Aluminum zinc oxide target material and preparation method and application thereof
By mixing small-particle aluminum-zinc oxide powder with unsintered large-particle powder and then sintering, the problem of excessive density of aluminum-zinc oxide targets is solved, the thermal shock resistance and electrical conductivity are improved, the mechanical strength is increased, and the steaming is carried out. Maintain high deposition rate and excellent photoelectric properties during plating.
Patent Information
- Application Number
- CN202410880987.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-11-19
AI Technical Summary
Excessive density of existing aluminum oxide zinc targets leads to unstable evaporation, prone to cracking targets and film pores, and insufficient conductivity and mechanical strength.
Small-grain aluminum-zinc powder is mixed with unsintered large-grain powder and then sintered. Large-grain powder is used as a skeleton to improve the thermal shock resistance and bulk density of the target material, reduce porosity, and improve the conductivity through small-grain powder filling. and mechanical strength.
The preparation of low-density aluminum oxide targets is realized, which improves the thermal shock resistance and conductivity of the target, reduces the linear expansion coefficient, increases the mechanical strength, and maintains a high deposition rate and excellent photoelectricity during the evaporation process. performance.
Smart Images

Figure BDA0004924498680000061 
Figure BDA0004924498680000071 
Figure BDA0004924498680000081
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductors, and in particular to an aluminum zinc oxide target material and a preparation method and application thereof. Background Art
[0002] Tin-doped indium oxide (In d iμm Tin Oxide, referred to as I TO) is the most widely used transparent conductive film at present. The existing I TO film preparation methods are mainly magnetron sputtering and vacuum evaporation. The magnetron sputtering method is mainly used for high-density I TO target materials, and the relative density of the target materials is greater than 99%. The principle of vacuum evaporation is to heat the low-density I TO target materials. Due to its low density, it evaporates and deposits on the substrate that needs to be coated. Evaporation coating uses the evaporation of evaporation materials under vacuum and high temperature to form a thin film and deposit it on the base material. It has the characteristics of convenient operation and high deposition rate. Generally, low-density evaporation materials are selected. The evaporated film has uniform purity, high density, unique film structure and performance, moderate hardness and excellent photoelectric properties. And because evaporation has the characteristics of fast deposition rate, too high target density will lead to unstable evaporation, cracked targets, easy to cause pores in the evaporation film, low density and tortuosity, and a tendency of insufficient film strength.
[0003] Chinese patent application 202311187610.2 discloses a high-density and high-uniformity zinc oxide aluminum target and a preparation method thereof. The preparation method is: small-particle zinc oxide aluminum powder with a particle size of 0.3 to 0.8 μm and large-particle zinc oxide aluminum powder with a particle size of 1 to 1.5 μm are mixed to obtain a mixed powder, and the mixed powder is sequentially subjected to molding, cold isostatic pressing, degreasing heat treatment, and sintering to obtain a high-density zinc oxide aluminum target.
[0004] In this scheme, unsintered small-particle zinc oxide aluminum powder is mixed with large-particle zinc oxide aluminum powder and then sintered to improve the target material density and conductivity.
[0005] Chinese patent application 201510344609.5 discloses a method for preparing a zinc oxide evaporation target with a skeleton network structure, the preparation method comprising: sintering zinc hydroxide, zinc gallium hydroxide, zinc aluminum hydroxide, zinc titanium hydroxide or zinc indium hydroxide at high temperature to obtain a powder corresponding to 2 μm to 12 μm, adding one or more of zinc oxide nanopowder, zinc oxide crushed particles, and hydroxide slurry to mix, then adding a binder to press into shape, and obtaining a zinc oxide evaporation target after high temperature sintering.
[0006] This solution uses sintered hydroxides and other types of oxides for mixed sintering to improve the target material density and conductivity.
[0007] It cannot be seen that the above two schemes use unsintered small-particle material and large-particle material mixed sintering, and sintered small-particle hydroxide and oxide mixed and then sintered to improve the target density and conductivity.
[0008] The problem that this solution needs to solve: How to propose a method for preparing low-density evaporation targets. Summary of the invention
[0009] The purpose of the present invention is to provide an aluminum zinc oxide target material and a preparation method and application thereof, wherein small-particle sintered powder is mixed with unsintered large-particle powder and then sintered, wherein the large-particle powder plays a skeleton role, improves the thermal shock resistance of the target material and reduces the linear expansion coefficient, and reduces the scrap rate of roasting; at the same time, the small-particle powder is used to fill the gaps between the large-particle powders, which is beneficial to improve the volume density and electrical conductivity of the target material, reduce the porosity, and increase the mechanical strength.
[0010] To achieve the above object, the present application discloses a method for preparing an aluminum zinc oxide target, which comprises the following steps:
[0011] Step 1: calcine aluminum zinc oxide powder in a crucible, sieve, and obtain powder 1;
[0012] Step 2: Spray the binder solution onto the powder 1 in step 1 and dry it to obtain powder 2;
[0013] Step 3: Mix the powder 2 in step 2 with aluminum zinc oxide powder, adjust the water content, and obtain powder 3;
[0014] Step 4: Granulate the powder in step 3, perform compression molding, and sinter to obtain an aluminum zinc oxide target;
[0015] The particle sizes of the aluminum zinc oxide powder in step 1 and the aluminum zinc oxide powder in step 3 are both 50-300 nm, and the mass ratio of the two is 95-98:2-5.
[0016] Preferably, the calcination process of step 1 is: calcination temperature is 1350-1500° C., heating rate is 3-5° C. / min, holding time is 8-12h, and cooling rate is 3-5° C. / min.
[0017] Preferably, the crucible in step 1 is an alumina crucible, and the mesh size of the sieve used for sieving is 80 to 200 meshes.
[0018] Preferably, in step 2, the mass ratio of the binder to deionized water in the binder solution is 2:1.
[0019] Preferably, the binder in step 2 is a mixture of polyvinyl alcohol and polyethylene glycol, polyvinyl alcohol or polyvinyl butyral, or one or more thereof, and the amount of the binder is 1% to 5% of the mass of the powder.
[0020] Preferably, in step 3, the mass ratio of powder 2 to aluminum zinc oxide powder is 10:1-2.
[0021] Preferably, the moisture content of the powder three in step 3 is 1% to 3%.
[0022] Preferably, the sintering process of step 4 is: heating to 300-600°C at a heating rate of 0.1-0.5°C / min, keeping warm for 6-12h; then heating to 1150-1350°C at a heating rate of 0.5-1°C / min, keeping warm for 8-20h, and then cooling to 50°C at a heating rate of 1°C / min.
[0023] In addition, it also includes an aluminum zinc oxide target material, which is prepared by a preparation scheme of an aluminum zinc oxide target material.
[0024] In addition, it also includes a vapor deposition target material, which is made of aluminum zinc oxide target material.
[0025] The beneficial effects of the present invention are:
[0026] The invention provides a method for preparing an aluminum zinc oxide target material. By mixing sintered small-particle aluminum zinc oxide powder with unsintered large-particle aluminum zinc oxide powder and then sintering, the thermal shock resistance of the target material and the linear expansion coefficient of the target material can be improved, and since the small-particle aluminum zinc oxide powder has been sintered once, the distance between the particles gradually decreases, the interconnected pores gradually shrink into closed pores, and then gradually spheroidize, the strength and density of the powder increase, and the alloying state is presented, so that its shape is fixed, resulting in no more shrinkage during the second sintering, thereby obtaining a low-density aluminum zinc oxide target material with a density of 55% to 65%. During use, the evaporation target material has a high deposition rate. Too high density of the target material will lead to unstable evaporation, cracked targets, and easy to cause pores in the evaporated film, low density and tortuosity, insufficient film strength and other performance problems. The low-density target material is selected during evaporation, and due to the high deposition rate, the evaporated film has excellent photoelectric properties such as uniform purity, high density, and moderate hardness. DETAILED DESCRIPTION
[0027] In the description of the present invention, it should be noted that, if the specific conditions are not specified in the examples, the experiments were carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.
[0028] Example 1
[0029] Step 1: put aluminum zinc oxide powder with a particle size of 200 nm into an alumina crucible and calcine it at a temperature of 1400°C and a heating rate of 4°C / min. Keep the temperature for 10 hours, cool it to room temperature, and sieve it through an 80-mesh sieve to obtain powder 1;
[0030] Step 2: prepare a solution of polyvinyl alcohol with a mass of 3% of the mass of powder 1, spray it on powder 1 in step 1, and dry it in an oven at 120° C. to obtain powder 2;
[0031] Step 3: Mix the powder 2 in step 2 with aluminum zinc oxide powder with a particle size of 200 nm at a mass ratio of 10:1.5, and adjust the water content to 2% of the total mass to obtain powder 3;
[0032] Step 4: Granulate the powder in step 3, perform compression molding, and sinter to obtain an aluminum zinc oxide target;
[0033] The sintering process in step 4 is as follows: heating to 450°C at a heating rate of 0.3°C / min, keeping the temperature for 9 hours; then heating to 1250°C at a heating rate of 0.8°C / min, keeping the temperature for 14 hours, and then cooling to 50°C at a heating rate of 1°C / min.
[0034] Example 2
[0035] It is basically the same as Example 1, except that the particle size of the aluminum zinc oxide powder in step 1 and step 3 is 300 nm.
[0036] Example 3
[0037] It is basically the same as Example 1, except that the particle size of the aluminum zinc oxide powder in step 1 and step 3 is 50 nm.
[0038] Example 4
[0039] The method is basically the same as Example 1, except that in step 2, the mass of polyvinyl alcohol is 1% of the mass of the powder.
[0040] Example 5
[0041] The method is basically the same as Example 1, except that in step 2, the mass of polyvinyl alcohol is 5% of the mass of powder 1.
[0042] Example 6
[0043] It is basically the same as Example 1, except that in step 3, the mass ratio of powder 2 to aluminum zinc oxide powder is 10:1.
[0044] Example 7
[0045] It is basically the same as Example 1, except that in step 3, the mass ratio of powder 2 to aluminum zinc oxide powder is 10:2.
[0046] Example 8
[0047] It is basically the same as Example 1, except that the sintering process in step 4 is: heating to 300°C at a heating rate of 0.1°C / min, keeping warm for 6 hours; then heating to 1150°C at a heating rate of 0.5°C / min, keeping warm for 8 hours, and then cooling to 50°C at a heating rate of 1°C / min.
[0048] Example 9
[0049] It is basically the same as Example 1, except that the sintering process in step 4 is: heating to 600°C at a heating rate of 0.5°C / min, keeping warm for 12 hours; then heating to 1350°C at a heating rate of 1°C / min, keeping warm for 20 hours, and then cooling to 50°C at a heating rate of 1°C / min.
[0050] Comparative Example 1
[0051] Step 1: Sieve the aluminum zinc oxide powder through an 80-mesh sieve to obtain powder 1;
[0052] Step 2: prepare a solution of polyvinyl alcohol with a mass of 3% of the mass of powder 1, spray it on powder 1 in step 1, and dry it in an oven at 120° C. to obtain powder 2;
[0053] Step 3: Mix the powder 2 in step 2 with aluminum zinc oxide powder with a particle size of 200 nm at a mass ratio of 10:1.5, and adjust the water content to 2% of the total mass to obtain powder 3;
[0054] Step 4: Granulate the powder in step 3, perform compression molding, and sinter to obtain an aluminum zinc oxide target;
[0055] The sintering process in step 4 is as follows: heating to 450°C at a heating rate of 0.3°C / min, keeping the temperature for 9 hours; then heating to 1250°C at a heating rate of 0.8°C / min, keeping the temperature for 14 hours, and then cooling to 50°C at a heating rate of 1°C / min.
[0056] Comparative Example 2
[0057] The method is basically the same as Example 1, except that in step 3, powder 2 is mixed with zinc oxide powder with a particle size of 200 nm in a mass ratio of 10:1.5, and the water content is adjusted to 2% of the total mass to obtain powder 3.
[0058] Comparative Example 3
[0059] The method is basically the same as Example 1, except that in step 3, powder 2 is mixed with a mixed powder of aluminum oxide and zinc oxide, both of which have a particle size of 200 nm and a molar ratio of aluminum to zinc of 0.5 to 0.8, at a mass ratio of 10:1.5, and the water content is adjusted to 2% of the total mass to obtain powder 3.
[0060] Comparative Example 4
[0061] It is basically the same as Comparative Example 1, except that the particle size of the powder obtained in step 1 is 200 nm.
[0062] Performance Testing
[0063] Density measurement method: The density of the target material is measured by the Archimedes drainage method;
[0064] Conductivity measurement method: four-probe method.
[0065] The test results are shown in Table 1:
[0066] Table 1
[0067]
[0068]
[0069] Results Analysis
[0070] 1. It can be seen from Example 1 and Comparative Example 1 that in Example 1, the aluminum zinc oxide powder of step 1 was pre-sintered, while in Comparative Example 1, it was used directly without sintering. The density of the aluminum zinc oxide target prepared in Example 1 was increased by 10% and the conductivity was increased by 98.509uS.cm compared with the aluminum zinc oxide target prepared in Comparative Example 1.
[0071] It can be seen that pre-sintering the aluminum zinc oxide powder in step 1 is beneficial to improving the relative density and conductivity of the target material;
[0072] 2. It can be seen from Example 1 and Comparative Example 4 that in Example 1, the particle size of the powder 1 in step 1 is greater than 200 nm after being sieved through an 80-mesh sieve, and the particle size of the aluminum oxide zinc powder in step 3 is 200 nm;
[0073] In Comparative Example 4, the particle size of the powder in step 1 and the particle size of the aluminum zinc oxide powder in step 3 are both 200 nm;
[0074] The properties of the aluminum zinc oxide target prepared by the above process are shown in Table 2:
[0075] Table 2
[0076]
[0077] It can be seen that by mixing the large particles of powder 1 with the small particles of aluminum zinc oxide powder and then sintering, a structure with large particles of powder as the skeleton and small particles of powder as filling is formed, which improves the conductivity of the target material and increases the mechanical strength of the target material.
[0078] 3. It can be seen from Example 1 and Comparative Examples 2-3 that in Example 1, the powder 2 in the step is mixed with aluminum zinc oxide powder with a particle size of 200 nm at a mass ratio of 10:1.5, and the water content is adjusted to 2% of the total mass to obtain powder 3;
[0079] In comparative example 2, the powder 2 in step 3 is mixed with zinc oxide powder with a particle size of 200 nm at a mass ratio of 10:1.5, and the water content is adjusted to 2% of the total mass to obtain powder 3;
[0080] In comparative example 3, the powder 2 in step 3 and a mixed powder of aluminum oxide and zinc oxide with a particle size of 200 nm and a molar ratio of aluminum to zinc of 0.5 to 0.8 are mixed at a mass ratio of 10:1.5, and the water content is adjusted to 2% of the total mass to obtain powder 3;
[0081] The properties of the aluminum zinc oxide target prepared by the above process are shown in Table 3:
[0082] Table 3
[0083] Group Relative density% Conductivity uS.cm Example 1 60 311.176 Comparative Example 2 46 164.578 Comparative Example 3 51 186.461
[0084] It can be seen that, under the premise of the same particle size, among the zinc oxide powder, the mixture of zinc oxide and aluminum oxide with the same molar ratio of aluminum element to zinc element as that in the aluminum oxide zinc powder, and the aluminum oxide zinc powder, the aluminum oxide zinc target prepared by using the same powder as the aluminum oxide zinc powder in step 1 has better performance.
[0085] It can be seen from Example 1 and Examples 6-7 that when the mass ratio of powder 2 to aluminum zinc oxide is 10:1 or 10:2, the performance of the aluminum zinc oxide target obtained is worse than that of the aluminum zinc oxide powder obtained when the mass ratio of powder 2 to aluminum zinc oxide is 10:1.5;
[0086] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention shall be equivalent replacement methods and shall be included in the protection scope of the present invention.
Claims
1. A method for preparing an aluminum zinc oxide target, characterized in that: The following steps are included: Step 1: calcine aluminum zinc oxide powder in a crucible, sieve, and obtain powder 1; Step 2: Spray the binder solution onto the powder 1 in step 1, and dry it to obtain powder 2; Step 3: Mix the powder 2 in step 2 with aluminum zinc oxide powder, adjust the water content, and obtain powder 3; Step 4: Granulate the powder in step 3, perform compression molding, and sinter to obtain an aluminum zinc oxide target; The particle sizes of the aluminum zinc oxide powder in step 1 and the aluminum zinc oxide powder in step 3 are both 50-300 nm, and the mass ratio of the two is 95-98:2-5.
2. The method for preparing an aluminum zinc oxide target according to claim 1, characterized in that: The calcination process of step 1 is as follows: the calcination temperature is 1350-1500° C., the heating rate is 3-5° C. / min, the heat preservation time is 8-12h, and the cooling rate is 3-5° C. / min.
3. The method for preparing an aluminum zinc oxide target according to claim 1, characterized in that: The crucible in step 1 is an alumina crucible, and the mesh number of the sieve used for sieving is 80 to 200 meshes.
4. The method for preparing an aluminum zinc oxide target according to claim 1, characterized in that: In the step 2, the mass ratio of the binder to the deionized water in the binder solution is 2:
1.
5. The method for preparing an aluminum zinc oxide target according to claim 1, characterized in that: The binder in step 2 is a mixture of polyvinyl alcohol and polyethylene glycol, polyvinyl alcohol or polyvinyl butyral or more, and the amount of the binder is 1% to 5% of the mass of the powder.
6. The method for preparing an aluminum zinc oxide target according to claim 1, characterized in that: In the step 3, the mass ratio of the second powder to the aluminum zinc oxide powder is 10:1-2.
7. The method for preparing an aluminum zinc oxide target according to claim 1, characterized in that: The moisture content of the powder three in step 3 is 1% to 3%.
8. The method for preparing an aluminum zinc oxide target according to claim 1, characterized in that: The sintering process of step 4 is as follows: heating to 300-600°C at a heating rate of 0.1-0.5°C / min, and keeping the temperature for 6-12 hours; then heating to 1150-1350°C at a heating rate of 0.5-1°C / min, and keeping the temperature for 8-20 hours; then cooling to 50°C at a cooling rate of 1°C / min.
9. An aluminum zinc oxide target, characterized in that: The target is prepared by the method for preparing the aluminum zinc oxide target described in any one of claims 1 to 8.
10. A vapor deposition target, characterized in that: It is made from the aluminum zinc oxide target material described in claim 9.
Citation Information
Patent Citations
Preparation method of zinc oxide evaporation target with skeleton network structure
CN104987060A
Preparation method of secondary phase controllable zinc-aluminum oxide sputtering target material
CN113149633A
Preparation method of indium tin oxide evaporation target material
CN113185279A
Method for preparing low-density ITO (Indium Tin Oxide) target material for evaporation by sanding process
CN115959897A
Low-density ITO (indium tin oxide) target material for evaporation prepared by sanding process and preparation method of low-density ITO target material
CN116903361A