Diamine compound, polyimide, polyimide film and preparation method thereof
By introducing benzozoles and fat ring structures into diamine compounds, the problem of difficult to take into account the color and high temperature resistance of the polyimide film, and a polyimide film with excellent heat resistance and transparency was prepared. Suitable for photoelectric display and solar substrates.
Patent Information
- Application Number
- CN202411070729.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-06
AI Technical Summary
The color of the traditional aromatic polyimide film is yellow or dark brown, which limits its application in transparent flexible substrates and transparent circuit boards, and it is difficult to achieve high optical transmittance and high temperature resistance at the same time.
By introducing benzozole structures and fat ring structures into diamine compounds, the molecular chain rigidity and flexibility and charge transfer interactions are balanced, and a polyimide film with excellent heat resistance and transparency is prepared.
It achieves high comprehensive performance of polyimide film, is suitable for photoelectric display and solar substrates and other fields, with good heat resistance and transparency.
Smart Images

Figure CN118978492A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer materials, and in particular to a diamine compound, a polyimide, a polyimide film and a preparation method thereof. Background Art
[0002] Polyimide is a type of polymer material obtained by the polymerization of dianhydride and diamine. It has excellent high and low temperature resistance, mechanical properties and radiation resistance, and has the advantage of adjustable molecular structure. It is widely used in national defense and military industry as well as civilian high-tech fields. Traditional aromatic polyimide films are yellow or dark brown in color, which limits their application in transparent flexible substrates and transparent circuit boards. Therefore, while maintaining the excellent heat resistance of polyimide, improving its transparency has become a research hotspot in related fields.
[0003] Numerous studies have shown that the charge transfer (CT) effect of electron donor diamine and electron acceptor dianhydride exists in polyimide molecules, and the color of the film is mainly affected by it. The weaker the CT effect, the lighter the color. In order to reduce the CT effect in polyimide molecules, there are mainly the following strategies based on molecular structure design: (1) introducing alicyclic structures such as cyclobutane, cyclohexane and other structures into the main chain of the molecule (CN116574260A, CN116425976A, CN116178388A); (2) introducing fluorine-containing groups, such as -CF3 and -F structures (CN116478402A, CN116253879A, CN115894258A); (3) introducing bulky side groups or non-coplanar structures (CN116535411A, CN104119532A, CN115557848A). Fluorine-containing groups can effectively inhibit the CT interaction of polyimide and improve the optical transparency of the film. However, fluorine-containing group monomers are generally expensive, which increases the cost of commercialization of polyimide. The introduction of fluorine-containing groups will also reduce the thermal and mechanical properties of the film. The introduction of alicyclic structures into the polyimide molecular chain can also weaken the CT effect, thereby improving the optical transparency of the polyimide film, but the alicyclic structure is not thermally stable enough, which reduces the thermal properties of the film. It is often difficult to achieve high optical transmittance and high temperature resistance of polyimide films at the same time. Therefore, how to achieve a good balance between optical and thermodynamic properties of polyimide films has become a design difficulty. In addition, the heat resistance of polyimide films is related to factors such as molecular chain rigidity and interchain interactions. The key to developing high-performance polyimide films is to conduct reasonable molecular structure design and balance the comprehensive performance of the film. Summary of the invention
[0004] In view of this, the present invention provides a diamine compound, a polyimide, a polyimide film and a preparation method thereof. The polyimide film prepared using the diamine compound provided by the present invention as a raw material has both heat resistance and transparency and has good comprehensive performance.
[0005] The present invention provides a diamine compound having a structure of formula (I) or formula (II):
[0006]
[0007] Wherein, X is selected from O or NH; and n is selected from an integer of 1 to 5.
[0008] In some specific implementations, n is 1, 2, 3, 4 or 5, preferably n is 1 or 2 or 3, and more preferably n is 1.
[0009] The present application introduces a benzoazole (such as benzoxazole or benzimidazole) structure and an aliphatic ring (such as cyclohexane) structure into the diamine compound structure, which can balance the rigidity and flexibility of the molecular chain and the charge transfer interaction. The polyimide film prepared with it as the raw material has excellent heat resistance and transparency, and can be applied to optoelectronic displays, solar substrates and other fields.
[0010] In some specific implementations, the diamine compound of the formula (I) has the structures of formula (I-1) and (I-2):
[0011]
[0012] The diamine compounds of formula (I-1) and (I-2) have a cis-trans structure, which can enhance the interaction force between molecules and improve the stability of the compound.
[0013] In some specific implementations, formula (I-1) has the structures of (I-1a) and (I-1b):
[0014]
[0015]
[0016] The diamine compounds of the formula (I-1a) and (I-1b) have a benzoxazole structure or a benzimidazole structure, which can enhance the strength of hydrogen bonds within the molecule, thereby improving the rigidity of the molecule.
[0017] In some specific implementations, formula (I-1a) has the structures of (I-1a-1) and (I-1a-2):
[0018]
[0019] The substitution position of benzoxazole and cyclohexane in the diamine compound of formula (I-1a-1) is the para position, which can reduce the steric hindrance effect between the substituents and improve the reaction yield; the substitution position of benzoxazole and cyclohexane in the diamine compound of formula (I-1a-2) is the meta position, which can improve the reaction activity of the diamine compound and shorten the time for the polymerization reaction to occur.
[0020] In some specific implementations, formula (I-1b) has the structures of (I-1b-1) and (I-1b-2):
[0021]
[0022] The substitution position of benzimidazole and cyclohexane in the diamine compound of formula (I-1b-1) is the para position, which can reduce the steric hindrance effect between the substituents and improve the reaction yield; the substitution position of benzimidazole and cyclohexane in the diamine compound of formula (I-1b-2) is the meta position, which can improve the reaction activity of the diamine compound and shorten the time for the polymerization reaction to occur.
[0023] In some specific implementations, formula (I-2) has the structures of (I-2a) and (I-2b):
[0024]
[0025] The diamine compounds of the formula (I-2a) and (I-2b) have a benzoxazole structure or a benzimidazole structure, which can enhance the strength of hydrogen bonds within the molecule, thereby improving the rigidity of the molecule.
[0026] In some specific implementations, formula (I-2a) has the structures of (I-2a-1) and (I-2a-2):
[0027]
[0028] The substitution position of benzoxazole and cyclohexane in the diamine compound of formula (I-2a-1) is the para position, which can reduce the steric hindrance effect between the substituents and improve the reaction yield; the substitution position of benzoxazole and cyclohexane in the diamine compound of formula (I-2a-2) is the meta position, which can improve the reaction activity of the diamine compound and shorten the time for the polymerization reaction to occur.
[0029] In some specific implementations, formula (I-2b) has the structures of (I-2b-1) and (I-2b-2):
[0030]
[0031] The substitution position of benzimidazole and cyclohexane in the diamine compound of formula (I-2b-1) is the para position, which can reduce the steric effect between the substituents and improve the reaction yield; the substitution position of benzimidazole and cyclohexane in the diamine compound of formula (I-2b-2) is the meta position, which can improve the reaction activity of the diamine compound and shorten the time for the polymerization reaction to occur.
[0032] In some specific implementations, the diamine compound of the formula (II) has the structures of formula (II-1) and (II-2):
[0033]
[0034] The diamine compounds of formula (II-1) and (II-2) have a cis-trans structure, which can enhance the interaction force between molecules and improve the stability of the compound.
[0035] In some specific implementations, formula (II-1) has the structures of (II-1a) and (II-1b):
[0036]
[0037] The diamine compounds of the formula (II-1a) and (II-1b) have a benzoxazole structure or a benzimidazole structure, which can enhance the strength of hydrogen bonds within the molecule, thereby improving the molecular rigidity.
[0038] In some specific implementations, formula (II-1a) has the structures of (II-1a-1) and (II-1a-2):
[0039]
[0040] The substitution position of benzoxazole and cyclohexane in the diamine compound of formula (II-1a-1) is the para position, which can reduce the steric hindrance effect between the substituents and improve the reaction yield; the substitution position of benzoxazole and cyclohexane in the diamine compound of formula (II-1a-2) is the meta position, which can improve the reaction activity of the diamine compound and shorten the time for the polymerization reaction to occur.
[0041] In some specific implementations, formula (II-1b) has the structures of (II-1b-1) and (II-1b-2):
[0042]
[0043] The substitution position of benzimidazole and cyclohexane in the diamine compound of formula (II-1b-1) is the para position, which can reduce the steric hindrance effect between the substituents and improve the reaction yield; the substitution position of benzimidazole and cyclohexane in the diamine compound of formula (II-1b-2) is the meta position, which can improve the reaction activity of the diamine compound and shorten the time for the polymerization reaction to occur.
[0044] In some specific implementations, formula (II-2) has the structures of (II-2a) and (II-2b):
[0045]
[0046]
[0047] The diamine compounds of the formula (II-2a) and (II-2b) have a benzoxazole structure or a benzimidazole structure, which can enhance the strength of the hydrogen bond within the molecule, thereby improving the molecular rigidity.
[0048] In some specific implementations, formula (II-2a) has the structures of (II-2a-1) and (II-2a-2):
[0049]
[0050] The substitution position of benzoxazole and cyclohexane in the diamine compound of formula (II-2a-1) is the para position, which can reduce the steric hindrance effect between the substituents and improve the reaction yield; the substitution position of benzoxazole and cyclohexane in the diamine compound of formula (II-2a-2) is the meta position, which can improve the reaction activity of the diamine compound and shorten the time for the polymerization reaction to occur.
[0051] In some specific implementations, formula (II-2b) has the structures of (II-2b-1) and (II-2b-2):
[0052]
[0053] The substitution position of benzimidazole and cyclohexane in the diamine compound of formula (II-2b-1) is the para position, which can reduce the steric hindrance effect between the substituents and improve the reaction yield; the substitution position of benzimidazole and cyclohexane in the diamine compound of formula (II-2b-2) is the meta position, which can improve the reaction activity of the diamine compound and shorten the time for the polymerization reaction to occur.
[0054] The present invention also provides a method for preparing a diamine compound, comprising:
[0055] A cycloalkane compound having a structure of formula (III), an aniline compound having a structure of formula (IV) or formula (V) and a reducing agent undergo a first reaction in an inert atmosphere, and then undergo a second reaction with a dehydrating agent to obtain a diamine compound represented by formula (I) or formula (II);
[0056]
[0057] Wherein, R3 is hydroxyl, R1 and R2 are independently acyl chloride, carboxyl or amino; or R3 is amino, R1 and R2 are independently acyl chloride, carboxyl or hydroxyl;
[0058] X is selected from O or NH;
[0059] n is an integer selected from 1-5.
[0060] The present invention uses a cycloalkane compound having a structure of formula (III) and an aniline compound having a structure of formula (IV) or formula (V) as raw materials, and first undergoes a first reaction under a reducing agent and an inert atmosphere to activate each reactant; then a dehydrating agent is added to undergo a second reaction, during which the amino group and R3 in the aniline compound condense with R1 or R2 in the cycloalkane compound to form a ring, thereby obtaining a diamine compound. Specifically, the diamine compound having a structure of formula (I) or formula (II) can be synthesized according to the route shown in the following scheme:
[0061]
[0062] Wherein, in the structure of formula (IV) or formula (V), R3 is selected from hydroxyl or amino; correspondingly, in the structure of formula (III), R1 or R2 is selected from a group that can undergo condensation ring reaction with hydroxyl or amino, such as acyl chloride, carboxyl, amino or hydroxyl. Specifically, R3 is hydroxyl, R1 and R2 are independently acyl chloride, carboxyl or amino; or R3 is amino, R1 and R2 are independently acyl chloride, carboxyl or hydroxyl. In formula (III), n is an integer of 1 to 5, for example, it can be 1, 2, 3, 4 or 5.
[0063] The above reaction is carried out in a solvent, and the solvent includes but is not limited to one or more of boric acid, concentrated sulfuric acid and polyphosphoric acid, preferably polyphosphoric acid. The present invention first heats the solvent, adds the cycloalkane compound and the reducing agent, and adds the aniline compound in batches under an inert atmosphere. After the addition is completed, stirring is continued to complete the first reaction.
[0064] In some specific implementations, the solvent is first heated to 40-80°C, preferably 45-75°C, more preferably 50-70°C, and then the reaction raw materials and catalyst are added to react. In some specific implementations, the mass ratio of the solvent to the cycloalkane compound is 15-30:1, preferably 20-30:1. In some specific implementations, the molar ratio of the cycloalkane compound to the aniline compound is 1:0.5-2, preferably 1:1-2. In some specific implementations, the reducing agent includes but is not limited to tin powder and stannous chloride, preferably stannous chloride, and the molar ratio of the reducing agent to the cycloalkane compound is 1-10:100, preferably 3-8:100. In some specific implementations, the time of the first reaction is 5-10h, preferably 6-9h, more preferably 7-8h. In some specific implementations, the inert atmosphere is preferably a nitrogen or argon atmosphere, more preferably a nitrogen atmosphere.
[0065] After the first reaction is completed, a dehydrating agent is added to the reaction system to carry out a second reaction, and a diamine compound is obtained after the reaction is complete.
[0066] In some specific implementations, the dehydrating agent includes but is not limited to phosphorus pentoxide, and the molar ratio of the dehydrating agent to the cycloalkane compound is 0.5 to 2:1, preferably 0.6 to 1.5:1, and more preferably 0.75 to 1.25:1. In some specific implementations, the temperature of the second reaction is 170 to 220°C, preferably 180 to 210°C, and more preferably 190 to 200°C. In some specific implementations, the time of the second reaction is 5 to 16 hours, preferably 7 to 14 hours, and more preferably 8 to 10 hours.
[0067] In some specific implementations, after obtaining the diamine compound, post-treatment is further included, and the post-treatment includes cooling, adjusting the solution pH, removing impurities and drying.
[0068] In some specific implementations, the cooling temperature is preferably room temperature. In some specific implementations, it is preferred to adjust the solution pH to 7-10, more preferably 8-9. In some specific implementations, the reagent used to adjust the solution pH is a saturated sodium carbonate solution. In some specific implementations, the impurity removal method includes but is not limited to filtering and washing. In some specific implementations, the solvent used for washing can be water or ethanol, and the washing is 1 to 5 times, preferably 2 to 4 times. This product has no special restrictions on the methods of filtering, washing and drying.
[0069] This application prepares high-performance transparent polyimide (CPI) films through molecular multi-level synchronous design, and synthesizes a series of diamines containing benzoazoles and aliphatic ring structures. First, the introduction of benzoazole structures increases the rigidity and linearity of the molecular chain, giving the film excellent heat resistance; secondly, the introduction of aliphatic ring structures inhibits the CT effect in the molecular chain and improves the optical properties of the film. This application combines the advantages of each monomer through copolymerization reactions, regulates the comprehensive performance of the film, and obtains high-performance CPI films with broad application prospects in the fields of flexible electronics and spacecraft thermal management.
[0070] The present invention also provides a polyimide having a structure of formula (VI) or formula (VII):
[0071]
[0072] Where k is the repeating unit in the polymer molecule The ratio of , 0≤k≤0.5;
[0073] X is selected from O or NH;
[0074] n is an integer selected from 1 to 5;
[0075] The Ar1 is selected from C6~C 30 Aromatic groups, substituted C6~C 30 Aromatic groups, C4~C 30 Cycloalkyl, substituted C4~C 30 Cycloalkyl, C6~C 30 Heteroaryl or substituted C6~C 30 heteroaryl;
[0076] Ar2 is selected from C6~C 30 Aromatic groups, substituted C6~C 30 Aromatic groups, C4~C 30 Cycloalkyl or substituted C4~C 30 Cycloalkyl, C6~C 30 Heteroaryl or substituted C6~C 30 The heteroaryl group.
[0077] In some specific implementations, n is 1, 2, 3, 4 or 5, preferably n is 1 or 2 or 3, and more preferably n is 1.
[0078] In some specific implementations, the aromatic group refers to a compound having a benzene ring structure, including but not limited to a monophenyl aromatic group and a polyphenyl aromatic group. In some specific implementations, the cycloalkyl group includes but is not limited to a monocyclic structure and a polycyclic structure. In some specific implementations, the heteroaryl group includes but is not limited to a monoaromatic ring monosubstituent, a monoaromatic ring polysubstituent, a polyaromatic ring monosubstituent, and a polyaromatic ring polysubstituent.
[0079] Specifically, the polyimide structure may be the following structure:
[0080]
[0081] The present application uses a diamine compound containing both a benzoazole structure and an aliphatic ring structure as a raw material to prepare polyimide, thereby improving the mechanical properties, thermodynamic properties and oxidative stability of the polyimide molecular chain, while increasing the free volume between molecular chains and reducing the charge transfer interactions within and between molecules.
[0082] In some specific implementations, Ar1 is preferably the following structure:
[0083]
[0084] More preferably, the following structure:
[0085]
[0086] In some specific implementations, Ar2 is preferably the following structure:
[0088]
[0089] Wherein, Y is selected from O, S, SO2, CO or
[0090] m is an integer of 1 to 4, preferably an integer of 1 to 3, and more preferably 1;
[0091] R1 and R2 are selected from H, C1-C6 alkyl, halogen-substituted C1-C6 alkyl, preferably H, fluorine-substituted C1-C6 alkyl, more preferably trifluoromethyl;
[0092] Z is selected from O, N or S.
[0093] The present invention provides a method for preparing a polyimide, comprising:
[0094] a) a diamine compound represented by formula (I) or formula (II), an optional diamine compound represented by formula (a) and a dianhydride compound represented by formula (b) are polymerized to obtain a polyamic acid;
[0095] b) subjecting the polyamic acid to imidization reaction to obtain polyimide;
[0096]
[0097] The diamine compounds represented by the formula (I) and the formula (II) have the same selection range as the diamine compounds represented by the aforementioned formula (I) and the formula (II), and will not be described in detail.
[0098] In the diamine compound represented by formula (a), the selection range of Ar2 is the same as the selection range of Ar2 described in the compound represented by the structure of formula (VI) or formula (VII), and will not be repeated here;
[0099] In the diamine compound represented by formula (b), the selection range of Ar1 is the same as the selection range of Ar1 described in the compound having the structure represented by formula (VI) or formula (VII) above, and will not be repeated here.
[0100] In some specific implementations, the diamine compound represented by formula (a) is preferably selected from the following structures:
[0101]
[0102] Wherein, Y is selected from O, S, SO2, CO or
[0103] m is an integer of 1 to 4, preferably an integer of 1 to 3, and more preferably 1;
[0104] R1 and R2 are selected from H, C1-C6 alkyl, halogen-substituted C1-C6 alkyl, preferably H, fluorine-substituted C1-C6 alkyl, more preferably trifluoromethyl;
[0105] Z is selected from O, N or S.
[0106] In some specific implementations, the dianhydride compound represented by formula (b) is preferably of the following structure:
[0107]
[0108] More preferably, the following structure:
[0109]
[0110] The present invention dissolves a diamine compound represented by formula (I) or formula (II), an optional diamine compound represented by formula (a) and a dianhydride compound represented by formula (b) in a solvent, and continuously stirs the mixture in an inert atmosphere, so that an amino group in the diamine compound and an acid anhydride in the dianhydride compound undergo a polymerization reaction to obtain a polyamic acid; the polyamic acid undergoes an imidization reaction under the action of an imidization agent, and undergoes dehydration cyclization to obtain a polyimide.
[0111] The polymerization reaction of the present invention is carried out in a solvent, and the solvent is a polar aprotic solvent, including but not limited to one or more of N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone, preferably N,N-dimethylacetamide. The present invention first dissolves a diamine compound, i.e., the total amount of a diamine compound represented by formula (I) or formula (II) and a diamine compound represented by formula (a), and a dianhydride compound in a solvent in an inert atmosphere, and continuously stirs to dehydrate and condense the amino group in the diamine compound and the acid anhydride in the dianhydride compound to obtain a polyamic acid solution.
[0112] In some specific implementations, the molar ratio of the reactant diamine compound to the dianhydride compound in the polymerization reaction is 0.9:1 to 1:0.9, preferably 0.95:1 to 1:0.95. In some specific implementations, the molar ratio of the diamine compound represented by formula (I) or formula (II) to the diamine compound represented by formula (a) is preferably 1 to 2:0 to 1, more preferably 1 to 2:1. In some specific implementations, the temperature of the polymerization reaction is 0 to 30°C, preferably 0 to 25°C, more preferably 0 to 20°C. In some specific implementations, the time of the polymerization reaction is 6 to 108h, preferably 10 to 100h, more preferably 20 to 80h.
[0113] After the polyamic acid solution is obtained, it is imidized. Specifically, an imidization agent can be added to the obtained polyamic acid solution, and stirring is continued for 6 to 24 hours, preferably 7 to 20 hours, and more preferably 8 to 15 hours, so that the polyamic acid therein is imidized to polyimide.
[0114] In some specific implementations, the reagents for the imidization reaction are acetic anhydride and pyridine, and the molar ratio of the acetic anhydride to the pyridine is 1:1 to 10, preferably 1:1 to 5, and more preferably 1:1 to 3. In some specific implementations, the molar ratio of the reagents for the imidization reaction to the diamine compound, i.e., the total amount of the diamine compound represented by formula (I) or formula (II) and the diamine compound represented by formula (a), is 0.5 to 3:1, preferably 0.8 to 2.5:1, and more preferably 1 to 2:1.
[0115] In some specific implementations, the obtained polyimide is further subjected to post-treatment, wherein the post-treatment includes precipitation, impurity removal and drying.
[0116] In some specific implementations, the precipitation includes immersing the polyimide solution in a polar solvent to precipitate a solid. In some specific implementations, the polar solvent includes but is not limited to methanol. In some specific implementations, the impurity removal includes but is not limited to filtering and washing. This product has no special restrictions on the methods of precipitation, impurity removal and drying.
[0117] In some specific implementations, the present application can also prepare polyimide by a one-step method, and the specific process is as follows:
[0118] Under an inert gas atmosphere, dianhydride and diamine are polymerized in a phenolic solvent to obtain polyimide.
[0119] In some specific implementations, the dianhydride and diamine are as described above, and the present application will not repeat them here. The phenolic solvent includes but is not limited to m-cresol or m-chlorophenol, etc., the polymerization reaction temperature is 180-210° C., and the polymerization reaction time is 6-72 hours.
[0120] The present invention provides a polyimide film, which is prepared from the polyimide having the structure of formula (VI) or formula (VII). The benzoxazole structure in the polyimide having the structure of formula (VI) or formula (VII) can improve the rigidity and linearity of the molecular chain, and give the film excellent heat resistance; the aliphatic ring structure can inhibit the CT effect in the molecular chain, and improve the optical properties of the film.
[0121] The present application has no special restrictions on the preparation method of the polyimide film, for example, the prepared polyimide can be dissolved, cast into a film, and dried to obtain the film. The present application has no special restrictions on the solvent used to dissolve the polyimide, and there is no special restriction on the temperature during the drying process.
[0122] In some specific implementations, after the polyimide is prepared in the present application, the polyimide solution can be directly cast into a film and dried to prepare a polyimide film without post-treatment. The specific process is similar to the process described above, and the present application will not repeat it here.
[0123] The present invention introduces a benzoxazole structure and an aliphatic ring structure into the diamine compound structure, which can balance the rigidity and flexibility of the molecular chain and the charge transfer interaction. The polyimide film prepared with the diamine compound as a raw material has excellent heat resistance and transparency, and can be applied to optoelectronic display and solar substrates. The experimental results show that the polyimide obtained by polymerizing the diamine compound provided by the present invention has both heat resistance and transparency after being made into a film, and has good comprehensive performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0124] Figure 1 is the diamine compound in Example 1 of the present invention 1 H NMR spectrum;
[0125] Figure 2 is the diamine compound in Example 2 of the present invention 1 H NMR spectrum;
[0126] Figure 3DMA curves of the polyimide films prepared in Examples 5 and 8 of the present invention;
[0127] Figure 4 The UV-visible light transmittance curves of the polyimide films prepared in Examples 5 and 8 of the present invention. DETAILED DESCRIPTION
[0128] It should be understood that the expression "one or more of..." includes each of the items recited after the expression individually and in various different combinations of two or more of the recited items, unless otherwise understood from the context and usage. The expression "and / or" in combination with three or more recited items should be understood to have the same meaning, unless otherwise understood from the context.
[0129] The use of the terms "comprising", "having" or "containing", including their grammatical synonyms, should generally be understood as open and non-restrictive, for example not excluding other unrecited elements or steps, unless otherwise specifically stated or otherwise understood from the context.
[0130] It should be understood that the order of steps or the order in which certain actions are performed is not important as long as the present invention remains operable. In addition, two or more steps or actions may be performed simultaneously.
[0131] The use of any and all examples or exemplary language, such as "for example" or "including", herein is intended only to better illustrate the invention and does not limit the scope of the invention unless otherwise claimed. No language in this specification should be construed as indicating that any non-claimed element is essential to the practice of the invention.
[0132] In addition, the numerical ranges and parameters used to define the present invention are approximate values, and the relevant values in the specific embodiments have been presented as accurately as possible. However, any numerical value inherently inevitably contains standard deviations due to individual test methods. Therefore, unless otherwise expressly stated, it should be understood that all ranges, quantities, values and percentages used in this disclosure are modified by "about". Here, "about" generally means that the actual value is within plus or minus 10%, 5%, 1% or 0.5% of a specific value or range.
[0133] The present invention is further described below in conjunction with the following examples. The protection scope of the present invention is not limited by the following examples.
[0134] Example 1
[0135] Under nitrogen protection, add polyphosphoric acid (1000g), trans-1,4-cyclohexanedicarboxylic acid (34.436g, 0.2mol) and stannous chloride dihydrate (4.513g, 0.02mol) to a 3L three-necked flask equipped with a mechanical stirring device, then heat to 60°C and add 2,4-diaminophenol dihydrochloride (78.824g, 0.4mol) in batches. After the addition is completed, stir for 5 to 10 hours until HCl gas no longer evaporates. Add phosphorus pentoxide (28.388g, 0.2mol) to the flask and continue stirring for 0.5 hours. Slowly heat to 150°C for 3 hours, then heat to 200°C for 10 hours. After the reaction is complete, cool the solution to room temperature. The solution pH was adjusted to about 8 using a saturated sodium carbonate solution, washed three times with water and ethanol respectively, filtered and dried to obtain a crude product, and purified to obtain diamine monomer I-1a-1 as a light yellow solid with a yield of 77%. 1 H NMR spectrum Figure 1 shown.
[0136]
[0137] The purified product was characterized by NMR, and the results of NMR hydrogen spectrum are as follows: 1 H NMR (500MHz, DMSO-d6) δ = 7.28 (dd, J = 8.6, 7.5, 2H), 6.78 (dd, J = 10.6, 2.2, 2H), 6.58 (ddd, J = 9.7, 8.6, 2.2, 2H), 3.06 (m,2H),2.22(m,2H),2.05(dt,J=13.2,5.7,2H),1.94(ddd,J=11.6,8.0,5.0,2H),1.74(dq,J=13.2,10.5,9.9,2H).
[0138] Example 2
[0139] Under nitrogen protection, polyphosphoric acid (1000g), cis-1,4-cyclohexanedicarboxylic acid (34.436g, 0.2mol) and stannous chloride dihydrate (4.513g, 0.02mol) were added to a 3L three-necked flask equipped with a mechanical stirring device, and then heated to 60°C, and 2,4-diaminophenol dihydrochloride (78.824g, 0.4mol) was added in batches. After the addition is completed, stir for 5 to 10 hours until HCl gas no longer evaporates. Then add phosphorus pentoxide (28.388g, 0.2mol) and stir for 0.5 hours. Slowly heat the solution to 150°C and stir for 3 hours, then heat to 200°C and react for 10 hours. After the reaction is complete, cool the solution to room temperature. Then, a saturated sodium carbonate solution was used to adjust the pH value of the solution to about 8, and the solution was washed three times with water and ethanol respectively, filtered and dried to obtain a crude product, and after purification, the diamine monomer I-2a-1 was obtained as a light yellow solid with a yield of 79%. 1 H NMR spectrum Figure 2 shown.
[0140]
[0141] The obtained product was characterized by NMR, and the results of NMR hydrogen spectrum are as follows: 1 H NMR (500MHz, DMSO-d6) δ=7.28(t,J=8.0,2H),6.78(dd,J=10.5,2.2,2H),6.58(td,J=9.7,9.2,2.3,2H),4.99(d,J=8.1,4H),3.19(dq,J=8 .2,4.4,4.0,1H),3.03-2.94(m,1H),2.22(hept,J=4.8,3.7,2H),2.05(dt,J=13.4,5.6,1H),1.98-1.89(m,1H),1.74(td,J=9.2,3.3,2H).
[0142] Example 3
[0143] Under nitrogen protection, add 4,4'-(hexafluoroisopropylidene) diphthalic anhydride 6FDA (3.554g, 8mmol) and 25g N,N-dimethylacetamide to a 100mL three-necked flask equipped with a mechanical stirring device. After the anhydride is dissolved, add diamine I-1a-1 (2.788g, 8mmol), react at 0°C for 72h, then add acetic anhydride (0.816g, 8mmol) and pyridine (15.8g, 20mmol) and continue stirring for 10h to obtain a crude polyimide product. The crude product is transferred to methanol for precipitation, filtered, broken, and dried to obtain a polyimide powder. The polyimide powder is redissolved in N,N-dimethylacetamide solvent to a solid content of 15wt%. The uniform polyimide solution was coated on a clean and flat glass plate, and the residual solvent was removed in an oven at 80℃ / 5h, 150℃ / 1h, 250℃ / 1h, and 300℃ / 1h. The dried polyimide was placed in hot water to allow the film to peel off automatically, and the film was placed in an oven and dried at 100℃ for 5h to remove the residual moisture, and a transparent polyimide film was obtained after taking it out.
[0144] Example 4
[0145] Under nitrogen protection, 1,2,4,5-cyclohexanetetracarboxylic dianhydride H-PMDA (1.793 g, 8 mmol) and 18 g N,N-dimethylacetamide were added to a 100 mL three-necked flask equipped with a mechanical stirring device. After the dianhydride was dissolved, diamine I-1a-1 (2.788 g, 8 mmol) was added, and the mixture was reacted at 0°C for 72 h. Acetic anhydride (0.816 g, 8 mmol) and pyridine (15.8 g, 20 mmol) were then added and stirred for 10 h to obtain a crude polyimide product. The crude product was transferred to methanol for precipitation, filtered, broken, and dried to obtain a polyimide powder. The polyimide powder was redissolved in N,N-dimethylacetamide solvent to a solid content of 15 wt%. The uniform polyimide solution was coated on a clean and flat glass plate, and the residual solvent was removed in an oven at 80℃ / 5h, 150℃ / 1h, 250℃ / 1h, and 300℃ / 1h. The dried polyimide was placed in hot water to allow the film to peel off automatically, and the film was placed in an oven and dried at 100℃ for 5h to remove the residual moisture, and a transparent polyimide film was obtained after taking it out.
[0146] Example 5
[0147] Under nitrogen protection, add cyclobutanetetracarboxylic acid dianhydride CBDA (1.569g, 8mmol) and N,N-dimethylacetamide 17g to a 100mL three-necked flask equipped with a mechanical stirring device. After the dianhydride is dissolved, add diamine I-1a-1 (2.788g, 8mmol), react at 0℃ for 72h, then add acetic anhydride (0.816g, 8mmol) and pyridine (15.8g, 20mmol) and continue stirring for 10h to obtain a crude polyimide product. The crude product is transferred to methanol for precipitation, filtered, broken, and dried to obtain a polyimide powder. The polyimide powder is redissolved in N,N-dimethylacetamide solvent to a solid content of 15wt%. The uniform polyimide solution is coated on a clean and flat glass plate, and the residual solvent is removed in an oven at 80℃ / 5h, 150℃ / 1h, 250℃ / 1h, and 300℃ / 1h. The dried polyimide was placed in hot water to allow the film to peel off automatically, and the film was placed in an oven and dried at 100° C. for 5 hours to remove residual moisture, and a transparent polyimide film was obtained after being taken out.
[0148] Example 6
[0149] Under nitrogen protection, add 4,4'-(hexafluoroisopropylidene) diphthalic anhydride 6FDA (3.554g, 8mmol) and 25g N,N-dimethylacetamide to a 100mL three-necked flask equipped with a mechanical stirring device. After the anhydride is dissolved, add diamine I-2a-1 (2.788g, 8mmol), react at 0°C for 72h, then add acetic anhydride (0.816g, 8mmol) and pyridine (15.8g, 20mmol) and continue stirring for 10h to obtain a crude polyimide product. The crude product is transferred to methanol for precipitation, filtered, broken, and dried to obtain a polyimide powder. The polyimide powder is redissolved in N,N-dimethylacetamide solvent to a solid content of 15wt%. The uniform polyimide solution was coated on a clean and flat glass plate, and the residual solvent was removed in an oven at 80℃ / 5h, 150℃ / 1h, 250℃ / 1h, and 300℃ / 1h. The dried polyimide was placed in hot water to allow the film to peel off automatically, and the film was placed in an oven and dried at 100℃ for 5h to remove the residual moisture, and a transparent polyimide film was obtained after taking it out.
[0150] Example 7
[0151] Under nitrogen protection, 1,2,4,5-cyclohexanetetracarboxylic dianhydride H-PMDA (1.793 g, 8 mmol) and 18 g N,N-dimethylacetamide were added to a 100 mL three-necked flask equipped with a mechanical stirring device. After the dianhydride was dissolved, diamine I-2a-1 (2.788 g, 8 mmol) was added, and the mixture was reacted at 0°C for 72 h. Acetic anhydride (0.816 g, 8 mmol) and pyridine (15.8 g, 20 mmol) were then added and stirred for 10 h to obtain a crude polyimide product. The crude product was transferred to methanol for precipitation, filtered, broken, and dried to obtain a polyimide powder. The polyimide powder was redissolved in N,N-dimethylacetamide solvent to a solid content of 15 wt%. The uniform polyimide solution was coated on a clean and flat glass plate, and the residual solvent was removed in an oven at 80℃ / 5h, 150℃ / 1h, 250℃ / 1h, and 300℃ / 1h. The dried polyimide was placed in hot water to allow the film to peel off automatically, and the film was placed in an oven and dried at 100℃ for 5h to remove the residual moisture, and a transparent polyimide film was obtained after taking it out.
[0152] Example 8
[0153] Under nitrogen protection, add cyclobutanetetracarboxylic acid dianhydride CBDA (1.569g, 8mmol) and N,N-dimethylacetamide 17g to a 100mL three-necked flask equipped with a mechanical stirring device. After the dianhydride is dissolved, add diamine I-2a-1 (2.788g, 8mmol), react at 0℃ for 72h, then add acetic anhydride (0.816g, 8mmol) and pyridine (15.8g, 20mmol) and continue stirring for 10h to obtain a crude polyimide product. The crude product is transferred to methanol for precipitation, filtered, broken, and dried to obtain a polyimide powder. The polyimide powder is redissolved in N,N-dimethylacetamide solvent to a solid content of 15wt%. The uniform polyimide solution is coated on a clean and flat glass plate, and the residual solvent is removed in an oven at 80℃ / 5h, 150℃ / 1h, 250℃ / 1h, and 300℃ / 1h. The dried polyimide was placed in hot water to allow the film to peel off automatically, and the film was placed in an oven and dried at 100° C. for 5 hours to remove residual moisture, and a transparent polyimide film was obtained after being taken out.
[0154] The polyimide films prepared in Example 5 and Example 8 were subjected to dynamic mechanical analysis and UV-visible light transmittance analysis. The results are as follows: Figure 3 and Figure 4 shown. Figure 3 The two curves in the upper part represent the storage modulus of Example 5 and Example 8 at different temperatures, and the two curves in the lower part represent the loss tangent of Example 5 and Example 8 at different temperatures. Figure 4The two curves in FIG. 1 represent the light transmittance of Example 5 and Example 8 under different wavelengths of light. Figure 3 and Figure 4 It can be seen that the glass transition temperatures of the polyimide films prepared in Example 5 and Example 8 are 400°C and 404°C, respectively, and the transmittances at 450nm are 83.7% and 83.5%, respectively, which indicates that the heat resistance and transparency of the polyimide film prepared by this method reach a good balance, which is conducive to its application in the fields of transparent flexible substrates and transparent circuit boards.
[0155] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A diamine compound represented by formula (I) or formula (II): in, X is selected from O or NH; n is an integer selected from 1-5.
2. The diamine compound according to claim 1, characterized in that Having the structure of formula (I-1), (I-2), (II-1) or (II-2):
3. The diamine compound according to claim 2, characterized in that Having the structure of formula (I-1a), (I-1b), (I-2a), (I-2b), (II-1a), (II-1b), (II-2a) or (II-2b): wherein n is selected from 1, 2 or 3.
4. The diamine compound according to claim 3, characterized in that Having the structure of formula (I-1a-1), (I-1b-1), (I-2a-1), (I-2b-1), (II-1a-1), (II-1b-1), (II-2a-1) or (II-2b-1):
5. A method for preparing a diamine compound, characterized in that: include: A cycloalkane compound having a structure of formula (III), an aniline compound having a structure of formula (IV) or formula (V) and a reducing agent undergo a first reaction in an inert atmosphere, and then undergo a second reaction with a dehydrating agent to obtain a diamine compound represented by formula (I) or formula (II); Wherein, R3 is hydroxyl, R1 and R2 are independently acyl chloride, carboxyl or amino; or R3 is amino, R1 and R2 are independently acyl chloride, carboxyl or hydroxyl; X is selected from O or NH; n is an integer selected from 1-5.
6. The preparation method according to claim 5, characterized in that: The molar ratio of the cycloalkane compound to the aniline compound is 1:0.5-2, the temperature of the first reaction is 40-80° C., and the time of the first reaction is 5-10 hours; The temperature of the second reaction is 170-220°C, and the time of the second reaction is 5-16h; The reducing agent is selected from tin powder or stannous chloride, and the molar ratio of the reducing agent to the cycloalkane compound is 1 to 10:100; The solvent of the reaction is selected from one or more of boric acid, concentrated sulfuric acid and polyphosphoric acid, and the mass ratio of the solvent to the cycloalkane compound is 15 to 30:1; The inert atmosphere is a nitrogen or argon atmosphere.
7. The preparation method according to claim 5, characterized in that: The dehydrating agent is selected from phosphorus pentoxide, and the molar ratio of the dehydrating agent to the cycloalkane compound is 0.5 to 2:
1.
8. A polyimide having a structure of formula (VI) or formula (VII): in, k is the repeating unit The molar ratio of , 0≤k≤0.5; X is selected from O or NH; n is an integer selected from 1 to 5; Ar1 is selected from C6~C 30 Aromatic groups, substituted C6~C 30 Aromatic groups, C4~C 30 Cycloalkyl, substituted C4~C 30 Cycloalkyl, C6~C 30 Heteroaryl or substituted C6~C 30 heteroaryl; Ar2 is selected from C6~C 30 Aromatic groups, substituted C6~C 30 Aromatic groups, C4~C 30 Cycloalkyl or substituted C4~C 30 Cycloalkyl, C6~C 30 Heteroaryl or substituted C6~C 30 The heteroaryl group.
9. The polyimide according to claim 8, characterized in that The Ar1 is selected from the following structures: The Ar2 is selected from the following structures: Wherein, Y is selected from O, S, SO2, CO or m is an integer of 1 to 4, R1 and R2 are selected from H, C1 to C6 alkyl, and halogen-substituted C1 to C6 alkyl; Z is selected from O, N or S.
10. A method for preparing polyimide, characterized in that: include: a) a diamine compound according to any one of claims 1 to 4, an optional diamine compound represented by formula (a) and a dianhydride compound represented by formula (b) are polymerized to obtain a polyamic acid; b) the polyamic acid is subjected to imidization reaction to obtain polyimide; H2N-Ar2-NH2(a) Wherein, Ar1 is selected from C6~C 30 Aromatic groups, substituted C6~C 30 Aromatic groups, C4~C 30 Cycloalkyl, substituted C4~C 30 Cycloalkyl, C6~C 30 Heteroaryl or substituted C6~C 30 heteroaryl; Ar2 is selected from C6~C 30 Aromatic groups, substituted C6~C 30 Aromatic groups, C4~C 30 Cycloalkyl or substituted C4~C 30 Cycloalkyl, C6~C 30 Heteroaryl or substituted C6~C 30 The heteroaryl group.
11. The preparation method according to claim 10, characterized in that: The diamine compound represented by the formula (a) is selected from the following structures: Wherein, Y is selected from O, S, SO2, CO or m is an integer of 1 to 4, R1 and R2 are selected from H, C1 to C6 alkyl, and halogen-substituted C1 to C6 alkyl; Z is selected from O, N or S; The dianhydride compound represented by the formula (b) is selected from the following structures:
12. The preparation method according to claim 10, characterized in that: In the step a), the molar ratio of the total amount of the diamine compound according to any one of claims 1 to 4 and the diamine compound represented by formula (a) to the dianhydride compound is 0.9:1 to 1:0.9, the reaction temperature is 0 to 30° C., and the reaction time is 6 to 108 hours; The solvent of the reaction is a polar aprotic solvent; The solid content of the reaction is 5wt% to 25wt%; The imidization reagents for the imidization reaction in step b) are acetic anhydride and pyridine, and the molar ratio of the reagents to the total amount of the diamine compound according to any one of claims 1 to 4 and the diamine compound represented by formula (a) is 0.5 to 3:1; The time of the imidization reaction is 6 to 24 hours.
13. A polyimide film prepared from the polyimide according to any one of claims 10 to 12.
Citation Information
Patent Citations
Method for preparing polyimide fibers by using liquid crystal spinning
CN102586930A
Polyimide material applied to flexible display substrate and preparation method thereof
CN110003470A
High-heat-resistance low-thermal-expansion-coefficient polyimide material and preparation method thereof
CN110105570A
Liquid crystal aligning agent, prepared liquid crystal alignment film and display element containing alignment film
CN116814278A
Cyclohexane-containing diamine monomer, transparent polyimide film and preparation method thereof
CN117624072A