Preparation process of heat insulation interlayer hollow glass

Through semi-temperature treatment and hot-pressed thermal insulation interlayer technology, combined with silicone sol and ultraviolet absorber, the impact resistance, airtightness and flame retardant of hollow glass are solved, and efficient thermal insulation and ultraviolet partitioning effects are achieved.

CN118978347AActive Publication Date: 2024-11-19西藏金宏泰科技有限公司

Patent Information

Application Number
CN202411064237.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

The existing hollow glass has poor impact strength, insufficient airtightness, no flame retardant and ultraviolet partitioning properties, and the nano-transparent heat insulation layer is easily affected by light.

Method used

A semi-tempered glass substrate is used and a thermally insulated interlayer is hot-pressed on its surface, including silicone sol and ultraviolet absorber, and is autoclaved by a hot press to form a sealed hollow glass cavity and is placed on the glass sheet. Interstitial gas is filled with.

Benefits of technology

It improves the impact strength and airtightness of hollow glass, has flame retardant and ultraviolet partitioning properties, extends service life, and improves thermal insulation performance and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978347A_ABST
    Figure CN118978347A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of hollow glass, in particular to a preparation process of heat insulation interlayer hollow glass. The preparation method comprises the following steps: cutting, edging, cleaning and drying a glass substrate, then carrying out semi-toughening treatment to obtain a toughened glass sheet, carrying out hot-pressing on the two surfaces of the toughened glass sheet with heat-insulating interlayers, pushing the toughened glass sheet into a dustproof chamber, carrying out lamination and lamination assembly together with a spacing frame, and carrying out sealing fixation to prepare the heat-insulating interlayer hollow glass. The impact strength of the obtained heat insulation interlayer hollow glass is 1969 J / cm < 2 >, the light transmittance is 99.1%, the heat conductivity coefficient is 0.9 W / (m < 2 >. K), and the isolation rate for ultraviolet rays with the wavelength of 350 nm is 78%. In addition, the thermal insulation interlayer formed by coating the polycarbonate plate with the organic silica sol is prepared, the vertical combustion grade of the thermal insulation interlayer is V-0 grade, and the thermal insulation interlayer has a flame retardant effect. The hollow glass prepared by the invention is high in explosion-proof performance and good in air tightness, has a heat insulation effect, and can block ultraviolet rays.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hollow glass preparation, in particular to a preparation process of heat-insulating interlayer hollow glass. Background Art

[0002] Insulating laminated insulating glass, as a building material with thermal insulation properties, has been widely used in the construction field in recent years. Insulating laminated insulating glass usually uses colorless float glass, coated glass, tempered glass, etc. as the base material, and after a series of treatments, it is coated with an insulating interlayer to prepare. The transparency and thermal insulation properties of the prepared glass material can meet daily needs. The spacer layer material mainly plays a supporting and thermal insulation role. In addition, the spacer layer is often filled with inert gases such as argon and nitrogen. These gases have low thermal conductivity and can significantly improve the thermal insulation performance of insulating glass. In addition, flame retardant materials can be added to the insulating interlayer of the insulating glass to improve its flame retardant properties and effectively prevent the spread of fire.

[0003] However, the quality of products in the field of hollow glass is uneven. For example, Chinese patent CN113565407B provides a hollow glass processing method, which includes the following steps: cutting, edge grinding, and tempering coated glass and white glass according to the required size, and coating a certain thickness of inner thermal insulation soft glue around to form a hollow glass cavity, and then curing the coated glass and white glass filled with outer support soft glue to form a hollow glass. The method can be widely used in hollow glass processing, but the prepared hollow glass has poor impact resistance, and the air tightness of the coated thermal insulation soft glue is poor, which is easy to cause inert gas leakage. Another example is Chinese patent CN111421918B, which discloses a laminated hollow intelligent dimming glass with a nano transparent heat insulation layer, which includes at least two glass layers, and a dimming film is provided between the adjacent two glass layers through a bonding film, and the surface of one glass layer is provided with a nano transparent heat insulation layer, which can intelligently control and adjust the glass to present a transparent state and a non-transparent state of different colors by controlling the on and off of the current, making the construction more convenient and having good heat insulation performance. However, the hollow glass prepared by the invention has a nano transparent heat insulation layer in the surface layer, which is easily affected by long-term light exposure and has no flame retardant effect. Another example is CN107446545B, which discloses a heat-insulating flame-retardant hollow glass and its preparation method. The prepared heat-insulating flame-retardant hollow glass includes a heat-insulating adhesive layer with a thickness of 10 to 20 μm, and a flame-retardant PET film is also bonded to the outside of the heat-insulating adhesive layer, which greatly improves the heat insulation performance of the hollow glass. Even if the glass bursts in a fire, the flame-retardant PET film can further prevent the spread of the fire. However, the hollow glass prepared by this invention does not have the ability to block ultraviolet rays.

[0004] Therefore, a preparation process of heat-insulating laminated hollow glass is proposed. Summary of the invention

[0005] The purpose of the present invention is to provide a process for preparing heat-insulating laminated hollow glass, wherein the glass substrate is cut, edged, cleaned, dried, and then semi-tempered to obtain a tempered glass sheet, and after heat-pressing the heat-insulating interlayer on both surfaces of the tempered glass sheet, the sheet is pushed into a dustproof room for lamination and assembly with a spacer frame, and then sealed and fixed to prepare the heat-insulating laminated hollow glass. The obtained heat-insulating laminated hollow glass has an impact strength of 1969 J / cm 2 The light transmittance is 99.1% and the thermal conductivity is 0.9W / (m 2 ·K), the UV blocking rate for wavelength 350nm is 78%. In addition, a heat-insulating interlayer coated with organic silica sol on a polycarbonate board is prepared, and its vertical combustion grade is V-0, which has a flame retardant effect. The hollow glass prepared by the present invention has strong explosion-proof performance, good air tightness, heat insulation effect, and can block ultraviolet rays.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] On the one hand, the present invention includes a process for preparing a heat-insulating laminated hollow glass, characterized in that it includes the following steps:

[0008] Cutting a glass substrate according to a required size and performing an edge grinding process to obtain edge grinding glass; placing the edge grinding glass in a solvent, soaking and cleaning it with water, a surfactant, acetone, and ethanol in sequence, and drying it after cleaning to obtain spare glass; semi-tempered treatment of the dried spare glass to obtain a tempered glass sheet; preheating the tempered glass sheet at 150-200° C., and then hot-pressing an insulating interlayer on both surfaces of the tempered glass sheet to obtain a prefabricated glass sheet; pushing two prefabricated glass sheets into a dustproof room in sequence, laminating and assembling them together with a spacing frame to form a hollow glass cavity, and then sealing and fixing them to obtain the insulating interlayer hollow glass;

[0009] The thickness of the glass substrate is 6 mm; both sides of the prefabricated glass sheet are coated with a heat-insulating interlayer with a thickness of 10 to 30 μm;

[0010] The preparation method of the thermal insulation interlayer comprises the following steps: dissolving tetraethyl orthosilicate in ethanol to obtain a tetraethyl orthosilicate solution; adding distilled water and dilute hydrochloric acid to the tetraethyl orthosilicate solution, stirring at 40-60° C. for 3 hours, adding a flame retardant and an ultraviolet absorber, and aging at 20-80° C. for 1 hour to obtain an organic silicon sol; coating the organic silicon sol on both surfaces of a polycarbonate plate to obtain a first layer; coating PVB film on both sides of the first layer to obtain a second layer; and coating PU film on both surfaces of the second layer to obtain a thermal insulation interlayer;

[0011] The thickness of the PVB film is 0.80 mm, and the thickness of the PU film is 1 mm.

[0012] Preferably, the surfactant is sodium dodecyl sulfate.

[0013] Preferably, the semi-tempered treatment is to heat the dried spare glass at 650-710° C. for 20-60 seconds and then quench it instantly with high-pressure air for 10 seconds.

[0014] Preferably, the hot pressing is performed at a temperature of 100° C. and a pressure of 1.2 MPa for 3 hours.

[0015] Preferably, the lamination and bonding are carried out in an environment with a temperature of 24±3° C. and a relative humidity of 23%±5%.

[0016] Preferably, the hollow glass cavity is filled with inert gas.

[0017] Preferably, the hot pressing is performed using a hot press; the temperature of the front roller of the hot press is 80° C., the temperature of the rear roller is 190° C., and the roller speed is 0.5 to 1.5 m / min.

[0018] Preferably, the concentration of the ethyl orthosilicate solution is 1.8-3.7 g / L; the concentration of the dilute hydrochloric acid is 0.2-1.1 mol / L.

[0019] Preferably, the flame retardant is a mixture of aluminum hydroxide and ammonium polyphosphate in a mass ratio of 1:1.5; the ultraviolet absorber is a benzotriazole ultraviolet absorber UVP-327, the main component of which is 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole.

[0020] On the other hand, the present invention also includes an insulating sandwich hollow glass, characterized in that: the insulating sandwich hollow glass is composed of two inner and outer prefabricated glass sheets, the spacer frame and the hollow glass cavity located between the two glass sheets; the insulating sandwich hollow glass is prepared by the preparation process as described above; the insulating sandwich hollow glass has an impact strength of 1969J / cm2; the light transmittance of the insulating sandwich hollow glass is 99.1%; the thermal conductivity of the insulating sandwich hollow glass is 0.9W / (m2·K); the insulating sandwich hollow glass includes an insulating interlayer, and the vertical combustion grade of the insulating interlayer is V-0 level; the insulating interlayer hollow glass has a UV blocking rate of 78% for a wavelength of 350nm.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. In the present invention, the glass substrate is cut to the required size and edge-grinded, then placed in a solvent, soaked and cleaned in water, surfactant sodium dodecyl sulfate, acetone, and ethanol in sequence, and dried after cleaning to obtain spare glass. The dried spare glass is semi-tempered to obtain a tempered glass sheet. The semi-tempered treatment is to heat the dried spare glass at 680°C for 30 seconds and then quench it instantly with high-pressure air for 10 seconds. Through the semi-tempered treatment, the impact strength of the finally prepared insulating laminated hollow glass is 1969J / cm 2 The present invention performs a semi-tempered treatment on ordinary glass and controls the temperature and heating time of the semi-tempered treatment, so that the finally prepared heat-insulating laminated hollow glass maintains the maximum impact strength and has strong explosion-proof performance. Therefore, it can withstand the environmental temperature difference load and aerodynamic load, is not easily deformed due to fatigue, and is more suitable for the exterior glass surface of a building.

[0023] 2. The present invention preheats the tempered glass sheet at 180°C first, and then heat-presses the two surfaces of the tempered glass sheet to obtain a prefabricated glass sheet; the hot pressing adopts a hot press, the front roller temperature of the hot press is 80°C, the rear roller temperature is 190°C, and the rolling speed is 0.8m / min; the hot pressing is performed at a temperature of 100°C and a pressure of 1.2Mpa for 3 hours; then the two prefabricated glass sheets are successively pushed into a dustproof room and stacked and assembled with a spacer frame to form a hollow glass cavity, and an inert gas is filled in the hollow glass cavity; the stacking and bonding are performed in an environment with a temperature of 24±3°C and a relative humidity of 23%±5%; then the prefabricated glass is sealed and fixed to obtain the insulating interlayer hollow glass. The heat-insulating laminated hollow glass obtained by the method has high transparency in the visible light wavelength range (380-780nm), and its light transmittance is 99.1%. The higher the visible light transmittance, the better the transparency and aesthetics of the heat-insulating laminated hollow glass. In addition, through the above preparation process of pressing and laminating, the obtained hollow glass has very good air tightness, can keep the inert gas from leaking, improves the heat insulation performance of the hollow glass to a certain extent, reduces the temperature difference between the two sides of the glass, and avoids fogging and frosting.

[0024] 3. In the present invention, ethyl orthosilicate is dissolved in ethanol to obtain a 2.2 g / L ethyl orthosilicate solution, distilled water and 0.5 mol / L dilute hydrochloric acid are added to the ethyl orthosilicate solution, and the organic silica sol prepared by the above preparation method is used to coat the two surfaces of the polycarbonate plate to obtain an insulating interlayer, which is hot-pressed to the two surfaces of the tempered glass sheet, and finally the thermal conductivity of the prepared insulating interlayer hollow glass is 0.9 W / (m 2·K). The present invention uses tetraethyl orthosilicate as a silicon source, which is hydrolyzed into silanol under acidic conditions and then further cross-linked into silica sol. Silica sol has a three-dimensional network structure, and the added flame retardant and ultraviolet absorber can enter the interior of the silica sol structure, so that the flame retardant performance and ultraviolet absorption performance of the final organic silica sol are more stable. In addition, the network structure of the organic silica sol can effectively limit the infrared heat radiation of the ambient temperature, thereby reducing local heat conduction, and the introduction of inert gas also has a certain heat insulation effect. The heat-insulating laminated hollow glass prepared by the present invention can be used as architectural glass to achieve the effects of maintaining room temperature, reducing the frequency of air conditioning startup, and saving energy.

[0025] 4. In the present invention, the ethyl orthosilicate solution and water are provided with acidic conditions by dilute hydrochloric acid, and then a flame retardant and a UV absorber are added after stirring at 40°C for 3 hours, and then aged at 60°C for 1 hour to obtain an organic silicon sol; the flame retardant is aluminum hydroxide and ammonium polyphosphate mixed in a mass ratio of 1:1.5; the UV absorber is a benzotriazole UV absorber UVP-327. The organic silicon sol obtained by the method is finally coated on a polycarbonate board to prepare a heat-insulating interlayer that is hot-pressed on the two surfaces of a tempered glass sheet. The obtained heat-insulating interlayer has a vertical combustion rating of V-0, which can effectively prevent the spread of a large fire in the event of a fire. The hollow glass prepared by the present invention is composed of two prefabricated glass sheets, and the two surfaces of the prefabricated glass sheets are heat-pressed with heat-insulating interlayers, and the heat-insulating interlayers contain organic silicon sol. By controlling the reaction temperature and aging temperature of the organic silicon sol, the finally obtained organic silicon sol can have a more regular spatial structure, which is conducive to the dispersion of the flame retardant in the organic silicon sol. Therefore, the finally prepared heat-insulating interlayer has a flame retardant effect. When it is heat-pressed to the facade glass of a building, it can effectively block the temperature and the spread of fire, and improve the escape rate in a fire.

[0026] 5. The present invention applies organic silica sol to both surfaces of a polycarbonate plate to obtain a first layer, applies PVB film to both sides of the first layer to obtain a second layer, and applies PU film to both surfaces of the second layer to obtain a heat-insulating interlayer; and both sides of the prefabricated glass sheet are coated with a heat-insulating interlayer with a thickness of 20 μm, the thickness of the PVB film is 0.80 mm, and the thickness of the PU film is 1 mm. Through the above-mentioned preparation process, the heat-insulating interlayer hollow glass finally prepared can have a UV cutoff rate of 78% for a wavelength of 350 nm. When preparing the organic silica sol, the present invention adds a benzotriazole ultraviolet light absorber UVP-327, which has good chemical stability and can absorb ultraviolet rays with a wavelength of 270 to 380 nm, so that the heat-insulating interlayer hollow glass finally prepared can achieve a certain degree of UV cutoff. In addition, the organic silica sol is in the inner layer of the heat-insulating interlayer, and long-term light exposure will not affect it. Ultraviolet radiation will accelerate the aging of human skin, so good UV protection can protect the room from ultraviolet radiation; and PVB film is coated in the thermal insulation interlayer, which can absorb impact energy. Even if the glass is damaged, its glass fragments will still stick to the middle film, which can reduce the probability of fragments flying and improve the safety performance of the prepared glass. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Schematic diagram of the heat-insulating interlayer structure prepared in the present invention, wherein 0 represents the innermost layer, 1 represents the first layer, A and B represent two surfaces respectively, for example 1A represents the A surface of the first layer, and so on. DETAILED DESCRIPTION

[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] See also Figure 1 The present invention provides a preparation process of heat-insulating laminated hollow glass, and the technical scheme is as follows:

[0030] Example 1

[0031] A preparation process of heat-insulating laminated hollow glass, comprising the following steps:

[0032] Cutting a glass substrate according to a required size and grinding the edge to obtain a ground glass; soaking the ground glass in a solvent with water, a surfactant sodium dodecyl sulfate, acetone, and ethanol in sequence, washing it, and drying it after washing to obtain a spare glass; semi-tempered treatment of the dried spare glass to obtain a tempered glass sheet; the semi-tempered treatment is to heat the dried spare glass at 650°C for 20 seconds and then quench it instantly with high-pressure air for 10 seconds; preheating the tempered glass sheet at 150°C, and then hot-pressing a heat-insulating interlayer on both surfaces of the tempered glass sheet to obtain a prefabricated glass sheet ; The hot pressing adopts a hot press; the temperature of the front roller of the hot press is 80°C, the temperature of the rear roller is 190°C, and the rolling speed is 0.5m / min; the hot pressing is steamed for 3 hours at a temperature of 100°C and a pressure of 1.2Mpa; the two prefabricated glass sheets are pushed into the dustproof room in turn and stacked and assembled with the spacing frame to form a hollow glass cavity; the hollow glass cavity is filled with inert gas; the stacking and assembly are carried out in an environment with a temperature of 24±3°C and a relative humidity of 23%±5%; and then sealed and fixed to obtain the thermal insulation sandwich hollow glass;

[0033] The thickness of the glass substrate is 6 mm; both sides of the prefabricated glass sheet are coated with a heat-insulating interlayer with a thickness of 10 μm;

[0034] The preparation method of the thermal insulation interlayer comprises the following steps: dissolving tetraethyl orthosilicate in ethanol to obtain a tetraethyl orthosilicate solution with a concentration of 1.8 g / L; adding distilled water and dilute hydrochloric acid with a concentration of 0.2 mol / L to the tetraethyl orthosilicate solution, stirring at 40° C. for 3 hours, adding a flame retardant and an ultraviolet absorber, and aging at 20° C. for 1 hour to obtain an organic silicon sol; the flame retardant is aluminum hydroxide and ammonium polyphosphate mixed in a mass ratio of 1:1.5; the ultraviolet absorber is a benzotriazole ultraviolet absorber UVP-327; applying the organic silicon sol to both surfaces of a polycarbonate board to obtain a first layer; applying PVB film on both sides of the first layer to obtain a second layer; and applying PU film on both surfaces of the second layer to obtain a thermal insulation interlayer;

[0035] The thickness of the PVB film is 0.80 mm, and the thickness of the PU film is 1 mm.

[0036] In Example 1, the glass substrate is an initial glass sheet, and the production company is Huizhou Yanghang Glass Products Co., Ltd.; for other specific conditions not specified, conventional conditions or conditions recommended by the manufacturer are followed; the reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially.

[0037] In the process of preparing the heat-insulating laminated insulating glass in Example 2-8, the temperature and heating time of the semi-tempered treatment are shown in Table 1, and the remaining steps and operations are the same as in Example 1.

[0038] Table 1 Temperature and heating time of semi-tempered treatment in Example 2-8

[0039]

[0040]

[0041] Example 9

[0042] The impact strength of the insulating laminated insulating glass prepared in the above Examples 1-8 was tested. The impact strength of the insulating laminated insulating glass was tested using a direct-drive electronic universal testing machine. The test results are shown in Table 2.

[0043] In Example 5, the glass substrate is cut to the required size and edge-grinded, then placed in a solvent, soaked and cleaned in water, surfactant sodium dodecyl sulfate, acetone, and ethanol in sequence, and dried after cleaning to obtain spare glass. The dried spare glass is semi-tempered to obtain a tempered glass sheet. The semi-tempered treatment is to heat the dried spare glass at 680°C for 30 seconds and then quench it instantly with high-pressure air for 10 seconds. Through the semi-tempered treatment, the impact strength of the finally prepared insulating laminated hollow glass is 1969J / cm 2 The present invention performs a semi-tempered treatment on ordinary glass and controls the temperature and heating time of the semi-tempered treatment, so that the finally prepared heat-insulating laminated hollow glass maintains the maximum impact strength and has strong explosion-proof performance. Therefore, it can withstand the environmental temperature difference load and aerodynamic load, is not easily deformed due to fatigue, and is more suitable for the exterior glass surface of a building.

[0044] Table 2 Impact strength of the insulating laminated hollow glass prepared in Examples 1-8

[0045] <![CDATA[Impact strength (J / cm 2 )]]> Example 1 1765 Example 2 1730 Example 3 1854 Example 4 1655 Example 5 1969 Example 6 1831 Example 7 1828 Example 8 1791

[0046] Example 10

[0047] A preparation process of heat-insulating laminated hollow glass, comprising the following steps:

[0048] Cutting a glass substrate into required sizes and grinding the edges to obtain grinding glass; soaking the grinding glass in a solvent with water, a surfactant, sodium dodecyl sulfate, acetone, and ethanol in turn, washing the glass, and drying the glass to obtain spare glass; semi-tempered the dried spare glass to obtain a tempered glass sheet; the semi-tempered treatment is to heat the dried spare glass at 680°C for 30 seconds and then quench it with high-pressure air for 10 seconds; preheating the tempered glass sheet at 160°C, and then hot-pressing a heat-insulating interlayer on both surfaces of the tempered glass sheet to obtain a prefabricated glass sheet ; The hot pressing adopts a hot press; the temperature of the front roller of the hot press is 80°C, the temperature of the rear roller is 190°C, and the rolling speed is 0.8m / min; the hot pressing is performed under the conditions of a temperature of 100°C and a pressure of 1.2Mpa for 3 hours; the two prefabricated glass sheets are sequentially pushed into a dustproof room and stacked and assembled with a spacing frame to form a hollow glass cavity; the hollow glass cavity is filled with inert gas; the stacking and assembly are performed under an environment of a temperature of 24±3°C and a relative humidity of 23%±5%; and then sealed and fixed to obtain the heat-insulating laminated hollow glass;

[0049] The thickness of the glass substrate is 6 mm; both sides of the prefabricated glass sheet are coated with a heat-insulating interlayer with a thickness of 10 μm;

[0050] The preparation method of the thermal insulation interlayer comprises the following steps: dissolving tetraethyl orthosilicate in ethanol to obtain a tetraethyl orthosilicate solution with a concentration of 1.8 g / L; adding distilled water and dilute hydrochloric acid with a concentration of 0.2 mol / L to the tetraethyl orthosilicate solution, stirring at 40° C. for 3 hours, adding a flame retardant and an ultraviolet absorber, and aging at 20° C. for 1 hour to obtain an organic silicon sol; the flame retardant is aluminum hydroxide and ammonium polyphosphate mixed in a mass ratio of 1:1.5; the ultraviolet absorber is a benzotriazole ultraviolet absorber UVP-327; applying the organic silicon sol to both surfaces of a polycarbonate board to obtain a first layer; applying PVB film on both sides of the first layer to obtain a second layer; and applying PU film on both surfaces of the second layer to obtain a thermal insulation interlayer;

[0051] The thickness of the PVB film is 0.80 mm, and the thickness of the PU film is 1 mm.

[0052] The preheating temperature and rolling speed in Examples 11-18 are shown in Table 3, and the remaining steps and operations are the same as in Example 10.

[0053] Table 3 Preheating temperature and rolling speed in Examples 11-18

[0054] Preheating temperature (℃) Rolling speed (m / min) Embodiment 11 150 1.5 Example 12 150 1.0 Embodiment 13 160 0.8 Embodiment 14 160 0.5 Embodiment 15 180 0.8 Example 16 180 1.0 Embodiment 17 200 0.8 Embodiment 18 200 0.5

[0055] Embodiment 19

[0056] The light transmittance of the heat-insulating laminated hollow glass prepared in the above Examples 10-18 was tested by a light transmittance meter, model HCBT-H, and the results are shown in Table 4.

[0057] In Example 15, the tempered glass sheet is first preheated at 180°C, and then an insulating interlayer is hot-pressed on both surfaces of the tempered glass sheet to obtain a prefabricated glass sheet; the hot pressing adopts a hot press, the front roller temperature of the hot press is 80°C, the rear roller temperature is 190°C, and the rolling speed is 0.8m / min; the hot pressing is performed at a temperature of 100°C and a pressure of 1.2Mpa for 3 hours; then the two prefabricated glass sheets are pushed into a dustproof room in turn and are stacked and assembled with a spacer frame to form a hollow glass cavity, and inert gas is filled in the hollow glass cavity; the stacking and assembly are carried out in an environment with a temperature of 24±3°C and a relative humidity of 23%±5%; then they are sealed and fixed to obtain the insulating interlayer hollow glass. The heat-insulating laminated hollow glass obtained by the method has high transparency in the visible light wavelength range (380-780nm), and its light transmittance is 99.1%. The higher the visible light transmittance, the better the transparency and aesthetics of the heat-insulating laminated hollow glass. In addition, through the above preparation process of pressing and laminating, the obtained hollow glass has very good air tightness, can keep the inert gas from leaking, improves the heat insulation performance of the hollow glass to a certain extent, reduces the temperature difference between the two sides of the glass, and avoids fogging and frosting.

[0058] Table 4 Light transmittance of insulating glass prepared in Examples 10-18

[0059] Light transmittance (%) Example 10 97.5 Embodiment 11 97.1 Example 12 98.6 Embodiment 13 98.5 Embodiment 14 99.0 Embodiment 15 99.1 Example 16 98.4 Embodiment 17 97.9 Embodiment 18 96.8

[0060] Embodiment 20

[0061] A preparation process of heat-insulating laminated hollow glass, comprising the following steps:

[0062] Cutting a glass substrate into required sizes and grinding the edges to obtain grinding glass; soaking the grinding glass in a solvent with water, a surfactant, sodium dodecyl sulfate, acetone, and ethanol in turn, washing the glass, and drying the glass to obtain spare glass; semi-tempered treatment of the dried spare glass to obtain a tempered glass sheet; the semi-tempered treatment is to heat the dried spare glass at 680°C for 30 seconds and then quench it instantly with high-pressure air for 10 seconds; preheating the tempered glass sheet at 180°C, and then hot-pressing a heat-insulating interlayer on both surfaces of the tempered glass sheet to obtain a prefabricated glass sheet ; The hot pressing adopts a hot press; the temperature of the front roller of the hot press is 80°C, the temperature of the rear roller is 190°C, and the rolling speed is 0.8m / min; the hot pressing is performed under the conditions of a temperature of 100°C and a pressure of 1.2Mpa for 3 hours; the two prefabricated glass sheets are sequentially pushed into a dustproof room and stacked and assembled with a spacing frame to form a hollow glass cavity; the hollow glass cavity is filled with inert gas; the stacking and assembly are performed under an environment of a temperature of 24±3°C and a relative humidity of 23%±5%; and then sealed and fixed to obtain the heat-insulating laminated hollow glass;

[0063] The thickness of the glass substrate is 6 mm; both sides of the prefabricated glass sheet are coated with a heat-insulating interlayer with a thickness of 10 μm;

[0064] The preparation method of the thermal insulation interlayer comprises the following steps: dissolving tetraethyl orthosilicate in ethanol to obtain a 2.0 g / L tetraethyl orthosilicate solution; adding distilled water and 0.2 mol / L dilute hydrochloric acid to the tetraethyl orthosilicate solution, stirring at 40° C. for 3 hours, adding a flame retardant and an ultraviolet absorber, and aging at 20° C. for 1 hour to obtain an organic silicon sol; the flame retardant is aluminum hydroxide and ammonium polyphosphate mixed in a mass ratio of 1:1.5; the ultraviolet absorber is a benzotriazole ultraviolet absorber UVP-327; applying the organic silicon sol to both surfaces of a polycarbonate board to obtain a first layer; applying PVB film on both sides of the first layer to obtain a second layer; and applying PU film on both surfaces of the second layer to obtain a thermal insulation interlayer;

[0065] The thickness of the PVB film is 0.80 mm, and the thickness of the PU film is 1 mm.

[0066] The concentrations of the ethyl orthosilicate solution and the dilute hydrochloric acid in Examples 21-28 are shown in Table 5, and the remaining steps and operations are the same as in Example 20.

[0067] Table 5 Concentration of ethyl orthosilicate solution and dilute hydrochloric acid in Examples 21-28

[0068]

[0069] Embodiment 29

[0070] The thermal insulation performance of the insulating laminated hollow glass prepared in the above Examples 20-28 was tested. The thermal insulation performance was characterized by the thermal conductivity, and the thermal conductivity was tested by the heat flow meter method, and the instrument used was a heat flow sensor, model HFP-01, and the test results are shown in Table 6.

[0071] In Example 24 of the present invention, tetraethyl orthosilicate is dissolved in ethanol to obtain a 2.2 g / L tetraethyl orthosilicate solution, distilled water and 0.5 mol / L dilute hydrochloric acid are added to the tetraethyl orthosilicate solution, and the organic silica sol prepared by the above preparation method is used to coat the two surfaces of the polycarbonate board to obtain an insulating interlayer, which is hot-pressed to the two surfaces of the tempered glass sheet, and finally the thermal conductivity of the prepared insulating interlayer hollow glass is 0.9 W / (m 2 ·K). The present invention uses tetraethyl orthosilicate as a silicon source, which is hydrolyzed into silanol under acidic conditions and then further cross-linked into silica sol. Silica sol has a three-dimensional network structure, and the added flame retardant and ultraviolet absorber can enter the interior of the silica sol structure, so that the flame retardant performance and ultraviolet absorption performance of the final organic silica sol are more stable. In addition, the network structure of the organic silica sol can effectively limit the infrared heat radiation of the ambient temperature, thereby reducing local heat conduction, and the introduction of inert gas also has a certain heat insulation effect. The heat-insulating laminated hollow glass prepared by the present invention can be used as architectural glass to achieve the effects of maintaining room temperature, reducing the frequency of air conditioning startup, and saving energy.

[0072] Table 6 Thermal conductivity of insulating glass prepared in Examples 20-28

[0073] <![CDATA[Thermal conductivity (W / (m 2 ·K))]]> Embodiment 20 1.0 Embodiment 21 1.0 Embodiment 22 1.1 Embodiment 23 1.0 Embodiment 24 0.9 Embodiment 25 1.0 Embodiment 26 1.1 Embodiment 27 1.2 Embodiment 28 1.1

[0074] Embodiment 30

[0075] A preparation process of heat-insulating laminated hollow glass, comprising the following steps:

[0076] Cutting a glass substrate into required sizes and grinding the edges to obtain grinding glass; soaking the grinding glass in a solvent with water, a surfactant, sodium dodecyl sulfate, acetone, and ethanol in turn, washing the glass, and drying the glass to obtain spare glass; semi-tempered treatment of the dried spare glass to obtain a tempered glass sheet; the semi-tempered treatment is to heat the dried spare glass at 680°C for 30 seconds and then quench it instantly with high-pressure air for 10 seconds; preheating the tempered glass sheet at 180°C, and then hot-pressing a heat-insulating interlayer on both surfaces of the tempered glass sheet to obtain a prefabricated glass sheet ; The hot pressing adopts a hot press; the temperature of the front roller of the hot press is 80°C, the temperature of the rear roller is 190°C, and the rolling speed is 0.8m / min; the hot pressing is performed under the conditions of a temperature of 100°C and a pressure of 1.2Mpa for 3 hours; the two prefabricated glass sheets are sequentially pushed into a dustproof room and stacked and assembled with a spacing frame to form a hollow glass cavity; the hollow glass cavity is filled with inert gas; the stacking and assembly are performed under an environment of a temperature of 24±3°C and a relative humidity of 23%±5%; and then sealed and fixed to obtain the heat-insulating laminated hollow glass;

[0077] The thickness of the glass substrate is 6 mm; both sides of the prefabricated glass sheet are coated with a heat-insulating interlayer with a thickness of 10 μm;

[0078] The preparation method of the thermal insulation interlayer comprises the following steps: dissolving tetraethyl orthosilicate in ethanol to obtain a 2.2 g / L tetraethyl orthosilicate solution; adding distilled water and 0.5 mol / L dilute hydrochloric acid to the tetraethyl orthosilicate solution, stirring at 50° C. for 3 hours, adding a flame retardant and an ultraviolet absorber, and aging at 20° C. for 1 hour to obtain an organic silicon sol; the flame retardant is aluminum hydroxide and ammonium polyphosphate mixed in a mass ratio of 1:1.5; the ultraviolet absorber is a benzotriazole ultraviolet absorber UVP-327; applying the organic silicon sol to both surfaces of a polycarbonate board to obtain a first layer; applying PVB film on both sides of the first layer to obtain a second layer; and applying PU film on both surfaces of the second layer to obtain a thermal insulation interlayer;

[0079] The thickness of the PVB film is 0.80 mm, and the thickness of the PU film is 1 mm.

[0080] The stirring temperature and aging temperature for preparing the organosilica sol in Examples 31-36 are shown in Table 7, and the remaining reagents and operations are the same as in Example 30.

[0081] Table 7 Stirring temperature and aging temperature of the organosilica sol prepared in Examples 31-36

[0082] Stirring temperature (℃) Aging temperature(℃) Embodiment 31 40 80 Embodiment 32 40 60 Embodiment 33 50 60 Embodiment 34 50 40 Embodiment 35 60 40 Embodiment 36 60 20

[0083] Embodiment 37

[0084] The flame retardant properties of the thermal insulation interlayers prepared in the above Examples 30-36 were tested. The flame retardant properties were described by the vertical burning grade. The test results are shown in Table 8.

[0085] In Example 32, the ethyl orthosilicate solution and water are provided with acidic conditions by dilute hydrochloric acid, and after stirring at 40°C for 3 hours, flame retardants and ultraviolet absorbers are added and aged at 60°C for 1 hour to obtain an organic silica sol; the flame retardant is aluminum hydroxide and ammonium polyphosphate mixed in a mass ratio of 1:1.5; the ultraviolet absorber is a benzotriazole ultraviolet light absorber UVP-327. The organic silica sol obtained by the method is finally coated on a polycarbonate board to prepare a heat-insulating interlayer that is hot-pressed on the two surfaces of the tempered glass sheet. The obtained heat-insulating interlayer has a vertical combustion rating of V-0, which can effectively prevent the spread of fire in the event of a fire. The hollow glass prepared by the present invention is composed of two prefabricated glass sheets, and the two surfaces of the prefabricated glass sheets are heat-pressed with heat-insulating interlayers, and the heat-insulating interlayers contain organic silicon sol. By controlling the reaction temperature and aging temperature of the organic silicon sol, the finally obtained organic silicon sol can have a more regular spatial structure, which is conducive to the dispersion of the flame retardant in the organic silicon sol. Therefore, the finally prepared heat-insulating interlayer has a flame retardant effect. When it is heat-pressed to the facade glass of a building, it can effectively block the temperature and the spread of fire, and improve the escape rate in a fire.

[0086] Table 8 Vertical combustion rating of thermal insulation interlayers prepared in Examples 30-36

[0087]

[0088]

[0089] Embodiment 38

[0090] A preparation process of heat-insulating laminated hollow glass, comprising the following steps:

[0091] Cutting a glass substrate into required sizes and grinding the edges to obtain grinding glass; soaking the grinding glass in a solvent with water, a surfactant, sodium dodecyl sulfate, acetone, and ethanol in turn, washing the glass, and drying the glass to obtain spare glass; semi-tempered treatment of the dried spare glass to obtain a tempered glass sheet; the semi-tempered treatment is to heat the dried spare glass at 680°C for 30 seconds and then quench it instantly with high-pressure air for 10 seconds; preheating the tempered glass sheet at 180°C, and then hot-pressing a heat-insulating interlayer on both surfaces of the tempered glass sheet to obtain a prefabricated glass sheet ; The hot pressing adopts a hot press; the temperature of the front roller of the hot press is 80°C, the temperature of the rear roller is 190°C, and the rolling speed is 0.8m / min; the hot pressing is performed under the conditions of a temperature of 100°C and a pressure of 1.2Mpa for 3 hours; the two prefabricated glass sheets are sequentially pushed into a dustproof room and stacked and assembled with a spacing frame to form a hollow glass cavity; the hollow glass cavity is filled with inert gas; the stacking and assembly are performed under an environment of a temperature of 24±3°C and a relative humidity of 23%±5%; and then sealed and fixed to obtain the heat-insulating laminated hollow glass;

[0092] The thickness of the glass substrate is 6 mm; both sides of the prefabricated glass sheet are coated with a heat-insulating interlayer with a thickness of 15 μm;

[0093] The preparation method of the thermal insulation interlayer comprises the following steps: dissolving tetraethyl orthosilicate in ethanol to obtain a 2.2 g / L tetraethyl orthosilicate solution; adding distilled water and 0.5 mol / L dilute hydrochloric acid to the tetraethyl orthosilicate solution, stirring at 40°C for 3 hours, adding a flame retardant and an ultraviolet absorber, and aging at 60°C for 1 hour to obtain an organic silicon sol; the flame retardant is aluminum hydroxide and ammonium polyphosphate mixed in a mass ratio of 1:1.5; the ultraviolet absorber is a benzotriazole ultraviolet absorber UVP-327; applying the organic silicon sol to both surfaces of a polycarbonate board to obtain a first layer; applying PVB film on both sides of the first layer to obtain a second layer; and applying PU film on both surfaces of the second layer to obtain a thermal insulation interlayer;

[0094] The thickness of the PVB film is 0.80 mm, and the thickness of the PU film is 1 mm.

[0095] In Example 39, both sides of the prefabricated glass sheet are coated with an insulating interlayer with a thickness of 20 μm, and the remaining reagents and operations are the same as in Example 38.

[0096] In Example 40, both sides of the prefabricated glass sheet are coated with a thermal insulation interlayer with a thickness of 25 μm, and the remaining reagents and operations are the same as in Example 38.

[0097] In Example 41, both sides of the prefabricated glass sheet are coated with a thermal insulation interlayer with a thickness of 30 μm, and the remaining reagents and operations are the same as in Example 38.

[0098] In Example 42, one side of the prefabricated glass sheet is coated with a thermal insulation interlayer with a thickness of 20 μm, and the remaining reagents and operations are the same as in Example 38.

[0099] In Example 43, no PVB film is applied, and the remaining reagents and operations are the same as in Example 38.

[0100] In Example 44, no PU film is coated, and the remaining reagents and operations are the same as in Example 38.

[0101] Comparative Example 1

[0102] The insulating interlayer was not hot pressed, and the remaining reagents and operations were the same as in Example 39.

[0103] Comparative Example 2

[0104] No organosilica sol was added, and the remaining reagents were the same as in Example 39.

[0105] Embodiment 45

[0106] The ultraviolet blocking rate of the heat-insulating laminated hollow glass prepared in the above Examples 38-44 was tested, and the test results are shown in Table 9. The ultraviolet blocking rate is used to evaluate the ultraviolet protection ability of the glass, and is tested by an ultraviolet blocking rate tester, and the manufacturer is Dongguan Haotian Testing Equipment Co., Ltd.

[0107] In Example 39, the organic silica sol is coated on both surfaces of the polycarbonate plate to obtain the first layer, the PVB film is coated on both sides of the first layer to obtain the second layer, and the PU film is coated on both surfaces of the second layer to obtain the heat insulation interlayer, and both sides of the prefabricated glass sheet are coated with a heat insulation interlayer with a thickness of 20 μm, the thickness of the PVB film is 0.80 mm, and the thickness of the PU film is 1 mm. Figure 1The figure shows a schematic diagram of the heat-insulating interlayer prepared by the present invention. Through the preparation process described above, the heat-insulating interlayer hollow glass finally prepared can have a UV cutoff rate of 78% for a wavelength of 350nm. When preparing the organic silica sol, the present invention adds a benzotriazole ultraviolet light absorber UVP-327, which has good chemical stability and can absorb ultraviolet rays with a wavelength of 270 to 380nm, so that the heat-insulating interlayer hollow glass finally prepared can achieve a certain degree of UV cutoff. In addition, the organic silica sol is in the inner layer of the heat-insulating interlayer, and long-term light exposure will not affect it. Ultraviolet radiation accelerates the aging of human skin, so good UV protection can protect the room from ultraviolet radiation; and the heat-insulating interlayer is coated with PVB film, which can absorb impact energy. Even if the glass is damaged, its glass fragments will still stick to the intermediate film, which can reduce the probability of fragments splashing and improve the safety performance of the prepared glass. In Example 43, the heat-insulating interlayer prepared without coating PVB film is prone to glass fragments splashing, causing safety hazards. Comparative Example 1 does not have a heat-insulating interlayer, and its heat insulation effect is poor, and the thermal conductivity is 1.4W / (m 2 ·K). Comparative Example 2 does not add organic silica sol, and its thermal conductivity is 1.3W / (m 2 ·K), indicating that the organosilicon sol plays an important role in thermal insulation in the thermal insulation interlayer.

[0108] Table 9 Ultraviolet blocking rate of insulating glass prepared in Examples 38-44

[0109]

[0110]

[0111] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A preparation process for heat-insulating laminated hollow glass, It is characterized in that The following steps are involved: Cutting a glass substrate according to a required size and performing an edge grinding process to obtain edge grinding glass; placing the edge grinding glass in a solvent, soaking and cleaning it with water, a surfactant, acetone, and ethanol in sequence, and drying it after cleaning to obtain spare glass; semi-tempered treatment of the dried spare glass to obtain a tempered glass sheet; preheating the tempered glass sheet at 150-200° C., and then hot-pressing an insulating interlayer on both surfaces of the tempered glass sheet to obtain a prefabricated glass sheet; pushing two prefabricated glass sheets into a dustproof room in sequence, laminating and assembling them together with a spacing frame to form a hollow glass cavity, and then sealing and fixing them to obtain the insulating interlayer hollow glass; The thickness of the glass substrate is 6 mm; both sides of the prefabricated glass sheet are coated with a heat-insulating interlayer with a thickness of 10 to 30 μm; The method for preparing the thermal insulation interlayer comprises the following steps: dissolving tetraethyl orthosilicate in ethanol to obtain a tetraethyl orthosilicate solution; Add distilled water and dilute hydrochloric acid to the tetraethyl orthosilicate solution, stir at 40-60° C. for 3 hours, then add flame retardant and ultraviolet absorber, age at 20-80° C. for 1 hour to obtain an organic silica sol; apply the organic silica sol to both surfaces of a polycarbonate plate to obtain a first layer; apply PVB film on both sides of the first layer to obtain a second layer; apply PU film on both surfaces of the second layer to obtain a heat insulation interlayer; The thickness of the PVB film is 0.80 mm, and the thickness of the PU film is 1 mm.

2. A process for preparing a heat-insulating laminated hollow glass according to claim 1, Features: The surfactant is sodium dodecyl sulfate.

3. The process for preparing the heat-insulating laminated hollow glass according to claim 1, Features: The semi-tempered treatment is to heat the dried spare glass at 650-710° C. for 20-60 seconds and then quench it instantly with high-pressure air for 10 seconds.

4. The process for preparing the heat-insulating laminated hollow glass according to claim 1, Features: The hot pressing is carried out under the conditions of a temperature of 100° C. and a pressure of 1.2 MPa for 3 hours.

5. The process for preparing the heat-insulating laminated hollow glass according to claim 1, Features: The lamination and bonding are carried out in an environment with a temperature of 24±3° C. and a relative humidity of 23%±5%.

6. The process for preparing the heat-insulating laminated hollow glass according to claim 1, Features: The hollow glass cavity is filled with inert gas.

7. The process for preparing the heat-insulating laminated hollow glass according to claim 1, Features: The hot pressing adopts a hot press; the temperature of the front roller of the hot press is 80°C, the temperature of the rear roller is 190°C, and the roller speed is 0.5-1.5m / min.

8. The process for preparing the heat-insulating laminated hollow glass according to claim 1, Features: The concentration of the ethyl orthosilicate solution is 1.8-3.7 g / L; the concentration of the dilute hydrochloric acid is 0.2-1.1 mol / L.

9. The process for preparing the heat-insulating laminated hollow glass according to claim 1, Features: The flame retardant is a mixture of aluminum hydroxide and ammonium polyphosphate in a mass ratio of 1:1.5; the ultraviolet absorber is a benzotriazole ultraviolet absorber UVP-327, the main component of which is 2-(2'-hydroxy-3', 5'-di-tert-phenyl)-5-chlorobenzotriazole.

10. A heat-insulating laminated hollow glass, Features: The insulating interlayer hollow glass is composed of two inner and outer prefabricated glass sheets, the spacer frame and the hollow glass cavity located between the two glass sheets; the insulating interlayer hollow glass is prepared by the preparation process according to any one of claims 1 to 9; the impact strength of the insulating interlayer hollow glass is 1969 J / cm 2 The light transmittance of the insulating interlayer hollow glass is 99.1%; the thermal conductivity of the insulating interlayer hollow glass is 0.9W / (m 2 ·K); the heat-insulating interlayer insulating glass comprises a heat-insulating interlayer, and the vertical combustion grade of the heat-insulating interlayer is V-0 level; the heat-insulating interlayer insulating glass has a UV blocking rate of 78% for a wavelength of 350nm.

Citation Information

Patent Citations

  • Facing explosion resistant, bulletproof and violence resistant hollow sandwich compound glass and method for manufacturing same

    CN101545348A

  • Silica sol enhanced hollow safety glass and preparation method thereof

    CN108751733A

  • Composite light body insulating glass with two pieces of glass and three cavities and manufacturing method thereof

    CN111980549A

  • High-performance light-weight passenger room side window for high-speed train

    CN112208562A

  • Bullet-proof glass and processing method thereof

    CN116252529A

Cited By

  • Manufacturing process of semi-tempered laminated hollow glass

    CN122565359A