Lightweight anti-radiation material prepared by foaming aluminum ash and preparation method of lightweight anti-radiation material

By mixing aluminum ash with industrial by-product gypsum and boron-containing compounds, lightweight radiation-proof materials with good mechanical and thermal insulation properties are prepared, which solves the problem of high cost of aluminum ash utilization and radiation-proof materials, and achieves low cost and high efficiency radiation resistance.

CN118978361APending Publication Date: 2024-11-19HUBEI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411011768.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing comprehensive utilization method of aluminum ash cannot take into account the environment and is prone to secondary pollution and has high costs. At the same time, the existing radiation-proof materials are costly and have limited shielding performance, making it difficult to meet the preparation needs of lightweight materials.

Method used

Solid waste such as aluminum ash and industrial by-product gypsum are used to mix it with boron-containing compounds to prepare lightweight radiation-proof materials with good mechanical properties and thermal insulation properties, and use the Al2O3 component of aluminum ash to enhance the radiation-proof ability of the material.

Benefits of technology

The lightweight radiation-proof material prepared has low density, moderate strength, good thermal insulation performance, and has a neutron shielding rate of 70-90%, meeting relevant standards and has good radiation-proof performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a light anti-radiation material prepared by foaming aluminum ash and a preparation method thereof, and the light anti-radiation material comprises the following components: a mixed dry material and aluminum ash accounting for 5-15% of the mass of the mixed dry material, wherein the mixed dry material is prepared by mixing a boron-containing compound, gypsum and cement clinker according to the mass ratio of (65-75): (10-20): (1-15). The invention provides a light anti-radiation material prepared by foaming aluminum ash and a preparation method of the light anti-radiation material, and the light anti-radiation material with better mechanical property and thermal insulation property is prepared from the aluminum ash, industrial byproduct gypsum and other solid wastes. The light anti-radiation material has certain anti-radiation capability on the basis of fully utilizing solid waste and ensuring density, strength and thermal insulation performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of solid waste resource utilization, and more specifically, to a lightweight radiation protection material prepared by foaming aluminum ash and a preparation method thereof. Background Art

[0002] As a byproduct of the aluminum industry, aluminum ash has been accumulating with the development of the aluminum industry. The existing comprehensive utilization of aluminum ash cannot take into account the environment and is prone to secondary pollution, and the cost is high. As one of the main ways and carriers of bulk solid waste consumption, concrete materials have the advantages of large volume and strong tolerance. At the same time, the Al and AlN components contained in aluminum ash can react with it to produce gas, which can replace aluminum powder as a gas generating agent to prepare lightweight cementitious materials. In addition, the Al2O3 component in aluminum ash is a high-quality high-aluminum material.

[0003] With the development of the nuclear industry, it is inevitable to face the harm caused by nuclear radiation. Concrete, which has a wide range of applications, has low cost and good shielding performance, and is an ideal radiation-proof material. At present, the radiation-proof cementitious materials mainly include barium cement, strontium cement and boron cement. Among them, boron cement can shield neutrons and meet the preparation conditions of lightweight materials. If boron compounds can be used in the preparation of lightweight cementitious materials by aluminum ash foaming, the radiation-proof ability of lightweight cementitious materials will be improved. Summary of the invention

[0004] The purpose of the present invention is to provide a lightweight radiation-proof material prepared by foaming aluminum ash and a preparation method thereof, and to use aluminum ash and solid waste such as industrial by-product gypsum to make a lightweight radiation-proof material with good mechanical properties and thermal insulation properties. The lightweight radiation-proof material not only fully utilizes solid waste, but also ensures density, strength and thermal insulation properties, and also has a certain radiation-proof ability.

[0005] In order to achieve these purposes and other advantages according to the present invention, a lightweight radiation protection material prepared by foaming aluminum ash is provided, comprising the following components:

[0006] Mix dry materials and 5-15% by mass of aluminum ash;

[0007] The mixed dry material includes a boron-containing compound, gypsum and cement clinker mixed in a mass ratio of 65-75:10-20:1-15.

[0008] Furthermore, in the lightweight radiation protection material prepared by foaming aluminum ash, the boron-containing compound is one or a mixture of any of borax, boraxite and boron oxide.

[0009] Furthermore, in the lightweight radiation protection material prepared by foaming aluminum ash, the aluminum ash includes the following components in percentage by mass:

[0010] Al2O3 40-70%, SiO2 5-15%, CaO 2-8%, Na2O 1-5%, Cl 1-5%, SO3 1-4%, Fe2O30.5-3% and MgO 0.1-8%.

[0011] Furthermore, in the lightweight radiation protection material prepared by foaming aluminum ash, the preparation method of the aluminum ash is as follows:

[0012] The aluminum ash raw material is magnetically separated and then ground into powder, and then passed through a 200-mesh sieve to obtain the aluminum ash.

[0013] The present invention also provides a method for preparing the lightweight radiation protection material described in any one of the above items, comprising the following steps:

[0014] S1. Evenly mix the boron-containing compound, gypsum and cement clinker to obtain a mixed dry material;

[0015] S2, adding water to the mixed dry materials obtained in S1 and stirring evenly, then adding aluminum ash and stirring at high speed to obtain foamed slurry;

[0016] S3, pouring the foam slurry obtained in S2 into a mold, and curing and molding it to obtain the lightweight radiation protection material.

[0017] Furthermore, in the method for preparing the lightweight radiation protection material, after adding water to the mixed dry materials in S2, the mixture is stirred at a stirring speed of 400-600 rpm for 2-5 minutes.

[0018] Furthermore, in the method for preparing the lightweight radiation protection material, after adding aluminum ash to S3, stirring is performed at a stirring speed of 800-1000 rpm for 0.5-2 min to obtain a foamed slurry;

[0019] Furthermore, in the method for preparing the lightweight radiation protection material, the curing temperature during curing in S3 is 20-40° C., the curing humidity is 50-70%, and the curing time is 12-24 hours.

[0020] The beneficial effects of the present invention are:

[0021] The present invention makes full use of solid wastes such as aluminum ash and industrial by-product gypsum to produce a lightweight radiation-proof material with good mechanical properties and thermal insulation properties. The density of the obtained lightweight radiation-proof test block is less than 530kg / m 3The porosity is 40-60%, which meets the B05 standard of "JC / T1062-2007-Foam Concrete Block"; the strength is 1.5-3.5MPa, which meets the A3.5 standard of "JC / T1062-2007-Foam Concrete Block". It also has good thermal insulation performance, and the neutron shielding rate can reach 70-90%, which has good radiation protection ability.

[0022] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. DETAILED DESCRIPTION

[0023] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.

[0024] It should be noted that the experimental methods described in the following embodiments are conventional methods unless otherwise specified, and the reagents and materials can be obtained from commercial channels unless otherwise specified.

[0025] Example 1

[0026] A method for preparing a lightweight radiation protection material comprises the following steps:

[0027] 75% by mass of cement clinker, 20% by mass of boron-containing compounds and 5% by mass of industrial by-product gypsum are weighed and mixed evenly to obtain a mixed dry material.

[0028] Add water to the mixed dry material and stir at a rate of 500 rpm for 3 minutes, then add aluminum ash with a mass of 15% of the mass of the mixed dry material, and stir at a rate of 1000 rpm for 1.5 minutes to obtain foamed concrete slurry.

[0029] The foamed concrete slurry was poured into a mold and placed in a curing room for curing for 18 hours. The curing temperature was controlled at 40°C and the curing humidity was maintained at 65% to obtain a lightweight radiation-proof test block.

[0030] The composition of the added aluminum ash is shown in Table 1 below:

[0031] Table 1 Analysis of main chemical components of aluminum ash (XRF)

[0032] Element <![CDATA[Al2O3]]> <![CDATA[SiO2]]> CaO <![CDATA[Na2O]]> Cl <![CDATA[SO3]]> <![CDATA[Fe2O3]]> MgO CuO ZnO <![CDATA[TiO2]]> <![CDATA[K2O]]> content,% 65.12 7.73 4.03 2.38 1.23 2.80 3.28 7.13 1.12 0.932 0.836 0.822

[0033] The lightweight radiation-proof test block provided in this embodiment was tested, and the test results showed that its density met the B05 standard, its strength met the A3.5 standard, and its neutron shielding rate reached 80%.

[0034] Example 2

[0035] A method for preparing a lightweight radiation protection material comprises the following steps:

[0036] 70% by mass of cement clinker, 20% by mass of boron-containing compounds and 10% by mass of industrial by-product gypsum are weighed and mixed evenly to obtain a mixed dry material.

[0037] Add water to the mixed dry materials and stir at a rate of 450 rpm for 2 minutes, then add aluminum ash whose mass is 10% of the mass of the mixed dry materials, and stir at a rate of 900 rpm for 1 minute to obtain foamed slurry.

[0038] The foamed concrete slurry was poured into a mold and placed in a curing room for curing for 12 hours. The curing temperature was controlled at 30°C and the curing humidity was maintained at 60% to obtain a lightweight radiation-proof test block.

[0039] Among them, the composition of the aluminum ash used in this embodiment is the same as that in Example 1.

[0040] The lightweight radiation-proof test block provided in this embodiment was tested, and the test results showed that its density met the B05 standard, its strength met the A3.5 standard, and its neutron shielding rate reached 70%.

[0041] Example 3

[0042] A method for preparing a lightweight radiation protection material comprises the following steps:

[0043] 65% by mass of cement clinker, 25% by mass of boron-containing compounds and 10% by mass of industrial by-product gypsum are weighed and mixed evenly to obtain a mixed dry material.

[0044] Add water to the mixed dry materials and stir at a rate of 600 rpm for 2 minutes, then add aluminum ash whose mass is 8% of the mass of the mixed dry materials, and stir at a rate of 1000 rpm for 1 minute to obtain foamed slurry.

[0045] The foamed concrete slurry was poured into a mold and placed in a curing room for curing for 20 hours. The curing temperature was controlled at 35°C and the curing humidity was maintained at 70% to obtain a lightweight radiation-proof test block.

[0046] Among them, the composition of the aluminum ash used in this embodiment is the same as that in Example 1.

[0047] The lightweight radiation-proof test block provided in this embodiment was tested, and the test results showed that its density met the B05 standard, its strength met the A3.5 standard, and its neutron shielding rate reached 75%.

[0048] In the above-mentioned embodiments 1-3, the test block uses a 252Cf neutron source, and the neutron transmittance of the sample is tested by a long counter, thereby calculating the neutron shielding rate of the test block. The selected isotope spontaneous fission neutron source 252Cf has an average energy of 2.28MeV for neutron emission. During the experiment, the total neutron emission rate of the source is 9.078×103s-1, and its energy spectrum meets the Watt spectrum distribution. The layout of this experiment is as follows: In order to reduce the reflection and scattering effects of the ground and the wall on neutrons, the measurement system is arranged on a steel structure platform 1.2m from the ground, the shortest distance from the wall is controlled at 2.8m, and the other three sides are more than 4m. The 252Cf spontaneous fission neutron source is aligned with the center height of the long counter, and the 252Cf spontaneous fission neutron source is adjusted in height using an appropriate bracket. When testing the sample, the sample is arranged close to the 252Cf spontaneous fission neutron source and is placed on the side close to the long counter.

[0049] In order to verify the beneficial effects of the lightweight radiation protection materials obtained in the above embodiments 1-3, comparative examples 1 and 2 are set as follows:

[0050] Comparative Example 1

[0051] A method for preparing a lightweight radiation-proof material by foaming aluminum ash, the method is the same as the preparation method in Example 1, the only difference is that the mass percentage of cement clinker in the mixed dry material is 50%, and the prepared lightweight radiation-proof test block can only meet the strength grade A1 requirement. Among them, the composition of the aluminum ash used in this comparative example is the same as that in Example 1.

[0052] Comparative Example 2

[0053] A method for preparing a lightweight radiation-proof material by foaming aluminum ash, the method is the same as the preparation method in Example 1, the only difference is that the mass percentage of the boron compound in the mixed dry material is 5%, and the neutron shielding rate of the prepared lightweight radiation-proof test block can only reach 20%. Among them, the composition of the aluminum ash used in this comparative example is the same as that in Example 1.

[0054] By comparing the results of Example 1 with those of Control Example 1, it can be seen that if the mass percentage of cement clinker in the mixed dry material is too high, the strength of the lightweight radiation-proof test block will be affected; by comparing the results of Example 2 with those of Control Example 2, it can be seen that if the mass percentage of boron compounds in the mixed dry material is too low, the radiation-proof ability of the lightweight radiation-proof test block will be affected.

[0055] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the embodiments shown and described herein.

Claims

1. A lightweight radiation protection material prepared by foaming aluminum ash, characterized in that: Includes the following components: Mix dry materials and 5-15% by mass of aluminum ash; The mixed dry material includes a boron-containing compound, gypsum and cement clinker mixed in a mass ratio of 65-75:10-20:1-15.

2. The lightweight radiation protection material prepared by foaming aluminum ash as claimed in claim 1, characterized in that: The boron-containing compound is one of borax, boraxite and boron oxide, or a mixture of any of the above.

3. The lightweight radiation protection material prepared by foaming aluminum ash as claimed in claim 1, characterized in that: The aluminum ash includes the following components in percentage by mass: Al2O3 40-70%, SiO2 5-15%, CaO 2-8%, Na2O 1-5%, Cl 1-5%, SO3 1-4%, Fe2O30.5-3% and MgO 0.1-8%.

4. The lightweight radiation protection material prepared by foaming aluminum ash as claimed in claim 3, characterized in that: The preparation method of the aluminum ash is as follows: The aluminum ash raw material is magnetically separated and then ground into powder, and then passed through a 200-mesh sieve to obtain the aluminum ash.

5. A method for preparing a lightweight radiation protection material according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1. Evenly mix the boron-containing compound, gypsum and cement clinker to obtain a mixed dry material; S2, adding water to the mixed dry materials obtained in S1 and stirring evenly, then adding aluminum ash and stirring at high speed to obtain foamed slurry; S3, pouring the foam slurry obtained in S2 into a mold, and curing and molding it to obtain the lightweight radiation protection material.

6. The method for preparing a lightweight radiation protection material according to claim 5, characterized in that: After adding water to the mixed dry materials in S2, stir at a stirring speed of 400-600 rpm for 2-5 minutes.

7. The method for preparing a lightweight radiation protection material according to claim 5, characterized in that: After adding aluminum ash to S3, stir at a stirring speed of 800-1000 rpm for 0.5-2 min to obtain foam slurry.

8. The method for preparing a lightweight radiation protection material according to claim 5, characterized in that: The curing temperature during curing in S3 is 20-40°C, the curing humidity is 50-70% and the curing time is 12-24h.