditions, they will interact electrostatically and hydrophobically with the silicon source to form a complex.
[0015] Preferably, in said S1, the silicon source is tetraethyl orthosilicate.
[0016] Tetraethyl orthosilicate as a silicon source eventually becomes mesoporous SiO2, which is a raw material precursor.
[0017] Preferably, in S1, the hydrothermal treatment crystallization comprises treating at 100-120° C. for 72-96 hours.
[0018] Controlling the crystallization temperature and time of hydrothermal treatment within a certain range is helpful to the formation rate of silicon particle micelles and the formation of complete silicon particle morphology.
[0019] Preferably, in S1, the drying comprises treating at 60-150° C. for 12-24 hours.
[0020] Preferably, in said S1, the calcination comprises calcining at 450-500° C. for 6-8 hours.
[0021] Controlling the calcination temperature and time within a certain range is helpful to keep the specific surface area of mesoporous SiO2 within an appropriate range.
[0022] Preferably, in the S1, the mass ratio of the pH adjuster, water, organic solvent and silicon source is (0.01-0.1):0.4:(0.01-0.1):(0.02-0.03).
[0023] By adjusting the mass ratio of the raw materials, the mesoporous morphology of the obtained mesoporous SiO2 is more complete.
[0024] Preferably, in said S2, the hydrothermal treatment comprises treating at 180-200° C. for 24-36 hours.
[0025] Controlling the temperature of the hydrothermal treatment within a certain range is helpful for graphene oxide to adsorb on the surface of mesoporous SiO2 to form a graphene oxide layer coating.
[0026] Preferably, in S2, the organic vapor is ethanol vapor.
[0027] The role of ethanol vapor is to introduce the precursor of the second coating carbon layer.
[0028] Preferably, in said S2, the inert gas is argon.
[0029] Preferably, in said S2, calcination comprises calcination at 600-650° C. for 2-4 hours.
[0030] Controlling the calcination temperature and time within a certain range is helpful to carbonize the ethanol organic carbon precursor and form a carbon coating layer.
[0031] Preferably, in the S2, the mass ratio of graphene oxide, water and mesoporous SiO2 is (0.001-0.01):(0.9-1):(0.04-0.05).
[0032] Controlling the mass ratio of graphene oxide, water, and mesoporous SiO2 helps to control the coating amount of graphene oxide, slow down the volume expansion effect of silicon negative electrode materials, inhibit pulverization, and improve the cycle stability of silicon negative electrode materials.
[0033] The present invention also proposes a silicon negative electrode material with improved cycle performance prepared by the above preparation method, comprising mesoporous SiO2 as a core and organic-derived carbon and a double carbon layer of graphene oxide coating the mesoporous SiO2 as a shell.
[0034] The beneficial effects of the present invention are:
[0035] During the lithiation / dehydrogenation process, the significant change in the volume of SiO2 causes the electrode to break or even shatter, resulting in rapid capacity degradation. The use of carbonaceous materials to construct composite materials can effectively improve the conductivity and buffer the volume change. The silicon negative electrode material of the present invention has good structural stability and slows down the volume expansion effect of the silicon negative electrode material when lithium is extracted and inserted, inhibits pulverization, and improves the cycle stability of the silicon negative electrode material. The formation of a double carbon modified coating on the surface of the silicon negative electrode material can effectively alleviate the volume effect of the silicon negative electrode during the cycle, providing double insurance for the electrical contact of the silicon negative electrode after the cycle. At the same time, changing the traditional silicon material to a mesoporous silicon material can also help alleviate Li + The stress of the embedding and de-embedding process can be reduced, which can slow down the loss of expansion performance caused by stress and improve the cycle stability of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is the capacity cycle retention rate of the battery corresponding to Example 1 of the present invention and Comparative Example 1.
[0037] Figure 2 This is a HRSEM high-resolution image of mesoporous SiO2 obtained in step S1 in Example 1 of the present invention.
[0038] Figure 3 This is the SEM image of the silicon negative electrode material obtained in Example 1. DETAILED DESCRIPTION
[0039] The technical solution of the present invention is described in detail through specific embodiments.
[0040] Unless otherwise specified, the materials, reagents, etc. used in the following examples and comparative examples can be obtained from commercial sources.
[0041] Example 1
[0042] A method for preparing a silicon negative electrode material with improved cycle performance comprises the following steps:
[0043] S1. Preparation of mesoporous SiO2: 9 g urea was dissolved in 40 ml water and the pH was adjusted to 8. 10 g CTAB was added and stirred for 2 h, and then 2.1 g ethyl orthosilicate was added and stirred for 24 h to obtain a mixed solution. The mixed solution was charged into a reactor and subjected to a hydrothermal reaction at 100 ° C for 72 h, followed by cooling and filtration, drying at 60 ° C for 12 h, and then calcining at 450 ° C for 6 h to obtain mesoporous SiO2;
[0044] S2. Preparation of C / rGO double carbon coating layer: 30 mg of graphene oxide was dispersed in 30 ml of water, 1.5 g of mesoporous SiO2 was added into a reactor, and a hydrothermal reaction was carried out at 180°C for 24 h. The reaction was centrifuged, washed, and freeze-dried to obtain SiO2 / rGO. SiO2 / rGO was calcined at 600°C for 2 h in an argon gas flow containing ethanol vapor to obtain a silicon negative electrode material SiO2@C / rGO with improved cycle performance.
[0045] Example 2
[0046] A method for preparing a silicon negative electrode material with improved cycle performance comprises the following steps:
[0047] S1. Preparation of mesoporous SiO2: 9 g urea was dissolved in 40 ml water and the pH was adjusted to 8. 5 g F127 was added and stirred for 2 h. 2.1 g ethyl orthosilicate was added and stirred for 24 h to obtain a mixed solution. The mixed solution was charged into a reactor and subjected to a hydrothermal reaction at 100 ° C for 72 h. The mixture was then cooled and filtered. The mixture was dried at 80 ° C for 12 h. The mixture was then calcined at 500 ° C for 6 h to obtain mesoporous SiO2.
[0048] S2. Preparation of C / rGO double carbon coating layer: 30 mg of graphene oxide was dispersed in 30 ml of water, 1.5 g of mesoporous SiO2 was added into a reactor, and a hydrothermal reaction was carried out at 180°C for 24 h. The reaction was centrifuged, washed, and freeze-dried to obtain SiO2 / rGO. SiO2 / rGO was calcined at 600°C for 2 h in an argon gas flow containing ethanol vapor to obtain a silicon negative electrode material SiO2@C / rGO with improved cycle performance.
[0049] Example 3
[0050] A method for preparing a silicon negative electrode material with improved cycle performance comprises the following steps:
[0051] S1. Preparation of mesoporous SiO2: 6 g urea was dissolved in 40 ml water and the pH was adjusted to 7.5. 10 g SDS was added and stirred for 2 h. 2.1 g ethyl orthosilicate was added and stirred for 24 h to obtain a mixed solution. The mixed solution was charged into a reactor and subjected to a hydrothermal reaction at 100 ° C for 72 h. The mixture was then cooled and filtered, dried at 60 ° C for 12 h, and then calcined at 450 ° C for 6 h to obtain mesoporous SiO2.
[0052] S2. Preparation of C / rGO double carbon coating layer: 30 mg of graphene oxide was dispersed in 30 ml of water, 1.5 g of mesoporous SiO2 was added into a reactor and hydrothermally reacted at 200 °C for 24 h, followed by centrifugation, washing and freeze-drying to obtain SiO2 / rGO. SiO2 / rGO was calcined at 600 °C for 2 h in an argon gas flow containing ethanol vapor to obtain a silicon negative electrode material SiO2@C / rGO with improved cycle performance.
[0053] Example 4
[0054] A method for preparing a silicon negative electrode material with improved cycle performance comprises the following steps:
[0055] S1. Preparation of mesoporous SiO2: 6 g urea was dissolved in 40 ml water and the pH was adjusted to 7.5. 5 g CTAB was added and stirred for 2 h, and 2.1 g ethyl orthosilicate was added and stirred for 24 h to obtain a mixed solution. The mixed solution was charged into a reactor and subjected to a hydrothermal reaction at 100 ° C for 72 h, followed by cooling and filtration, drying at 60 ° C for 12 h, and then calcining at 450 ° C for 6 h to obtain mesoporous SiO2;
[0056] S2. Preparation of C / rGO double carbon coating layer: 30 mg of graphene oxide was dispersed in 30 ml of water, 1.5 g of mesoporous SiO2 was added into a reactor, and a hydrothermal reaction was carried out at 180°C for 24 h. The reaction was centrifuged, washed, and freeze-dried to obtain SiO2 / rGO. SiO2 / rGO was calcined at 650°C for 4 h in an argon gas flow containing ethanol vapor to obtain a silicon negative electrode material SiO2@C / rGO with improved cycle performance.
[0057] Comparative Example 1
[0058] SiO2 is used as the silicon negative electrode material.
[0059] The silicon negative electrode material obtained in Example 1 and Comparative Example 1 was uniformly mixed with graphite in a mass ratio of 3.6:96.4 and used as the negative electrode material. It was assembled into a lithium-ion battery with a positive electrode material, an electrolyte, and a separator, and its cycle capacity retention rate was tested. The specific test method is: the cycle capacity retention rate of the lithium-ion battery was tested at the same rate: charging at a rate of 0.5C from 2.8V to 4.35V, maintaining a constant current charge of 4.35V, and the cut-off current was 0.05C; discharging at a rate of 1C to 2.8V; this process was cycled and the capacity cycle retention rate of 200 cycles was tested. Two sets of parallel experiments were performed for Example 1 and Comparative Example 1, and the test results are shown in Tables 1 and Figure 1 .
[0060] Table 1 Capacity cycle retention rate of the battery corresponding to Example 1 and Comparative Example 1
[0061]
[0062] From Table 1 and Figure 1 It can be seen from the data that the capacity cycle retention rate of the silicon negative electrode material prepared by the present invention is about 93%, which is higher than that of the comparative example, indicating that the silicon negative electrode material prepared by the present invention helps to improve the cycle performance. In summary, the silicon negative electrode material provided by the present invention helps to improve the cycle performance.
[0063] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a silicon negative electrode material with improved cycle performance, It is characterized in that The following steps are involved: S1. Preparation of mesoporous SiO 2 : The pH regulator is dissolved in water to adjust the pH, and the organic solvent and the silicon source are added in sequence and stirred evenly to obtain a mixed solution. The mixed solution is subjected to hydrothermal treatment, crystallization, suction filtration, drying, and calcination to obtain mesoporous SiO 2 ; S2. Preparation of C / rGO dual carbon coating: Graphene oxide was dispersed in water and mesoporous SiO 2 Hydrothermal treatment, centrifugation, washing and freeze drying were performed to obtain SiO 2 / rGO, SiO 2 / rGO is calcined in an inert gas stream containing organic vapor to obtain a silicon negative electrode material SiO with improved cycle performance 2 @C / rGO.
2. The preparation method according to claim 1, It is characterized in that In the S1, the pH regulator is urea; the organic solvent is anionic and cationic surfactants; and the silicon source is tetraethyl orthosilicate.
3. The preparation method according to claim 1, It is characterized in that In the above-mentioned S1, the hydrothermal treatment crystallization includes treating at 100-120° C. for 72-96 hours.
4. The preparation method according to claim 1, It is characterized in that In the above S1, the drying comprises treating at 60-150° C. for 12-24 hours.
5. The preparation method according to claim 1, It is characterized in that In the S1, the calcination includes calcining at 450-500° C. for 6-8 hours.
6. The preparation method according to claim 1, It is characterized in that In the S2, the hydrothermal treatment includes treating at 180-200° C. for 24-36 hours.
7. The preparation method according to claim 1, It is characterized in that In the S2, the organic vapor is ethanol vapor; the inert gas is argon; and the calcination includes calcination at 600-650° C. for 2-4 hours.
8. A silicon negative electrode material with improved cycle performance, It is characterized in that The invention is prepared by the preparation method according to any one of claims 1 to 7.
Citation Information
Patent Citations
Preparation method of mesoporous hollow silicon dioxide microsphere
CN108275687A
Silicon-carbon composite material as well as preparation method and application thereof
CN113488624A
Preparation method of negative electrode material, negative electrode material and application
CN113555536A