Retarder for oil well cement and preparation method thereof

The retarder prepared by polymerization, combined with polymer and photoinitiator, solves the performance differences of oil well cement retarder in high and low temperature environments, achieves excellent high and low temperature resistance, and improves the stability of cement slurry and compressive strength.

CN118978356AInactive Publication Date: 2024-11-19CHONGQING KEDI NEW MATERIAL TECHNOLOGY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411063121.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing oil well cement retarder has poor performance in high-temperature and low-temperature environments. The high-temperature retarder is prone to super-retarding under low-temperature conditions, and the salt resistance and chemical properties are unstable, making it difficult to control the cementing quality.

Method used

Using a retarder including the first polymer and the second polymer, polymerization is carried out by polymerization by 2-acrylamide-2-methylpropanesulfonic acid monomer, unsaturated carboxylic acid monomer and rigid monomer, and chain transfer is added. The agent, photoinitiator and emulsifier are prepared by curing with ultraviolet light irradiation to form a retarder with excellent high temperature and low temperature resistance.

Benefits of technology

Improve the high temperature resistance of the retarder, extend the thickening time of the cement slurry, reduce the water loss, enhance chemical effects, improve the stability and compressive strength in high temperature environments, and solve the problem of retarder at high temperatures. and the performance difference at low temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978356A_ABST
    Figure CN118978356A_ABST
Patent Text Reader

Abstract

The invention provides a retarder for oil well cement and a preparation method thereof.The preparation method of the retarder comprises the steps that a 2-acrylamido-2-methylpropanesulfonic acid monomer, an unsaturated carboxylic acid monomer and a rigid monomer are added into deionized water and stirred to be dissolved, and the pH value is adjusted to 4-5; heating the mixed solution to 50-90 DEG C, adding a chain transfer agent, and carrying out polymerization reaction; adding a second polymer and water into the reaction product, adding a photoinitiator and an emulsifier, and stirring in a nitrogen atmosphere; and carrying out ultraviolet irradiation reaction on the stirred product, curing, washing with ethanol, and drying to obtain the retarder. The retarder provided by the invention has excellent stability and high temperature resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of retarders for oil well cement, and in particular to a retarder for oil well cement and a preparation method thereof. Background Art

[0002] Cementing is a major step in the oil well construction process. The quality of cementing is directly related to the continued drilling of the oil well, as well as the quality of subsequent completion, oil production, workover and other operations. Cementing operations have two steps, namely, casing and cementing. Through cementing construction, the annular space between the casing and the wellbore is filled with oil well cement. The main function of cement slurry is to isolate the flow of fluid between layers, support the casing, prevent pipe wall corrosion, and isolate the leakage layer or low-pressure layer.

[0003] The problem of difficult to control cementing quality is often encountered in large temperature difference cementing environment, mainly because the temperature difference between the upper and lower ends of the cementing well section during cementing construction is large, and although there are many types of retarders on the market, their performance is single. The high-temperature and low-temperature performance of commonly used retarders are quite different, and high-temperature resistant retarders are very likely to produce super-retardation under low-temperature conditions.

[0004] In view of this, how to obtain a retarder having excellent performance in both high temperature and low temperature environments is of great significance. Summary of the invention

[0005] The present application provides a retarder for oil well cement and a preparation method thereof, which are used to solve the technical problems of poor temperature resistance, poor salt resistance, unstable chemical properties and the like existing in the prior art retarders.

[0006] In a first aspect, the present application provides a retarder for oil well cement, the retarder comprising: a first polymer and a second polymer;

[0007] The first polymer structural formula is as follows:

[0008]

[0009] Among them, the value range of x is 40 to 80, the value range of y is 15 to 35, and the value range of z is 10 to 18;

[0010] The R1 is selected from any one of -H, -CH3, -CH2CH3, -COOCH3 or -CH2COOH;

[0011] The R2 is selected from any one of -SO3H, -N(CH3)2, -NHCH2COOH or imidazole;

[0012] The second polymer includes: polyurethane acrylic resin or polyester acrylic resin;

[0013] The mass ratio of the first polymer to the second polymer is 1:0.4-0.7.

[0014] In a possible implementation manner, the retarder further includes water, and the water accounts for 50-60% of the total weight of the retarder.

[0015] In a possible implementation manner, the retarder also includes a photoinitiator;

[0016] The amount of the photoinitiator added is 5% to 18% of the second polymer.

[0017] In one possible implementation, the photoinitiator is selected from α-hydroxyisobutyrophenone or 1-hydroxycyclohexylphenyl ketone.

[0018] In a possible implementation manner, the retarder further includes an emulsifier, and the amount of the emulsifier added is 1% to 6% of the amount of the second polymer;

[0019] The emulsifier includes Spahn 80 and Tween 80 in a mass ratio of 1:1 to 1.2.

[0020] In a second aspect, the present application provides a method for preparing a retarder for oil well cement, the preparation method comprising:

[0021] Add 2-acrylamide-2-methylpropanesulfonic acid monomer, unsaturated carboxylic acid monomer and rigid monomer into deionized water, stir to dissolve, and adjust the pH value to 4-5;

[0022] The mixed solution is heated to 50-90°C, a chain transfer agent is added, and a polymerization reaction is carried out;

[0023] Adding the second polymer and water to the above reaction product, and then adding a photoinitiator and an emulsifier, and stirring under a nitrogen atmosphere;

[0024] The stirred product is irradiated with ultraviolet light for reaction, solidified, washed with ethanol, and dried to obtain the retarder.

[0025] In a possible implementation, the chain transfer agent includes one or more of 3-mercaptopropionic acid, 3-mercaptoacetic acid, mercaptoethanol, n-butyl mercaptan, n-dodecyl mercaptan and isopropanol.

[0026] In a possible implementation manner, the added amount of the chain transfer agent accounts for 0.01% to 1% of the total mass of the monomer.

[0027] In a possible implementation, the inorganic salt includes one or more of sodium sulfite, sodium bisulfite, ammonium sulfite, potassium sulfite and potassium bisulfite;

[0028] The added amount of the inorganic salt accounts for 0.3% to 0.8% of the total mass of the monomer.

[0029] In a third aspect, the present application provides an oil well cement, comprising the retarder described in any one of the embodiments of the first aspect of the present application, and / or the retarder prepared by any one of the preparation methods of the second aspect of the present application.

[0030] The retarder for oil well cement and the preparation method thereof provided in the present application have the following beneficial effects compared with the prior art:

[0031] 1. The present application adopts a polymerization reaction of 2-acrylamide-2-methylpropanesulfonic acid monomer, an unsaturated carboxylic acid monomer and a rigid monomer to obtain a first polymer, and the imidazole group, carboxylic acid group and the like in the first polymer can improve the high temperature resistance of the retarder and regulate the thickening time of the cement slurry system under a high temperature environment; at the same time, in order to prevent the first polymer from having insufficient shrinkage ability under a high temperature environment, a second polymer is added to play a synergistic role with the first polymer, thereby further improving the shrinkage ability of the retarder under a high temperature environment and reducing the water loss.

[0032] 2. The first polymer in the present application has a rigid molecular structure, which improves the van der Waals force and porosity of the first polymer, and can improve the synergistic performance of the first polymer and the second polymer, so that there is a strong chemical reaction between the first polymer and the second polymer, so that the first polymer and the second polymer will not be separated in a high temperature environment, thereby reducing the synergistic effect between the first polymer and the second polymer. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0034] Figure 1 The present invention provides a process flow chart of a method for preparing a retarder for oil well cement.

[0035] The above drawings have shown clear embodiments of the present application, which will be described in more detail later. These drawings and text descriptions are not intended to limit the scope of the present application in any way, but to illustrate the concept of the present application to those skilled in the art by referring to specific embodiments. DETAILED DESCRIPTION

[0036] Exemplary embodiments will be described in detail herein, examples of which are shown in the accompanying drawings. When the following description refers to the drawings, the same numbers in different drawings represent the same or similar elements unless otherwise indicated. The implementations described in the following exemplary embodiments do not represent all implementations consistent with the present application. Instead, they are merely examples of devices and methods consistent with some aspects of the present application as detailed in the appended claims.

[0037] The technical solution of the present application and how the technical solution of the present application solves the above-mentioned technical problems are described in detail below with specific embodiments. The following specific embodiments can be combined with each other, and the same or similar concepts or processes may not be repeated in some embodiments. The embodiments of the present application will be described below in conjunction with the accompanying drawings.

[0038] The retarder provided in the embodiment of the present application is prepared by the following preparation method:

[0039] S101, adding 2-acrylamide-2-methylpropanesulfonic acid monomer, unsaturated carboxylic acid monomer and rigid monomer into deionized water, stirring to dissolve, and adjusting the pH value to 4-5;

[0040] S102, heating the mixed solution to 50-90° C., adding a chain transfer agent, and performing a polymerization reaction;

[0041] S103, adding the second polymer and water to the above reaction product, and then adding a photoinitiator and an emulsifier, and stirring under a nitrogen atmosphere;

[0042] S104, irradiating the stirred product with ultraviolet light for reaction, curing it, washing it with ethanol, and drying it to obtain a retarder.

[0043] The monomers in the first polymer are monomers corresponding to x, y, and z, respectively, obtained through polymerization reaction. For example, the monomer of the first polymer can be a 2-acrylamide-2-methylpropanesulfonic acid monomer, and the unsaturated acid monomer can be itaconic acid, methacrylic acid, or any monomer corresponding to the above structural formula y. Similarly, the rigid monomer can be any of the following:

[0044]

[0045] Example 1

[0046] A retarder, the preparation method comprising:

[0047] S201, adding 2-acrylamide-2-methylpropanesulfonic acid monomer, itaconic acid monomer and rigid monomer (1) into deionized water, stirring to dissolve, and adjusting the pH value to 4.5 with sodium hydroxide aqueous solution.

[0048] S202, raising the temperature of the mixed solution to 650°C, adding 0.1% of the total mass of the monomers as a chain transfer agent 3-mercaptopropionic acid, and carrying out a polymerization reaction.

[0049] S203, adding the second polymer polyurethane acrylic resin, water and 0.6% sodium sulfite of the total weight of the monomers to the above reaction product, and then adding 12% of the amount of the second polymer as photoinitiator α-hydroxyisobutyrophenone and 5% of the amount of the second polymer as emulsifier, and stirring under a nitrogen atmosphere.

[0050] S204, subjecting the stirred product to ultraviolet irradiation reaction, curing, washing with ethanol, and drying to obtain a retarder; wherein the ratio of the first polymer to the second polymer is 1 to 0.6.

[0051] Example 2

[0052] The only difference between this embodiment and embodiment 1 is that the rigid monomer uses a monomer of formula (2).

[0053] Example 3

[0054] The only difference between this embodiment and embodiment 1 is that the second polymer uses polyester acrylic resin, and the inorganic salt uses sodium bisulfite, ammonium sulfite and potassium sulfite in any proportion.

[0055] Comparative Example 1

[0056] The only difference between this comparative example and Example 1 is that there is no second polymer, and the preparation steps do not include step S203 and step S204.

[0057] Comparative Example 2

[0058] The only difference between this comparative example and comparative example 1 is that the first polymer monomer does not contain a rigid monomer.

[0059] Comparative Example 3

[0060] The only difference between this comparative example and comparative example 1 is that the first polymer monomer does not contain an unsaturated carboxylic acid monomer.

[0061] Performance Test:

[0062] The cement used in the test in this application is ordinary G-grade oil well cement, wherein the water-cement ratio is 0.44 to support the cement slurry, and the retarders of the above-mentioned Examples 1 to 3 and Comparative Examples 1 to 3 are added respectively, wherein the content of the retarder added accounts for 1.5% of the mass of the cement, and a fluid loss reducer (brand SCF-180L) accounting for 5% of the mass of the cement, as well as silica fume, etc. are added.

[0063] 1. Thickening time: The thickening time of cement slurry was tested according to the method described in standard GB / T19139-2015, where the test temperature was 160°C, the test time was 80 min, and the test pressure was 80 MPa.

[0064] 2. Compressive strength: The compressive strength of cement slurry was tested according to the method described in standard GB / T19139-2015. To meet the application condition of 80°C temperature difference, the test temperature was 80°C, the test time was 80 minutes, and the test pressure was 80 MPa.

[0065] 3. Stability: The stability of the retarder is tested according to the method described in SY / T5504.1-2013, and the test is conducted at room temperature, normal pressure, and in a sealed transparent container.

[0066] The above test results are shown in Table 1.

[0067] Table 1. Test results:

[0068]

[0069] It can be seen from Table 1 that the cement slurries with retarders in Examples 1 to 3 have better stability than the cement slurries with retarders added in proportions 1 to 3, and the cement slurries with retarders in Examples 1 to 3 have thickening times greater than 310 min, and the compressive strength of the cement solids is greater than 24 MPa.

[0070] 4. Thickening time: The thickening time of cement slurry was tested according to the method described in standard GB / T19139-2015, where the test temperature was 220°C, the test time was 80 min, and the test pressure was 80 MPa.

[0071] 5. Compressive strength: The compressive strength of cement slurry was tested according to the method described in standard GB / T19139-2015, where the test temperature was 160°C, the test time was 80 min, and the test pressure was 80 MPa.

[0072] The above test results are shown in Table 2.

[0073] Table 2. Test results:

[0074]

[0075] It can be seen from Table 2 that the cement slurry prepared with the retarder in Examples 1 to 3 of the present application has excellent high temperature resistance and stability.

[0076] It should be noted that, for the aforementioned method embodiments, for the sake of simplicity, they are all expressed as a series of action combinations, but those skilled in the art should be aware that the present application is not limited by the described order of actions, because according to the present application, certain steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also be aware that the embodiments described in the specification are all optional embodiments, and the actions and modules involved are not necessarily required by the present application.

[0077] In the above embodiments, the description of each embodiment has its own emphasis. For parts not described in detail in a certain embodiment, please refer to the relevant description of other embodiments. The technical features of the above embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0078] Those skilled in the art will readily appreciate other embodiments of the present application after considering the specification and practicing the invention disclosed herein. The present application is intended to cover any modification, use or adaptation of the present application, which follows the general principles of the present application and includes common knowledge or customary techniques in the art that are not disclosed in the present application. The specification and examples are intended to be exemplary only, and the true scope and spirit of the present application are indicated by the following claims.

[0079] It should be understood that the present application is not limited to the precise structures that have been described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof. The scope of the present application is limited only by the appended claims.

Claims

1. A retarder for oil well cement, characterized in that: The retarder comprises: a first polymer and a second polymer; The first polymer structural formula is as follows: Among them, the value range of x is 40 to 80, the value range of y is 15 to 35, and the value range of z is 10 to 18; The R1 is selected from any one of -H, -CH3, -CH2CH3, -COOCH3 or -CH2COOH; The R2 is selected from any one of -SO3H, -N(CH3)2, -NHCH2COOH or imidazole; The second polymer includes: polyurethane acrylic resin or polyester acrylic resin; The mass ratio of the first polymer to the second polymer is 1:0.4-0.

7.

2. The retarder for oil well cement according to claim 1, characterized in that: The retarder also includes water, and the water accounts for 50-60% of the total weight of the retarder.

3. The retarder for oil well cement according to claim 1, characterized in that: The retarder also includes a photoinitiator; The amount of the photoinitiator added is 5% to 18% of the second polymer.

4. The retarder for oil well cement according to claim 3, characterized in that: The photoinitiator is selected from α-hydroxyisobutyrophenone or 1-hydroxycyclohexylphenyl ketone.

5. The retarder for oil well cement according to claim 1, characterized in that: The retarder also includes an emulsifier, and the amount of the emulsifier added is 1% to 6% of the amount of the geopolymer; The emulsifier includes Spahn 80 and Tween 80 in a mass ratio of 1:1 to 1.

2.

6. A method for preparing a retarder for oil well cement, characterized in that: The preparation method comprises: Add 2-acrylamide-2-methylpropanesulfonic acid monomer, unsaturated carboxylic acid monomer and rigid monomer into deionized water, stir to dissolve, and adjust the pH value to 4-5; The mixed solution is heated to 50-90°C, a chain transfer agent is added, and a polymerization reaction is carried out; Adding the second polymer, water and inorganic salt to the above reaction product, and then adding a photoinitiator and an emulsifier, and stirring under a nitrogen atmosphere; The stirred product is irradiated with ultraviolet light for reaction, solidified, washed with ethanol, and dried to obtain the retarder.

7. The method for preparing a retarder for oil well cement according to claim 6, characterized in that: The chain transfer agent includes one or more of 3-mercaptopropionic acid, 3-mercaptoacetic acid, mercaptoethanol, n-butyl mercaptan, n-dodecyl mercaptan and isopropanol.

8. The method for preparing a retarder for oil well cement according to claim 7, characterized in that: The added amount of the chain transfer agent accounts for 0.01% to 1% of the total weight of the monomer.

9. The method for preparing a retarder for oil well cement according to claim 6, characterized in that: The inorganic salt includes one or more of sodium sulfite, sodium bisulfite, ammonium sulfite, potassium sulfite and potassium bisulfite; The added amount of the inorganic salt accounts for 0.3% to 0.8% of the total mass of the monomer.

10. An oil well cement, characterized in that: The cement comprises the retarder according to any one of claims 1 to 5, and / or the retarder prepared by the preparation method according to any one of claims 6 to 9.

Citation Information

Patent Citations

  • Polymer wide-temperature-zone retarder for oil-gas well cement and preparation method thereof

    CN103740350A

  • High-temperature-resistant copolymer oil well cement retarder and preparation method thereof

    CN104403056A

  • High-temperature-resistant and salt-resistant fluid loss agent and preparation method therefor

    CN105441040A

  • High-temperature-resistant oil-well cement retarder and preparation method thereof

    CN106085389A

  • Oil well cement high-temperature retarder microcapsule and preparation method thereof

    CN108570313A