Scale inhibitor and preparation method thereof

By using scale inhibitors with sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate and other components, the existing scale inhibitors pollute the environment and eutrophication of water bodies is solved, and environmentally friendly scale inhibition effect is achieved to avoid Ecological damage to water bodies.

CN118978269APending Publication Date: 2024-11-19BEIJING LEWEN SCI & TECH DEV CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310690934.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-12
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing scale inhibitors are mainly phosphorus-based or polymers, which are prone to breed bacteria and algae and pollute the environment, and silicon-based scale inhibitors are prone to scale. Overuse of organic phosphorus or inorganic phosphorus scale inhibitors will lead to eutrophication of water and damage the ecology. balance.

Method used

The scale inhibitor consisting of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidants, chitinamine and organic corrosion inhibitors is used to form an environmentally friendly scale inhibitor through specific proportions and preparation methods. Avoid breeding algae and scaling, and prevent the water from eutrophication.

Benefits of technology

Effectively prevent scale inhibitors from breeding bacterial algae, polluting the environment and scaling, reducing negative impacts on the environment, solving the problems of eutrophication and ecological balance of water bodies, and making scale inhibitors more environmentally friendly.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a flame retardant and a preparation method thereof, and the preparation method comprises the following steps: a scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, an antioxidant, chitosan, an organic corrosion inhibitor and water; the corrosion inhibitor comprises the following components in parts by weight: 4-9 parts of sodium hydroxide, 6-15 parts of potassium hydroxide, 15-19 parts of alkyl epoxy carboxylate, 5-9 parts of oleoyl chloride, 2-6 parts of antioxidant, 6-10 parts of chitosan, 6-10 parts of organic corrosion inhibitor and 27-31 parts of water. The scale inhibitor is prepared from the sodium hydroxide, the potassium hydroxide, the alkyl epoxy carboxylate, the antioxidant, the chitosan, the organic corrosion inhibitor and the water, can be used instead of a phosphorus or polymer-based corrosion and scale inhibitor, and can effectively prevent the scale inhibitor from breeding bacteria and algae, polluting the environment and scaling; and meanwhile, the conditions of eutrophication of a water body and destroy of ecological balance of the water body caused by excessive use can be prevented, so that the use of the blocking agent is more environment-friendly, and the negative influence on the environment is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of scale inhibitors, in particular to a scale inhibitor and a preparation method thereof. Background Art

[0002] Scale inhibitors are a type of agent that can disperse insoluble inorganic salts in water, prevent or interfere with the precipitation and scaling of insoluble inorganic salts on metal surfaces, and maintain good heat transfer effects on metal equipment. Scale inhibitors can remove scale and prevent the formation of scale, improve heat exchange efficiency, reduce electricity or fuel consumption, and water treatment can also reduce sewage discharge and improve water utilization, generally saving more than 60%;

[0003] With the increase in the amount of water produced in oil fields, scaling of oil field water is an inevitable problem in oil field production. Scaling is extremely harmful to oil fields. Scale is deposited in the oil production and gathering and transportation systems, which will not only increase the resistance to fluid flow, thereby increasing energy consumption, but also cause under-scale corrosion, affecting normal production. In addition, scale deposition in formation water will also cause problems such as pore blockage. Therefore, scaling is becoming an urgent problem that needs to be solved in oil fields. Existing scale inhibitors are mainly phosphorus-based or polymer-based corrosion and scale inhibitors. However, phosphorus-based scale inhibitors are prone to breed bacteria and algae and pollute the environment, and silicon-based scale inhibitors are prone to scaling. In addition, excessive use of organic phosphorus or inorganic phosphorus scale inhibitors will lead to eutrophication of water bodies and destroy the ecological balance of water bodies. Summary of the invention

[0004] The purpose of the present invention is to provide a scale inhibitor and a preparation method thereof, which have the advantage of environmental protection and solve the problem that the existing scale inhibitors are mainly phosphorus-based or polymer-based corrosion inhibitors, but phosphorus-based scale inhibitors are easy to breed bacteria and algae and pollute the environment, and silicon-based scale inhibitors are easy to scale. In addition, excessive use of organic phosphorus or inorganic phosphorus scale inhibitors will lead to eutrophication of water bodies and destroy the ecological balance of water bodies.

[0005] To achieve the above purpose, the present invention provides the following technical solution: a scale inhibitor, which consists of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and its ratio is: 4-9 parts of sodium hydroxide, 6-15 parts of potassium hydroxide, 15-19 parts of alkyl epoxy carboxylate, 5-9 parts of oleoyl chloride, 2-6 parts of antioxidant, 6-10 parts of chitosan, 6-10 parts of organic corrosion inhibitor and 27-31 parts of water.

[0006] Preferably, the scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and its ratio is: 4 parts of sodium hydroxide, 6 parts of potassium hydroxide, 15 parts of alkyl epoxy carboxylate, 5 parts of oleoyl chloride, 2 parts of antioxidant, 6 parts of chitosan, 6 parts of organic corrosion inhibitor and 27 parts of water.

[0007] Preferably, the scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and its ratio is: 5 parts of sodium hydroxide, 8 parts of potassium hydroxide, 16 parts of alkyl epoxy carboxylate, 6 parts of oleoyl chloride, 3 parts of antioxidant, 7 parts of chitosan, 7 parts of organic corrosion inhibitor and 28 parts of water.

[0008] Preferably, the scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and its ratio is: 6 parts of sodium hydroxide, 11 parts of potassium hydroxide, 17 parts of alkyl epoxy carboxylate, 7 parts of oleoyl chloride, 4 parts of antioxidant, 8 parts of chitosan, 8 parts of organic corrosion inhibitor and 29 parts of water.

[0009] Preferably, the scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and its ratio is: 7 parts of sodium hydroxide, 13 parts of potassium hydroxide, 18 parts of alkyl epoxy carboxylate, 8 parts of oleoyl chloride, 5 parts of antioxidant, 9 parts of chitosan, 9 parts of organic corrosion inhibitor and 30 parts of water.

[0010] Preferably, the scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and its ratio is: 8 parts of sodium hydroxide, 15 parts of potassium hydroxide, 19 parts of alkyl epoxy carboxylate, 9 parts of oleoyl chloride, 6 parts of antioxidant, 10 parts of chitosan, 10 parts of organic corrosion inhibitor and 31 parts of water.

[0011] Preferably, the preparation method comprises the following steps:

[0012] A. Purchase sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan and organic corrosion inhibitor in proportion;

[0013] B. Add sodium hydroxide, potassium hydroxide and water into a blender and stir;

[0014] C. Sodium hydroxide and potassium hydroxide are dissolved in water and stirred to produce inorganic alkali;

[0015] D. Continue stirring and add alkyl epoxy carboxylate while stirring;

[0016] E. After the alkyl epoxy carboxylate is completely dissolved, chitosan, organic corrosion inhibitor and oleoyl chloride are added;

[0017] F. Add water again and stir thoroughly to obtain the scale inhibitor;

[0018] G. Using a packaging machine to seal and package the scale inhibitor obtained in step F.

[0019] Preferably, in the steps B, D, E and F, when the sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan and organic corrosion inhibitor are uniformly stirred, an agitator is required, and the rotation speed is 220 rpm.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The scale inhibitor prepared by the present invention is prepared by using sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water. The scale inhibitor can replace the corrosion and scale inhibitor mainly based on phosphorus or polymer, and can effectively prevent the scale inhibitor from breeding bacteria and algae, polluting the environment and scaling. At the same time, it can also prevent the eutrophication of water bodies and the destruction of the ecological balance of water bodies due to excessive use, so that the use of the scale inhibitor is more environmentally friendly and reduces the negative impact on the environment. The existing scale inhibitor is mainly a corrosion and scale inhibitor mainly based on phosphorus or polymer, but the phosphorus scale inhibitor is easy to breed bacteria and algae and pollute the environment, and the silicon scale inhibitor is easy to scale. In addition, excessive use of organic phosphorus or inorganic phosphorus scale inhibitors will lead to eutrophication of water bodies and destroy the ecological balance of water bodies. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0023] The present invention provides a technical solution:

[0024] A scale inhibitor consists of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and the proportion is: 4-9 parts of sodium hydroxide, 6-15 parts of potassium hydroxide, 15-19 parts of alkyl epoxy carboxylate, 5-9 parts of oleoyl chloride, 2-6 parts of antioxidant, 6-10 parts of chitosan, 6-10 parts of organic corrosion inhibitor and 27-31 parts of water.

[0025] The scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and its proportion is: 4 parts of sodium hydroxide, 6 parts of potassium hydroxide, 15 parts of alkyl epoxy carboxylate, 5 parts of oleoyl chloride, 2 parts of antioxidant, 6 parts of chitosan, 6 parts of organic corrosion inhibitor and 27 parts of water.

[0026] The scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and its proportion is: 5 parts of sodium hydroxide, 8 parts of potassium hydroxide, 16 parts of alkyl epoxy carboxylate, 6 parts of oleoyl chloride, 3 parts of antioxidant, 7 parts of chitosan, 7 parts of organic corrosion inhibitor and 28 parts of water.

[0027] The scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and its proportion is: 6 parts of sodium hydroxide, 11 parts of potassium hydroxide, 17 parts of alkyl epoxy carboxylate, 7 parts of oleoyl chloride, 4 parts of antioxidant, 8 parts of chitosan, 8 parts of organic corrosion inhibitor and 29 parts of water.

[0028] The scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and the proportion is: 7 parts of sodium hydroxide, 13 parts of potassium hydroxide, 18 parts of alkyl epoxy carboxylate, 8 parts of oleoyl chloride, 5 parts of antioxidant, 9 parts of chitosan, 9 parts of organic corrosion inhibitor and 30 parts of water.

[0029] The scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and its proportion is: 8 parts of sodium hydroxide, 15 parts of potassium hydroxide, 19 parts of alkyl epoxy carboxylate, 9 parts of oleyl chloride, 6 parts of antioxidant, 10 parts of chitosan, 10 parts of organic corrosion inhibitor and 31 parts of water.

[0030] The preparation method comprises the following steps:

[0031] A. Purchase sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan and organic corrosion inhibitor in proportion;

[0032] B. Add sodium hydroxide, potassium hydroxide and water into a blender and stir;

[0033] C. Sodium hydroxide and potassium hydroxide are dissolved in water and stirred to produce inorganic alkali;

[0034] D. Continue stirring and add alkyl epoxy carboxylate while stirring;

[0035] E. After the alkyl epoxy carboxylate is completely dissolved, chitosan, organic corrosion inhibitor and oleoyl chloride are added;

[0036] F. Add water again and stir thoroughly to obtain the scale inhibitor;

[0037] G. Using a packaging machine to seal and package the scale inhibitor obtained in step F.

[0038] Embodiment 1:

[0039] The scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and its proportion is: 4 parts of sodium hydroxide, 6 parts of potassium hydroxide, 15 parts of alkyl epoxy carboxylate, 5 parts of oleoyl chloride, 2 parts of antioxidant, 6 parts of chitosan, 6 parts of organic corrosion inhibitor and 27 parts of water.

[0040] Its preparation comprises the following steps:

[0041] A. Purchase sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan and organic corrosion inhibitor in proportion;

[0042] B. Add sodium hydroxide, potassium hydroxide and water into a blender and stir;

[0043] C. Sodium hydroxide and potassium hydroxide are dissolved in water and stirred to produce inorganic alkali;

[0044] D. Continue stirring and add alkyl epoxy carboxylate while stirring;

[0045] E. After the alkyl epoxy carboxylate is completely dissolved, chitosan, organic corrosion inhibitor and oleoyl chloride are added;

[0046] F. Add water again and stir thoroughly to obtain the scale inhibitor;

[0047] G. Using a packaging machine to seal and package the scale inhibitor obtained in step F.

[0048] The scale inhibitor prepared by the present invention is prepared by using sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water. The scale inhibitor can replace the corrosion and scale inhibitor mainly based on phosphorus or polymer, and can effectively prevent the scale inhibitor from breeding bacteria and algae, polluting the environment and scaling. At the same time, it can also prevent the eutrophication of water bodies and the destruction of the ecological balance of water bodies due to excessive use, so that the use of the scale inhibitor is more environmentally friendly and reduces the negative impact on the environment. The existing scale inhibitor is mainly a corrosion and scale inhibitor mainly based on phosphorus or polymer, but the phosphorus scale inhibitor is easy to breed bacteria and algae and pollute the environment, and the silicon scale inhibitor is easy to scale. In addition, excessive use of organic phosphorus or inorganic phosphorus scale inhibitors will lead to eutrophication of water bodies and destroy the ecological balance of water bodies.

[0049] Embodiment 2:

[0050] In the first embodiment, the following steps are added:

[0051] The scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and its proportion is: 5 parts of sodium hydroxide, 8 parts of potassium hydroxide, 16 parts of alkyl epoxy carboxylate, 6 parts of oleoyl chloride, 3 parts of antioxidant, 7 parts of chitosan, 7 parts of organic corrosion inhibitor and 28 parts of water.

[0052] Its preparation comprises the following steps:

[0053] A. Purchase sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan and organic corrosion inhibitor in proportion;

[0054] B. Add sodium hydroxide, potassium hydroxide and water into a blender and stir;

[0055] C. Sodium hydroxide and potassium hydroxide are dissolved in water and stirred to produce inorganic alkali;

[0056] D. Continue stirring and add alkyl epoxy carboxylate while stirring;

[0057] E. After the alkyl epoxy carboxylate is completely dissolved, chitosan, organic corrosion inhibitor and oleoyl chloride are added;

[0058] F. Add water again and stir thoroughly to obtain the scale inhibitor;

[0059] G. Using a packaging machine to seal and package the scale inhibitor obtained in step F.

[0060] The scale inhibitor prepared by the present invention is prepared by using sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water. The scale inhibitor can replace the corrosion and scale inhibitor mainly based on phosphorus or polymer, and can effectively prevent the scale inhibitor from breeding bacteria and algae, polluting the environment and scaling. At the same time, it can also prevent the eutrophication of water bodies and the destruction of the ecological balance of water bodies due to excessive use, so that the use of the scale inhibitor is more environmentally friendly and reduces the negative impact on the environment. The existing scale inhibitor is mainly a corrosion and scale inhibitor mainly based on phosphorus or polymer, but the phosphorus scale inhibitor is easy to breed bacteria and algae and pollute the environment, and the silicon scale inhibitor is easy to scale. In addition, excessive use of organic phosphorus or inorganic phosphorus scale inhibitors will lead to eutrophication of water bodies and destroy the ecological balance of water bodies.

[0061] Embodiment three:

[0062] In the second embodiment, the following steps are added:

[0063] The scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and its proportion is: 6 parts of sodium hydroxide, 11 parts of potassium hydroxide, 17 parts of alkyl epoxy carboxylate, 7 parts of oleoyl chloride, 4 parts of antioxidant, 8 parts of chitosan, 8 parts of organic corrosion inhibitor and 29 parts of water.

[0064] Its preparation comprises the following steps:

[0065] A. Purchase sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan and organic corrosion inhibitor in proportion;

[0066] B. Add sodium hydroxide, potassium hydroxide and water into a blender and stir;

[0067] C. Sodium hydroxide and potassium hydroxide are dissolved in water and stirred to produce inorganic alkali;

[0068] D. Continue stirring and add alkyl epoxy carboxylate while stirring;

[0069] E. After the alkyl epoxy carboxylate is completely dissolved, chitosan, organic corrosion inhibitor and oleoyl chloride are added;

[0070] F. Add water again and stir thoroughly to obtain the scale inhibitor;

[0071] G. Using a packaging machine to seal and package the scale inhibitor obtained in step F.

[0072] The scale inhibitor prepared by the present invention is prepared by using sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water. The scale inhibitor can replace the corrosion and scale inhibitor mainly based on phosphorus or polymer, and can effectively prevent the scale inhibitor from breeding bacteria and algae, polluting the environment and scaling. At the same time, it can also prevent the eutrophication of water bodies and the destruction of the ecological balance of water bodies due to excessive use, so that the use of the scale inhibitor is more environmentally friendly and reduces the negative impact on the environment. The existing scale inhibitor is mainly a corrosion and scale inhibitor mainly based on phosphorus or polymer, but the phosphorus scale inhibitor is easy to breed bacteria and algae and pollute the environment, and the silicon scale inhibitor is easy to scale. In addition, excessive use of organic phosphorus or inorganic phosphorus scale inhibitors will lead to eutrophication of water bodies and destroy the ecological balance of water bodies.

[0073] Embodiment 4:

[0074] In the third embodiment, the following steps are added:

[0075] The scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and the proportion is: 7 parts of sodium hydroxide, 13 parts of potassium hydroxide, 18 parts of alkyl epoxy carboxylate, 8 parts of oleoyl chloride, 5 parts of antioxidant, 9 parts of chitosan, 9 parts of organic corrosion inhibitor and 30 parts of water.

[0076] Its preparation comprises the following steps:

[0077] A. Purchase sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan and organic corrosion inhibitor in proportion;

[0078] B. Add sodium hydroxide, potassium hydroxide and water into a blender and stir;

[0079] C. Sodium hydroxide and potassium hydroxide are dissolved in water and stirred to produce inorganic alkali;

[0080] D. Continue stirring and add alkyl epoxy carboxylate while stirring;

[0081] E. After the alkyl epoxy carboxylate is completely dissolved, chitosan, organic corrosion inhibitor and oleoyl chloride are added;

[0082] F. Add water again and stir thoroughly to obtain the scale inhibitor;

[0083] G. Using a packaging machine to seal and package the scale inhibitor obtained in step F.

[0084] The scale inhibitor prepared by the present invention is prepared by using sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water. The scale inhibitor can replace the corrosion and scale inhibitor mainly based on phosphorus or polymer, and can effectively prevent the scale inhibitor from breeding bacteria and algae, polluting the environment and scaling. At the same time, it can also prevent the eutrophication of water bodies and the destruction of the ecological balance of water bodies due to excessive use, so that the use of the scale inhibitor is more environmentally friendly and reduces the negative impact on the environment. The existing scale inhibitor is mainly a corrosion and scale inhibitor mainly based on phosphorus or polymer, but the phosphorus scale inhibitor is easy to breed bacteria and algae and pollute the environment, and the silicon scale inhibitor is easy to scale. In addition, excessive use of organic phosphorus or inorganic phosphorus scale inhibitors will lead to eutrophication of water bodies and destroy the ecological balance of water bodies.

[0085] Embodiment five:

[0086] In the fourth embodiment, the following steps are added:

[0087] The scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and its proportion is: 8 parts of sodium hydroxide, 15 parts of potassium hydroxide, 19 parts of alkyl epoxy carboxylate, 9 parts of oleyl chloride, 6 parts of antioxidant, 10 parts of chitosan, 10 parts of organic corrosion inhibitor and 31 parts of water.

[0088] Its preparation comprises the following steps:

[0089] A. Purchase sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan and organic corrosion inhibitor in proportion;

[0090] B. Add sodium hydroxide, potassium hydroxide and water into a blender and stir;

[0091] C. Sodium hydroxide and potassium hydroxide are dissolved in water and stirred to produce inorganic alkali;

[0092] D. Continue stirring and add alkyl epoxy carboxylate while stirring;

[0093] E. After the alkyl epoxy carboxylate is completely dissolved, chitosan, organic corrosion inhibitor and oleoyl chloride are added;

[0094] F. Add water again and stir thoroughly to obtain the scale inhibitor;

[0095] G. Using a packaging machine to seal and package the scale inhibitor obtained in step F.

[0096] The scale inhibitor prepared by the present invention is prepared by using sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water. The scale inhibitor can replace the corrosion and scale inhibitor mainly based on phosphorus or polymer, and can effectively prevent the scale inhibitor from breeding bacteria and algae, polluting the environment and scaling. At the same time, it can also prevent the eutrophication of water bodies and the destruction of the ecological balance of water bodies due to excessive use, so that the use of the scale inhibitor is more environmentally friendly and reduces the negative impact on the environment. The existing scale inhibitor is mainly a corrosion and scale inhibitor mainly based on phosphorus or polymer, but the phosphorus scale inhibitor is easy to breed bacteria and algae and pollute the environment, and the silicon scale inhibitor is easy to scale. In addition, excessive use of organic phosphorus or inorganic phosphorus scale inhibitors will lead to eutrophication of water bodies and destroy the ecological balance of water bodies.

[0097] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0098] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A scale inhibitor, Features: The scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and its proportion is: 4-9 parts of sodium hydroxide, 6-15 parts of potassium hydroxide, 15-19 parts of alkyl epoxy carboxylate, 5-9 parts of oleoyl chloride, 2-6 parts of antioxidant, 6-10 parts of chitosan, 6-10 parts of organic corrosion inhibitor and 27-31 parts of water.

2. A scale inhibitor according to claim 1, Features: The scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and its proportion is: 4 parts of sodium hydroxide, 6 parts of potassium hydroxide, 15 parts of alkyl epoxy carboxylate, 5 parts of oleoyl chloride, 2 parts of antioxidant, 6 parts of chitosan, 6 parts of organic corrosion inhibitor and 27 parts of water.

3. A scale inhibitor according to claim 1, Features: The scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and its proportion is: 5 parts of sodium hydroxide, 8 parts of potassium hydroxide, 16 parts of alkyl epoxy carboxylate, 6 parts of oleoyl chloride, 3 parts of antioxidant, 7 parts of chitosan, 7 parts of organic corrosion inhibitor and 28 parts of water.

4. The scale inhibitor according to claim 1, Features: The scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and its proportion is: 6 parts of sodium hydroxide, 11 parts of potassium hydroxide, 17 parts of alkyl epoxy carboxylate, 7 parts of oleoyl chloride, 4 parts of antioxidant, 8 parts of chitosan, 8 parts of organic corrosion inhibitor and 29 parts of water.

5. The scale inhibitor according to claim 1, Features: The scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and the proportion is: 7 parts of sodium hydroxide, 13 parts of potassium hydroxide, 18 parts of alkyl epoxy carboxylate, 8 parts of oleoyl chloride, 5 parts of antioxidant, 9 parts of chitosan, 9 parts of organic corrosion inhibitor and 30 parts of water.

6. The scale inhibitor according to claim 1, Features: The scale inhibitor is composed of sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan, organic corrosion inhibitor and water, and its proportion is: 8 parts of sodium hydroxide, 15 parts of potassium hydroxide, 19 parts of alkyl epoxy carboxylate, 9 parts of oleyl chloride, 6 parts of antioxidant, 10 parts of chitosan, 10 parts of organic corrosion inhibitor and 31 parts of water.

7. A method for preparing a scale inhibitor according to any one of claims 1 to 6, Features: The preparation method comprises the following steps: A. Purchase sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan and organic corrosion inhibitor in proportion; B. Add sodium hydroxide, potassium hydroxide and water into a blender and stir; C. Sodium hydroxide and potassium hydroxide are dissolved in water and stirred to produce inorganic alkali; D. Continue stirring and add alkyl epoxy carboxylate while stirring; E. After the alkyl epoxy carboxylate is completely dissolved, chitosan, organic corrosion inhibitor and oleoyl chloride are added; F. Add water again and stir thoroughly to obtain the scale inhibitor; G. Using a packaging machine to seal and package the scale inhibitor obtained in step F.

8. The method for preparing a scale inhibitor according to claim 7, Features: In the steps B, D, E and F, when the sodium hydroxide, potassium hydroxide, alkyl epoxy carboxylate, antioxidant, chitosan and organic corrosion inhibitor are uniformly stirred, an agitator is required, and the rotation speed is 220 rpm.

Citation Information

Patent Citations

  • Water treatment corrosion inhibitor and water treatment agent containing same

    CN103172183A

  • Efficient environment-friendly scale inhibitor and preparation method thereof

    CN105668813A

  • Corrosion and scale inhibitor

    CN111472007A

  • Corrosion-and scaling-inhibiting water treating agent

    CN1435384A

  • Scale Inhibitor and Methods of Using Scale Inhibitors

    US20170114272A1