Photocuring stretchable conductive hydrogel electrode for physiological signal detection
By curing MXene and polyacrylamide composite sol in a silicone mold, the stretchable conductive hydrogel electrode is formed, which solves the shortcomings of traditional electrodes in the flexibility requirements of strain mechanics, and achieves high performance and simple preparation. It is suitable for Physiological signal detection.
Patent Information
- Application Number
- CN202411222946.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-03
AI Technical Summary
The existing conductive hydrogel electrodes have poor mechanical properties in strain mechanical flexibility requirements such as bending, folding, twisting and tensile, which is difficult to meet the needs of future wearable flexible electronic products. The traditional preparation methods are complex and costly.
UV curing is performed in silicone mold using MXene and polyacrylamide composite sol to form a stretchable conductive hydrogel electrode. MXene is used to build a three-dimensional conductive network and polyacrylamide provides a flexible framework, combining glycerol and carboxylated cellulose nanofibers Enhance hydrogen bonding and adhesion.
The mechanical and electrical conductivity of the electrode is significantly improved, providing higher flexibility and electrical signal conduction efficiency, simplifying the preparation process, reducing costs, and improving compatibility and wear comfort for organisms.
Smart Images

Figure CN118978641A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of flexible electronic materials, and in particular relates to a stretchable conductive hydrogel electrode for physiological signal detection and a preparation method thereof. Background Art
[0002] The advent of the 5G era and the development of artificial intelligence have made flexible electronics very popular. Flexible epidermal electrodes made by imitating human skin can accurately detect external stimuli and physiological signals, making them more widely used in fields such as tactile sensors and wearable electronic devices. Currently, the most common electrodes are various metals, alloys, and oxide semiconductors, which cannot meet the requirements of future wearable flexible electronic products for large strain mechanical flexibility such as bending, folding, twisting, and even stretching.
[0003] Hydrogel is a flexible polymer composed of a three-dimensional cross-linked hydrophilic polymer network and water, with excellent flexibility, adjustable elastic modulus and unique biological properties. On this basis, conductive hydrogel combined with conductive polymers or conductive nanofillers has adjustable conductive properties, which can improve the conductivity of traditional hydrogels to a certain extent, and is therefore considered to be an ideal choice for high-performance flexible epidermal electrodes.
[0004] According to the design requirements of flexible electronic devices, the matching electrodes are also required to have flexible and stretchable properties, and still maintain their original conductivity in the stretched state. However, in actual use, many problems such as poor mechanical properties and easy damage make it difficult for traditional conductive hydrogels to meet people's increasingly high performance requirements for flexible epidermal electrodes, resulting in greatly limited applications of electrodes prepared therefrom. Therefore, it is of great significance to study a stretchable conductive hydrogel electrode with good mechanical properties and conductive properties for physiological signal detection. Summary of the invention
[0005] The purpose of the present invention is to provide a stretchable conductive hydrogel electrode for physiological signal detection and a preparation method thereof in view of the deficiencies of the prior art. The method pours a MXene / polyacrylamide composite sol into silica gel and controls the thickness, then crosslinks it by ultraviolet light curing to obtain a MXene / polyacrylamide composite gel, which is finally used as a light-cured stretchable conductive hydrogel electrode for physiological signal detection. The method of the present invention is simple and easy to operate, and the mechanical properties of the prepared hydrogel are significantly improved.
[0006] The technical solution of the present invention is:
[0007] A stretchable conductive hydrogel electrode for physiological signal detection, the preparation method of the electrode comprising the following steps:
[0008] (1) mixing acrylamide, sodium acrylate and sodium alginate and stirring the mixture at 60 to 90° C. for 0.5 to 2 hours to obtain a mixed solution;
[0009] Wherein, 0.1-0.44 g of sodium alginate is added for every 1.44 g of acrylamide and 0.24-0.36 g of sodium acrylate;
[0010] (2) adding glycerol, carboxylated cellulose nanofibers and MXene to the mixed solution, stirring at 60 to 90° C. for 6 to 12 hours to obtain a MXene / polyacrylamide composite solution;
[0011] For every 1.5-2.5 g of composite solution, add 0.01-0.66 g of glycerol, 0.01-0.07 g of carboxylated cellulose nanofibers, and 0.01-0.05 g of MXene;
[0012] (3) cooling the composite solution to room temperature, adding 2-hydroxy-2-methyl-1-phenyl-1-propanone, dissolving by shaking and ultrasonication, and deoxygenating by nitrogen to obtain a MXene / polyacrylamide composite sol;
[0013] Add 0.01-0.07 g of 2-hydroxy-2-methyl-1-phenyl-1-propanone per 1.8-2.7 g of composite sol;
[0014] (4) The MXene / polyacrylamide composite sol is added into a silicone mold and photocured under ultraviolet light for 5 to 30 minutes to obtain a MXene / polyacrylamide composite gel, which is a stretchable conductive hydrogel electrode.
[0015] The stirring rate in steps (1) and (2) is 500 to 1000 rpm;
[0016] The light curing parameters are light intensity 10000~30000uW / cm 2 , distance 10-20cm, wavelength 405nm;
[0017] In step (3), the dissolution is carried out by oscillation for 5 to 10 minutes; the dissolution is carried out by ultrasonication for 20 to 30 minutes; and the nitrogen degassing treatment is carried out for 5 to 30 minutes.
[0018] The thickness of the MXene / polyacrylamide composite gel obtained in step (4) is in the range of 2 to 10 mm.
[0019] The stretchable conductive hydrogel electrode prepared by the method is used as an electrode patch in sports detection or medical detection sensors.
[0020] The essential features of the present invention are:
[0021] The raw materials acrylamide, sodium acrylate, sodium alginate, MXene, glycerol, carboxylated cellulose nanofibers, and 2-hydroxy-2-methyl-1-phenyl-1-propanone involved in the preparation of a photocurable stretchable conductive hydrogel electrode for physiological signal detection in the present invention are all biocompatible and harmless to the human body. MXene in the material provides good conductivity and stretchability, and can provide a higher electrical signal conduction efficiency between the electrode and the organism and a wider detection range;
[0022] The MXene / polyacrylamide composite sol was added into a silicone mold and photocured under ultraviolet light for 5 minutes to obtain a MXene / polyacrylamide composite gel. This step uses photocuring to achieve rapid preparation.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) Improved electrical properties: MXene is used in the preparation process. MXene is an excellent two-dimensional conductive filler that constructs a three-dimensional conductive network for electronic conductivity, greatly improving the electrical conductivity and increasing the efficiency of electrical signal conduction between the electrode and the organism.
[0025] (2) Improved mechanical properties: Stretchable conductive hydrogel electrodes are prepared. Different from commercial metal electrodes and solid polymer electrodes, polyacrylamide is used as a flexible skeleton and has a wide detection range. MXene has good mechanical properties and can be stably dispersed in the hydrogel. The two provide the composite hydrogel with better flexibility.
[0026] (3) Improved adhesion properties: Acrylamide and glycerol are used in the preparation process, both of which can provide a large number of hydrogen bonds, thereby enhancing the adhesion of the hydrogel to biological tissues, and ultimately improving the stability and reliability of the electrode on the organism;
[0027] (4) Providing biocompatibility: The prepared hydrogel electrode has a uniform porous structure, which gives the hydrogel electrode excellent air permeability. Combined with the photothermal therapy effect of MXene itself, it avoids the problem of skin itching and redness caused by the airtightness when the wearable electronic device is in contact with the human skin for a long time, and can provide a more comfortable wearing experience;
[0028] (5) Provides simplicity and energy saving: Different from other preparation methods such as freeze-thaw curing, thermal curing and ion curing, the UV curing method is used to prepare stretchable conductive hydrogel electrodes. The method is simple, easy to operate, fast curing, precise control, and no need to add additional chemical reagents. At the same time, the main raw materials involved in the preparation process are simple and easy to obtain, low cost, and resource saving. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1This is a scanning electron microscope image of the stretchable hydrogel electrode prepared in Example 1 of the present invention.
[0030] Figure 2 This is the stress-strain diagram of the stretchable hydrogel prepared in Example 2 of the present invention.
[0031] Figure 3 This is the tensile strain response diagram of the stretchable hydrogel electrode prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0032] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.
[0033] The sources or properties of the raw materials used in the specific embodiments of the present invention are as follows: acrylamide was purchased from Beijing Inokai Technology Co., Ltd., with the item number A24881; sodium acrylate was purchased from Shanghai MacLean Biochemical Technology Co., Ltd., with the item number S833838; sodium alginate was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., with the item number S100128; glycerol was purchased from Beijing Inokai Technology Co., Ltd., with the item number G1100; carboxylated cellulose nanofibers were purchased from Beijing Inokai Technology Co., Ltd., with the item number C916412; titanium carbide (Ti3C2T x )MXene was purchased from Shanghai MacLean Biochemical Technology Co., Ltd., item number 102508; 2-Hydroxy-2-methyl-1-phenyl-1-propanone was purchased from Beijing Inotech Technology Co., Ltd., item number H70001.
[0034] Example 1
[0035] (1) 1.44 g acrylamide, 0.36 g sodium acrylate and 0.11 g sodium alginate were dissolved by stirring at 60° C. for 2 hours at a stirring rate of 600 rpm to obtain a mixed solution;
[0036] (2) adding 0.22 g of glycerol, 0.035 g of carboxylated cellulose nanofibers, and 0.01 g of MXene to the solution obtained in step 1), adjusting the temperature to 90° C., and stirring at 600 rpm for 12 hours to obtain a MXene / polyacrylamide composite solution;
[0037] (3) The MXene / polyacrylamide composite solution of step 2) is cooled to room temperature, 0.035g of 2-hydroxy-2-methyl-1-phenyl-1-propanone is added, and after oscillation and dissolution for 10 minutes, ultrasonic dissolution is performed for 30 minutes until the added material is completely dissolved to form a completely transparent light yellow liquid without any impurities or suspended matter. After complete dissolution, it is degassed with nitrogen for 20 minutes to remove dissolved oxygen in the solution to prevent incomplete polymerization; after the above solution is deoxygenated with nitrogen, a MXene / polyacrylamide composite sol is obtained.
[0038] (4) Pour the prepared MXene / polyacrylamide composite sol into silica gel and control the thickness to 2 mm. Place the sol poured into the mold in a UV curing box (light intensity 20000uW / cm 2 , distance 16 cm, wavelength 405 nm), cross-linked for 5 min, and obtained MXene / polyacrylamide composite gel, which is a stretchable conductive hydrogel electrode.
[0039] Example 2
[0040] (1) 1.44 g acrylamide, 0.36 g sodium acrylate and 0.22 g sodium alginate were dissolved by stirring at 60° C. for 2 hours at a stirring rate of 600 rpm to obtain a mixed solution;
[0041] (2) adding 0.22 g of glycerol, 0.035 g of carboxylated cellulose nanofibers, and 0.01 g of MXene to the solution obtained in step 1), adjusting the temperature to 90° C., and stirring at 600 rpm for 12 hours to obtain a MXene / polyacrylamide composite solution;
[0042] (3) The MXene / polyacrylamide composite solution of step 2) is cooled to room temperature, 0.035g of 2-hydroxy-2-methyl-1-phenyl-1-propanone is added, and after oscillation and dissolution for 10 minutes, ultrasonic dissolution is performed for 30 minutes until the added material is completely dissolved to form a completely transparent light yellow liquid without any impurities or suspended matter. After complete dissolution, it is degassed with nitrogen for 20 minutes to remove dissolved oxygen in the solution to prevent incomplete polymerization; after the above solution is deoxygenated with nitrogen, a MXene / polyacrylamide composite sol is obtained.
[0043] (4) Pour the prepared MXene / polyacrylamide composite sol into silica gel and control the thickness to 2 mm. Place the sol poured into the mold in a UV curing box (light intensity 20000uW / cm 2 , distance 16 cm, wavelength 405 nm), cross-linked for 5 min, and obtained MXene / polyacrylamide composite gel, which is a stretchable conductive hydrogel electrode.
[0044] Example 3
[0045] (1) 1.44 g acrylamide, 0.36 g sodium acrylate and 0.33 g sodium alginate were dissolved by stirring at 60° C. for 2 hours at a stirring rate of 600 rpm to obtain a mixed solution;
[0046] (2) adding 0.22 g of glycerol, 0.035 g of carboxylated cellulose nanofibers, and 0.01 g of MXene to the solution obtained in step 1), adjusting the temperature to 90° C., and stirring at 600 rpm for 12 hours to obtain a MXene / polyacrylamide composite solution;
[0047] (3) The MXene / polyacrylamide composite solution of step 2) is cooled to room temperature, 0.035g of 2-hydroxy-2-methyl-1-phenyl-1-propanone is added, and after oscillation and dissolution for 10 minutes, ultrasonic dissolution is performed for 30 minutes until the added material is completely dissolved to form a completely transparent light yellow liquid without any impurities or suspended matter. After complete dissolution, it is degassed with nitrogen for 20 minutes to remove dissolved oxygen in the solution to prevent incomplete polymerization; after the above solution is deoxygenated with nitrogen, a MXene / polyacrylamide composite sol is obtained.
[0048] (4) Pour the prepared MXene / polyacrylamide composite sol into silica gel and control the thickness to 2 mm. Place the sol poured into the mold in a UV curing box (light intensity 20000uW / cm 2 , distance 16 cm, wavelength 405 nm), cross-linked for 5 min, and obtained MXene / polyacrylamide composite gel, which is a stretchable conductive hydrogel electrode.
[0049] Example 4
[0050] (1) 1.44 g of acrylamide, 0.36 g of sodium acrylate and 0.44 g of sodium alginate were dissolved by stirring at 60° C. for 2 hours at a stirring rate of 600 rpm to obtain a mixed solution;
[0051] (2) adding 0.22 g of glycerol, 0.035 g of carboxylated cellulose nanofibers, and 0.01 g of MXene to the solution obtained in step 1), adjusting the temperature to 90° C., and stirring at 600 rpm for 12 hours to obtain a MXene / polyacrylamide composite solution;
[0052] (3) The MXene / polyacrylamide composite solution of step 2) is cooled to room temperature, 0.035g of 2-hydroxy-2-methyl-1-phenyl-1-propanone is added, and after oscillation and dissolution for 10 minutes, ultrasonic dissolution is performed for 30 minutes until the added material is completely dissolved to form a completely transparent light yellow liquid without any impurities or suspended matter. After complete dissolution, it is degassed with nitrogen for 20 minutes to remove dissolved oxygen in the solution to prevent incomplete polymerization; after the above solution is deoxygenated with nitrogen, a MXene / polyacrylamide composite sol is obtained.
[0053] (4) Pour the prepared MXene / polyacrylamide composite sol into silica gel and control the thickness to 2 mm. Place the sol poured into the mold in a UV curing box (light intensity 20000uW / cm 2 , distance 16 cm, wavelength 405 nm), cross-linked for 5 min, and obtained MXene / polyacrylamide composite gel, which is a stretchable conductive hydrogel electrode.
[0054] Scanning electron microscopy test: The hydrogel samples were freeze-dried and sprayed with gold, and the surface morphology of the hydrogel was observed by scanning electron microscopy (AperoS).
[0055] Mechanical properties test: The tensile test was performed on a dumbbell-shaped stretchable conductive hydrogel electrode (35 mm long, 6 mm wide, and 1 mm thick) using an electronic universal tensile tester (AGS-X) to test its tensile properties.
[0056] Sensing performance test: A flexible tensile tester was used to perform a tensile sensing test on a dumbbell-shaped stretchable conductive hydrogel electrode (35 mm long, 6 mm wide, and 1 mm thick) at a stretching speed of 10 mm / min to measure its tensile strain response performance.
[0057] Figure 1 : is a scanning electron microscope image of the stretchable conductive hydrogel electrode prepared in Example 1. From the image, it can be seen that the hydrogel has a thick and continuous pore wall 3D network structure.
[0058] Figure 2 is a stress-strain diagram of the stretchable conductive hydrogel electrode prepared in Example 2. As can be seen from the figure, the maximum stretching rate of the stretchable conductive hydrogel electrode is 1150%.
[0059] Figure 3 This is the tensile strain response diagram of the stretchable conductive hydrogel electrode prepared in Example 3. As can be seen from the figure, it can achieve sensing detection under 0-200% strain conditions. Therefore, it can be placed on the human epidermis as a strain sensor to accurately detect various movements of the human body.
[0060] In summary, the hydrogel electrodes prepared in Example 1, Example 2, and Example 3 have the advantages of being stretchable and conductive, with a maximum stretching rate of 1150%, and can achieve tensile sensing performance detection under 0-200% strain conditions. In addition, since the hydrogel contains a large number of hydrogen bonds and can adhere to human skin, it has the potential to be used as an electrode patch in sports detection or medical detection sensors.
[0061] Finally, it should be noted that the above is only a preferred embodiment of the present invention, and the present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
[0062] Matters not covered by the present invention are known technologies.
Claims
1. A stretchable conductive hydrogel electrode for physiological signal detection, Its characteristics are The preparation method of the electrode comprises the following steps: (1) mixing acrylamide, sodium acrylate and sodium alginate and stirring at 60 to 90° C. for 0.5 to 2 hours to obtain a mixed solution; Wherein, 0.1-0.44 g of sodium alginate is added for every 1.44 g of acrylamide and 0.24-0.36 g of sodium acrylate; (2) adding glycerol, carboxylated cellulose nanofibers and MXene to the mixed solution, stirring at 60 to 90° C. for 6 to 12 hours to obtain a MXene / polyacrylamide composite solution; For every 1.5-2.5 g of composite solution, add 0.01-0.66 g of glycerol, 0.01-0.07 g of carboxylated cellulose nanofibers, and 0.01-0.05 g of MXene; (3) cooling the composite solution to room temperature, adding 2-hydroxy-2-methyl-1-phenyl-1-propanone, dissolving by shaking and ultrasonication, and deoxygenating by nitrogen to obtain a MXene / polyacrylamide composite sol; Add 0.01-0.07 g of 2-hydroxy-2-methyl-1-phenyl-1-propanone per 1.8-2.7 g of composite sol; (4) The MXene / polyacrylamide composite sol is added into a silicone mold and photocured under ultraviolet light for 5 to 30 minutes to obtain a MXene / polyacrylamide composite gel, which is a stretchable conductive hydrogel electrode.
2. The stretchable conductive hydrogel electrode for physiological signal detection according to claim 1, Its characteristics are The stirring rate in steps (1) and (2) is 500 to 1000 rpm.
3. The stretchable conductive hydrogel electrode for physiological signal detection as claimed in claim 1, characterized in that the light curing parameter is a light intensity of 10000 to 30000 uW / cm 2 , distance 10~20cm, wavelength 405nm.
4. The stretchable conductive hydrogel electrode for physiological signal detection according to claim 1, Its characteristics are In step (3), the dissolution is carried out by oscillation for 5 to 10 minutes; the dissolution is carried out by ultrasonication for 20 to 30 minutes; and the nitrogen degassing treatment is carried out for 5 to 30 minutes.
5. The stretchable conductive hydrogel electrode for physiological signal detection according to claim 1, Its characteristics are The thickness of the MXene / polyacrylamide composite gel obtained in step (4) is in the range of 2 to 10 mm.
6. The stretchable conductive hydrogel electrode for physiological signal detection according to claim 1, Its characteristics are Used as electrode patches in motion detection or medical detection sensors.
Citation Information
Patent Citations
Preparation method of artificial synaptic device based on Ti3C2-MXene / electrolyte structure
CN112103388A
Electric field sensitive polyacrylamide / MXene hydrogel as well as preparation method and application thereof
CN112808253A
Bionic MXene aerogel-based sensing material as well as preparation method and application thereof
CN112834088A
Chitosan / polyacrylamide / MXene hybrid hydrogel electrolyte as well as preparation method and application thereof
CN117116667A
Preparation method of hydrogel flexible wearable sensor for respiration monitoring
CN117186466A