Radial positive electrode precursor and preparation method and application thereof
By controlling the composition of the precipitant during the co-precipitation process of the positive electrode precursor of the lithium-ion battery, a radial structure of the positive electrode precursor is formed, which solves the structural stability and thermal runaway problems of the high-nickel ternary material, and improves the performance and safety of the battery , and simplified the preparation process, suitable for industrial production.
Patent Information
- Application Number
- CN202411069654.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
AI Technical Summary
The existing high-nickel ternary materials have problems such as poor structural stability, risk of thermal runaway and degradation of cycling performance in lithium-ion batteries. The preparation process of traditional core-shell structures and gradient structure materials is cumbersome and has poor repeatability, making it difficult to achieve industrialization.
By controlling the composition of precipitant agents at different stages of co-precipitation, a positive electrode precursor with a radial structure is prepared. The nucleation stage and one-step growth stage introduce carbonate to form a core, and the 2-step growth stage does not have carbonate to form a shell. Dense structure, which alleviates volume expansion and stress concentration during charging and discharging, and promotes the transmission of lithium ions.
It significantly improves the rate performance, cycle stability and safety of the battery, simplifies the preparation process, is suitable for industrial production, and shows excellent discharge capacity and cycle stability.
Smart Images

Figure CN118978192A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of battery materials and relates to a radial positive electrode precursor and a preparation method and application thereof. Background Art
[0002] As the global demand for clean energy and sustainable energy storage solutions continues to grow, lithium-ion battery technology has become the focus of research due to its high energy density, long cycle life and environmental friendliness. In this field, high-nickel ternary materials have attracted much attention due to their high specific capacity, but they also face challenges such as poor structural stability, thermal runaway risk and decreased cycle performance.
[0003] Traditional high nickel ternary materials, such as LiNi 0.8 Co 0.1 Mn 0.1 O2, although it has advantages in improving battery energy density, but in practical applications, due to the increase in nickel content, the material is prone to structural stress during the charge and discharge process, resulting in particle breakage and electrolyte decomposition, thus affecting the cycle stability and safety of the battery. In addition, high-nickel materials have poor thermal stability under high temperature conditions, increasing the risk of thermal runaway of the battery. To overcome these challenges, researchers have been exploring new material design and preparation methods. Among them, improving the performance of the material by controlling its microstructure is an effective strategy.
[0004] CN108878818A discloses a method for preparing a core-shell structured nickel-cobalt-manganese ternary positive electrode material precursor, in which a core-shell structured precursor with a high nickel core and a low nickel shell is synthesized by a co-precipitation method. However, the core-shell structure has poor cycle stability due to the mismatch in lattice constants between the inner core layer and the outer shell layer, and the anisotropic volume change during the cycle easily leads to core-shell separation and structural breakage.
[0005] CN108878869A discloses a method for preparing a gradient structured NCM ternary positive electrode material for a lithium-ion battery. The method synthesizes a ternary positive electrode material precursor with a concentration gradient by a co-precipitation method, wherein the Mn content remains constant from the center to the outer layer, the Ni content gradually decreases, and the Co content gradually increases. However, the preparation process of the gradient structured material is relatively complicated and has poor repeatability, making it difficult to realize industrialization.
[0006] The positive electrode precursor material prepared by the above scheme fails to significantly exert the high capacity characteristics of the positive electrode material, and has problems such as complicated preparation process, high cost or poor cycle stability. Therefore, it is urgent to develop a positive electrode precursor material with a new structure to solve the above technical problems. Summary of the invention
[0007] The purpose of the present invention is to provide a radial positive electrode precursor and a preparation method and application thereof. The present invention prepares a radial positive electrode precursor by controlling the precipitant composition in different stages of co-precipitation. This radial structure helps to alleviate the volume expansion during the charge and discharge process, reduce the stress concentration of the material, and promote the transmission of lithium ions, thereby comprehensively improving the rate performance, cycle stability and safety of the battery.
[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a method for preparing a radial positive electrode precursor, the preparation method comprising the following steps:
[0010] (1) injecting a mixed metal salt solution, a complexing agent solution and a first precipitant solution into a bottom liquid in parallel, and obtaining a half-step precursor through a nucleation reaction and a one-step growth reaction;
[0011] (2) replacing the first precipitant solution in step (1) with a second precipitant solution, and obtaining the radial positive electrode precursor through a two-step growth reaction;
[0012] Wherein, the solute of the first precipitant solution includes carbonate and caustic alkali, and the solute of the second precipitant solution includes caustic alkali.
[0013] The present invention improves the precipitant composition of co-precipitation to prepare a positive electrode precursor with a radial structure. The present invention introduces carbonate to participate in the co-precipitation process during the nucleation period and the one-step growth stage, which is conducive to forming a structure in which the inner core is thin, loose, porous and disorderly distributed primary grains, while the second growth stage has no carbonate participation, forming an outer shell of primary grains that are radially arranged from the inside to the outside and are relatively dense. This special structure can significantly alleviate the volume expansion during the charge and discharge process, reduce the stress concentration of the material, and promote the transmission of lithium ions, thereby comprehensively improving the rate performance, cycle stability and safety of the battery.
[0014] Preferably, the caustic comprises sodium hydroxide and / or potassium hydroxide.
[0015] Preferably, the carbonate comprises any one of sodium carbonate, potassium carbonate, ammonium carbonate, sodium bicarbonate or ammonium bicarbonate, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of sodium carbonate and potassium carbonate, a combination of potassium carbonate and ammonium carbonate, or a combination of sodium carbonate and ammonium carbonate, etc.
[0016] Preferably, the solute of the mixed metal salt solution in step (1) includes any one of nickel salt, cobalt salt or manganese salt, or a combination of at least two of them.
[0017] Preferably, the total concentration of metal ions in the mixed metal salt solution in step (1) is 1 to 3 mol / L, for example, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L or 3 mol / L, etc., not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0018] Preferably, the complexing agent solution in step (1) comprises any one of aqueous ammonia, ammonium carbonate solution, ammonium bicarbonate solution, oxalic acid solution or ethylenediaminetetraacetic acid solution, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of aqueous ammonia and ammonium carbonate solution, a combination of ammonium carbonate solution and ammonium bicarbonate solution, or a combination of oxalic acid solution and ethylenediaminetetraacetic acid solution.
[0019] Preferably, the mass concentration of the complexing agent solution in step (1) is 10-20%, for example, 10%, 12%, 15%, 18% or 20%, etc., not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0020] Preferably, the base solution in step (1) comprises caustic soda, carbonate and a complexing agent.
[0021] Preferably, the mass concentration of carbonate in the base liquid in step (1) is 2 to 8 g / L, for example, 2 g / L, 4 g / L, 5 g / L, 6 g / L or 8 g / L, etc., not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0022] Preferably, the mass concentration of the complexing agent in the base solution of step (1) is 2 to 12 g / L, for example, 2 g / L, 5 g / L, 8 g / L, 10 g / L or 12 g / L, etc., not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0023] Preferably, the pH of the base solution in step (1) is 11.2 to 12.5, for example, 11.2, 11.5, 12, 12.2 or 12.5, etc., and is not limited to the listed values. Other values not listed within the range are also applicable.
[0024] Preferably, the mass proportion of caustic soda in the first precipitant solution in step (1) is 20-40%, for example: 20%, 25%, 30%, 35% or 40%, etc., not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0025] Preferably, the mass proportion of carbonate in the first precipitant solution in step (1) is 1-10%, for example: 1%, 2%, 5%, 8% or 10%, etc., not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0026] Preferably, the pH of the nucleation reaction in step (1) is 11.3 to 12.5, for example, 11.3, 11.5, 12, 12.2 or 12.5, etc., and is not limited to the listed values. Other values not listed within the range are also applicable.
[0027] Preferably, the time of the nucleation reaction in step (1) is 2 to 6 hours, for example, 2 hours, 3 hours, 4 hours, 5 hours or 6 hours, etc., and is not limited to the listed values. Other values not listed within the numerical range are also applicable.
[0028] Preferably, the pH of the one-step growth reaction in step (1) is 9.6 to 10.6, for example, 9.6, 9.8, 10, 10.3 or 10.6, etc., and is not limited to the listed values. Other values not listed within the numerical range are also applicable.
[0029] Preferably, the mass concentration of caustic soda in the second precipitant solution in step (2) is 20-40%, for example, 20%, 25%, 30%, 35% or 40%, etc., not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0030] Preferably, the pH of the two-step growth reaction in step (2) is 10.2-11.2, for example, 10.2, 10.5, 10.8, 11 or 11.2, etc., and is not limited to the listed values. Other values not listed within the range are also applicable.
[0031] Preferably, the pH of the two-step growth reaction in step (2) - the pH of the one-step growth reaction in step (1) > 0.4.
[0032] Preferably, the median particle size D50 of the half-step precursor is a, and the median particle size D50 of the radial positive electrode precursor is b, wherein a / b = (0.2-0.7):1, for example: 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1 or 0.7:1, etc., not limited to the listed values, other unlisted values within the numerical range are also applicable, preferably (0.3-0.5):1.
[0033] Preferably, b is 5 to 16 μm, for example, 5 μm, 8 μm, 10 μm, 12 μm or 16 μm, etc., and is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0034] In a second aspect, the present invention provides a radial positive electrode precursor, which is prepared by the method described in the first aspect.
[0035] The radial positive electrode precursor of the present invention has a structure that is loose inside and dense outside, which can prevent the electrolyte from excessively contacting and corroding the internal crystal grains, and is beneficial to improving the cycle stability.
[0036] In a third aspect, the present invention provides a positive electrode material, which is prepared by mixing and sintering the radial positive electrode precursor as described in the second aspect with a lithium source.
[0037] In a fourth aspect, the present invention provides a lithium-ion battery, wherein the lithium-ion battery comprises the positive electrode material as described in the third aspect.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] (1) In the present invention, a small amount of carbonate is added to the alkaline solution in the early stage of the reaction to assist in co-precipitation. The prepared precursor has good spherical secondary particle characteristics, which are loose and disordered inside and dense and arranged in a radial structure outside. It not only helps to alleviate the volume expansion during the charge and discharge process and reduce the stress concentration of the material, but also promotes the transmission of lithium ions and avoids excessive contact between the electrolyte and the internal particles to aggravate the side reactions, thereby comprehensively improving the rate performance, cycle stability and safety of the battery.
[0040] (2) The present invention does not contain other difficult-to-handle organic or inorganic additives during the reaction process, the process operation is simple, and it is fully compatible with the existing production line and easy to carry out industrial production.
[0041] (3) The 0.1C first discharge specific capacity of the battery made of the positive electrode precursor of the present invention can reach more than 206.3mAh / g, the 1C / 0.1C capacity ratio can reach more than 90.1%, and the capacity retention rate of 1C cycle 100 weeks can reach more than 82.4%. By adjusting the content of sodium carbonate in the first precipitant solution, the 0.1C first discharge specific capacity of the battery can reach 212.3mAh / g, the 1C / 0.1C capacity ratio can reach 91.8%, and the capacity retention rate of 1C cycle 100 weeks can reach 85.7%, showing relatively excellent discharge capacity, rate performance and cycle stability, and its content will affect the internal microstructure of the precursor and thus affect its electrochemical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is a SEM image of the radial positive electrode precursor prepared in Example 1 of the present invention.
[0043] Figure 2 This is a cross-sectional SEM image of the radial positive electrode precursor prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0044] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0045] Example 1
[0046] This embodiment provides a radial positive electrode precursor, and the preparation method of the radial positive electrode precursor is as follows:
[0047] According to the molecular formula Ni 0.84 Co 0.11 Mn 0.05 (OH)2 (NCM841105) was used to prepare a mixed metal sulfate solution with a total metal ion concentration of 2 mol / L; an ammonia solution with a mass fraction of 16% was prepared; a first precipitant solution was prepared according to a mass ratio of sodium hydroxide: sodium carbonate: pure water = 32:4:64, and a second precipitant solution was prepared according to a mass ratio of sodium hydroxide: pure water = 32:68; a reaction bottom solution with a pH of 11.9-12.2, an ammonia concentration of 5.5 g / L, and a sodium carbonate mass fraction of about 5 g / L was prepared with liquid caustic soda, sodium carbonate, concentrated ammonia water and 20 L of pure water;
[0048] (1) Under the protection of nitrogen atmosphere, the prepared mixed metal sulfate solution, the first precipitant solution and the ammonia solution were added to a 50L reactor containing the bottom liquid in parallel at a uniform speed to carry out a co-precipitation reaction. The pH of the nucleation stage was controlled at 12.0±0.2 and maintained for 4 hours, and then the feed flow rate of the precipitant solution was gradually reduced so that the pH of the reaction system reached the pH of the one-step growth stage at 10 hours = 10.2±0.1. When the particle size D50 reached 6.0μm, the one-step growth reaction was stopped to obtain a half-step precursor;
[0049] (2) Switch the first precipitant solution to the second precipitant solution, increase the feed rate of the precipitant solution, gradually raise the pH of the system to pH = 10.8 ± 0.1, continue the reaction until the particle size D50 reaches 12.0 μm, stop feeding, and obtain a precursor slurry. After washing the slurry with three times of dilute sodium hydroxide solution and three times of hot pure water, bake it at 100 ° C for 12 hours to obtain a radial positive electrode precursor. The reaction temperature of the entire coprecipitation reaction is maintained at 58 ± 1 ° C, the stirring speed is 500 rpm, and the ammonia concentration is maintained at 5-6 g / L.
[0050] The SEM image of the radial positive electrode precursor is as follows Figure 1-2 As shown by Figure 1-2It can be seen that in the early stage of the reaction (nucleation period and the first growth stage), sodium hydroxide and a small amount of carbonate are added for co-precipitation, while in the later stage of the reaction, only sodium hydroxide is used as a precipitant. Combined with the adjustment of pH in the two stages, the prepared precursor has a structural characteristic of being loose and disordered inside and dense and radially arranged outside. This special radial structure helps to alleviate the volume expansion during charging and discharging, reduce the stress concentration of the material, and promote the transmission of lithium ions, thereby comprehensively improving the battery's rate performance, cycle stability and safety.
[0051] Example 2
[0052] This embodiment provides a radial positive electrode precursor, and the preparation method of the radial positive electrode precursor is as follows:
[0053] According to the molecular formula Ni 0.84 Co 0.11 Mn 0.05 (OH)2 (NCM841105) was used to prepare a mixed metal sulfate solution with a total metal ion concentration of 1 mol / L; an ammonia solution with a mass fraction of 10% was prepared; a first precipitant solution was prepared according to a mass ratio of sodium hydroxide: sodium carbonate: pure water = 20:1:79, and a second precipitant solution was prepared according to a mass ratio of sodium hydroxide: pure water = 20:80; a reaction bottom solution with a pH of 11.3-12, an ammonia concentration of 2g / L, and a sodium carbonate mass fraction of about 2g / L was prepared using liquid caustic soda, sodium carbonate, concentrated ammonia water and 20L pure water;
[0054] (1) Under the protection of nitrogen atmosphere, the prepared mixed metal sulfate solution, the first precipitant solution and the ammonia solution were added to a 50L reactor containing the bottom liquid in a uniform and parallel flow manner to carry out a co-precipitation reaction. The pH of the nucleation stage was controlled at 11.5±0.2 and maintained for 6 hours, and then the feed flow rate of the precipitant solution was gradually reduced so that the pH of the reaction system reached the pH of the one-step growth stage at 9.7±0.1 in 8 hours. When the particle size D50 reached 4.8μm, the one-step growth reaction was stopped to obtain a half-step precursor;
[0055] (2) Switch the first precipitant solution to the second precipitant solution, increase the feed rate of the precipitant solution, gradually raise the pH of the system to pH = 10.3 ± 0.1, continue the reaction until the particle size D50 reaches 16.0 μm, stop feeding, and obtain a precursor slurry. After washing the slurry with three times of dilute sodium hydroxide solution and three times of hot pure water, bake it at 100 ° C for 12 hours to obtain a radial positive electrode precursor. The reaction temperature of the entire coprecipitation reaction is maintained at 58 ± 1 ° C, the stirring speed is 500 rpm, and the ammonia concentration is maintained at 3-4 g / L.
[0056] Example 3
[0057] This embodiment provides a radial positive electrode precursor, and the preparation method of the radial positive electrode precursor is as follows:
[0058] According to the molecular formula Ni 0.84 Co 0.11 Mn 0.05 (OH)2 (NCM841105) was used to prepare a mixed metal sulfate solution with a total metal ion concentration of 3 mol / L; an ammonia solution with a mass fraction of 20% was prepared; a first precipitant solution was prepared according to a mass ratio of sodium hydroxide: sodium carbonate: pure water = 40:10:50, and a second precipitant solution was prepared according to a mass ratio of sodium hydroxide: pure water = 40:60; a reaction bottom solution with a pH of 12.3-12.5, an ammonia concentration of 12 g / L, and a sodium carbonate mass fraction of about 8 g / L was prepared using liquid caustic soda, sodium carbonate, concentrated ammonia water and 20 L of pure water;
[0059] (1) Under the protection of nitrogen atmosphere, the prepared mixed metal sulfate solution, the first precipitant solution and the ammonia solution were added to a 50L reactor containing the bottom liquid in a uniform and parallel flow manner to carry out a co-precipitation reaction. The pH of the nucleation stage was controlled at 12.3±0.2 and maintained for 6 hours, and then the feed flow rate of the precipitant solution was gradually reduced so that the pH of the reaction system reached the pH of the one-step growth stage at 10.5±0.1 in 8 hours. When the particle size D50 reached 2.5μm, the one-step growth reaction was stopped to obtain a half-step precursor;
[0060] (2) Switch the first precipitant solution to the second precipitant solution, increase the feed rate of the precipitant solution, gradually raise the pH of the system to pH = 11.1 ± 0.1, continue the reaction until the particle size D50 reaches 5 μm, stop feeding, and obtain a precursor slurry. After washing the slurry with three times of dilute sodium hydroxide solution and three times of hot pure water, bake it at 100 ° C for 12 hours to obtain a radial positive electrode precursor. The reaction temperature of the entire coprecipitation reaction is maintained at 58 ± 1 ° C, the stirring speed is 500 rpm, and the ammonia concentration is maintained at 9-10 g / L.
[0061] Example 4
[0062] The only difference between this embodiment and embodiment 1 is that the mass proportion of carbonate in the first precipitant solution is 0.5%, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0063] Example 5
[0064] The only difference between this embodiment and embodiment 1 is that the mass proportion of carbonate in the first precipitant solution is 12%, and other conditions and parameters are exactly the same as those in embodiment 1.
[0065] Example 6
[0066] The only difference between this embodiment and embodiment 1 is that the pH value of the first growth stage in step (1) is 10.6, and the pH value of the second growth stage in step (2) is 10.9. The other conditions and parameters are exactly the same as those in embodiment 1.
[0067] Example 7
[0068] The only difference between this embodiment and embodiment 1 is that the D50 of the half-step precursor obtained in step (1) is 2 μm, and the D50 of the particles of the radial positive electrode precursor in step (2) is 10 μm. Other conditions and parameters are exactly the same as those in embodiment 1.
[0069] Example 8
[0070] The only difference between this embodiment and embodiment 1 is that the D50 of the half-step precursor obtained in step (1) is 7 μm, and the D50 of the particles of the radial positive electrode precursor in step (2) is 10 μm. Other conditions and parameters are exactly the same as those in embodiment 1.
[0071] Comparative Example 1
[0072] The only difference between this comparative example and Example 1 is that sodium carbonate is not added in step (1), and the other conditions and parameters are exactly the same as those in Example 1.
[0073] Comparative Example 2
[0074] The only difference between this comparative example and Example 1 is that step (1) uses sodium hydroxide solution as the precipitant, and step (2) uses sodium carbonate solution as the precipitant. Other conditions and parameters are exactly the same as those in Example 1.
[0075] Comparative Example 3
[0076] The difference between this comparative example and Example 1 is that the pH of the first growth stage in step (1) is equal to the pH of the second growth stage in step (2) = 10.5, and the other conditions and parameters are exactly the same as those in Example 1.
[0077] Performance Test:
[0078] The nickel-cobalt-manganese ternary precursor material obtained in the above examples and comparative examples was evenly mixed with lithium hydroxide according to a lithium ratio of Li / TM=1.05, and then sintered at 820°C for 18 hours to obtain a nickel-cobalt-manganese-oxide lithium positive electrode material, and assembled into a button cell for electrochemical performance testing. The specific experimental steps are as follows: First, the active material (sintered lithium cobalt-manganese-oxide positive electrode material), conductive agent acetylene black, and binder polyvinylidene fluoride were dissolved in N-methylpyrrolidone at a mass ratio of 8:1:1, and the slurry was mixed using a homogenizer in a multi-stage mode at room temperature; then, the ground slurry was evenly applied to the aluminum foil with a coater, and dried at 80°C in a vacuum drying oven for 12 hours; finally, the aluminum foil was punched into 1.13 cm 2Circular electrode sheet.
[0079] The obtained electrode sheet was used as the positive electrode, the lithium metal sheet was used as the counter electrode, and the porous polypropylene membrane (Celgard2400, USA) was used as the separator to separate the positive electrode and the counter electrode. The CR-2032 battery was assembled in a glove box filled with Ar gas. The battery was tested using a battery test system (Blue Electric CT2001A, Wuhan, China). First, it was activated three times at 0.1C rate / 2.7~4.3V, and then the activated button cell was tested for electrochemical performance under 2.7-4.3V@0.1C / 1C conditions. The test results are shown in Table 1:
[0080] Table 1
[0081]
[0082] As can be seen from Table 1, from Examples 1-3, the 0.1C first discharge specific capacity of the battery made from the positive electrode precursor of the present invention can reach more than 206.3mAh / g, the 1C / 0.1C capacity ratio can reach more than 90.1%, and the 1C cycle 100-week capacity retention rate can reach more than 82.4%. By adjusting the content of sodium carbonate in the first precipitant solution, the 0.1C first discharge specific capacity of the obtained battery can reach 212.3mAh / g, the 1C / 0.1C capacity ratio can reach 91.8%, and the 1C cycle 100-week capacity retention rate can reach 85.7%, showing relatively excellent discharge capacity, rate performance and cycle stability, and its content will affect the internal microstructure of the precursor and thus affect its electrochemical properties.
[0083] By comparing Example 1 with Examples 4-5, it can be seen that in the preparation process of the radial positive electrode precursor of the present invention, the mass proportion of carbonate in the first precipitant solution will affect its performance. When the mass proportion of carbonate in the first precipitant solution is controlled at 1-10%, the performance of the radial positive electrode precursor is better. If the mass proportion of carbonate in the first precipitant solution is too high, more carbonate precursors will be formed, which is not conducive to the uniformity of the structure and affects the material performance; if the mass proportion of carbonate in the first precipitant solution is too low, an effective structure with high porosity and disordered distribution of primary grains cannot be formed, which reduces the effect of improving stress concentration and preventing cracking, and also affects the cycle stability.
[0084] By comparing Example 1 and Example 6, it can be seen that in the preparation process of the radial positive electrode precursor of the present invention, the relationship between the pH of the one-step growth stage of step (1) and the pH of the two-step growth stage of step (2) will affect its performance. By controlling the pH of the two-step growth stage of step (2) to be at least 0.4 greater than the pH of the one-step growth stage of step (1), the performance of the radial positive electrode precursor is better. If the difference between the two is too small, it is not conducive to forming an external dense structure, and it cannot effectively prevent the electrolyte from corroding the internal grains during the charge and discharge process, thereby aggravating the side reactions and affecting the cycle stability.
[0085] By comparing Example 1 with Examples 7-8, it can be seen that in the preparation process of the radial positive electrode precursor of the present invention, the relationship between the median particle size D50 of the half-step precursor obtained in step (1) and the radial precursor obtained in step (2) will affect its performance. The median particle size D50 of the half-step precursor is a, and the median particle size D50 of the radial positive electrode precursor is b. When a / b is controlled at (0.3-0.5):1, the performance of the radial positive electrode precursor is better. If a / b is too large, the precursor is easily formed into a hollow structure and ruptured when sintered into a positive electrode material, which is not conducive to the improvement of the compaction density of the material, thereby affecting the cycle performance and capacity; if a / b is too small, it cannot play a good role in improving the volume expansion and stress concentration during the charge and discharge process, and will also affect its cycle stability.
[0086] By comparing Example 1 and Comparative Example 1, it can be seen that the present invention introduces carbonates to participate in the co-precipitation process during the nucleation period and the one-step growth stage, which is conducive to forming a structure in which the inner core is thin, loose, porous and disorderly distributed primary grains, while there is no carbonate participation in the second growth stage, forming an outer shell in which the primary grains are radially arranged from the inside to the outside and are relatively dense. This special structure can significantly alleviate the volume expansion during the charge and discharge process, reduce the stress concentration of the material, and promote the transmission of lithium ions, avoiding excessive contact between the electrolyte and the internal particles and aggravating side reactions, thereby comprehensively improving the battery's rate performance, cycle stability and safety.
[0087] By comparing Example 1 and Comparative Example 2, it can be seen that the first precipitant solution is a sodium hydroxide solution and the second precipitant solution is a sodium carbonate solution, and the precursor will form a microstructure that is dense inside and loose outside, which will intensify the side reactions caused by the contact between the electrolyte and the active material during the charge and discharge process, thereby resulting in a significant decrease in the cycle stability.
[0088] By comparing Example 1 and Comparative Example 3, it can be seen that the pH of the one-step growth stage in step (1) and the two-step growth stage in step (2) are equal and relatively low, forming a relatively loose internal structure, which will aggravate the side reactions caused by the contact between the electrolyte and the active material during the charge and discharge process, thereby resulting in a decrease in the cycle stability.
[0089] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a radial positive electrode precursor, characterized in that: The preparation method comprises the following steps: (1) injecting a mixed metal salt solution, a complexing agent solution and a first precipitant solution into a bottom liquid in parallel, and obtaining a half-step precursor through a nucleation reaction and a one-step growth reaction; (2) replacing the first precipitant solution in step (1) with a second precipitant solution, and obtaining the radial positive electrode precursor through a two-step growth reaction; Wherein, the solute of the first precipitant solution includes carbonate and caustic alkali, and the solute of the second precipitant solution includes caustic alkali.
2. The preparation method according to claim 1, characterized in that The caustic alkali includes sodium hydroxide and / or potassium hydroxide; Preferably, the carbonate includes any one of sodium carbonate, potassium carbonate, ammonium carbonate, sodium bicarbonate or ammonium bicarbonate, or a combination of at least two thereof.
3. The preparation method according to claim 1 or 2, characterized in that: The solute of the mixed metal salt solution in step (1) includes any one of nickel salt, cobalt salt or manganese salt, or a combination of at least two thereof; Preferably, the total concentration of metal ions in the mixed metal salt solution in step (1) is 1 to 3 mol / L; Preferably, the complexing agent solution in step (1) comprises any one of ammonia water, ammonium carbonate solution, ammonium bicarbonate solution, oxalic acid solution or ethylenediaminetetraacetic acid solution, or a combination of at least two thereof; Preferably, the mass concentration of the complexing agent solution in step (1) is 10-20%; Preferably, the base solution in step (1) comprises caustic soda, carbonate and a complexing agent; Preferably, the mass concentration of carbonate in the base solution in step (1) is 2 to 8 g / L; Preferably, the mass concentration of the complexing agent in the base solution of step (1) is 2 to 12 g / L; Preferably, the pH of the base solution in step (1) is 11.2 to 12.5; Preferably, in step (1), the mass percentage of caustic soda in the first precipitant solution is 20-40%; Preferably, in step (1), the mass proportion of carbonate in the first precipitant solution is 1-10%.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The pH of the nucleation reaction in step (1) is 11.3 to 12.5; Preferably, the nucleation reaction time in step (1) is 2 to 6 hours; Preferably, the pH of the one-step growth reaction in step (1) is 9.6 to 10.
6.
5. The preparation method according to any one of claims 1 to 4, characterized in that: Step (2) The mass concentration of caustic soda in the second precipitant solution is 20-40%.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The pH of the two-step growth reaction in step (2) is 10.2 to 11.2; Preferably, the pH of the two-step growth reaction in step (2) - the pH of the one-step growth reaction in step (1) > 0.
4.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The median particle size D50 of the half-step precursor is a, and the median particle size D50 of the radial positive electrode precursor is b, wherein a / b=(0.2-0.7):1, preferably (0.3-0.5):1; Preferably, b is 5 to 16 μm.
8. A radial positive electrode precursor, characterized in that: The radial positive electrode precursor is prepared by the method according to any one of claims 1 to 7.
9. A positive electrode material, characterized in that: The positive electrode material is prepared by mixing and sintering the radial positive electrode precursor as claimed in claim 8 and a lithium source.
10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the positive electrode material according to claim 9.
Citation Information
Cited By
High-crystallinity hollow positive electrode precursor and preparation method and application thereof
CN119430316A