Composition as well as preparation method and application thereof

By loading potassium salt on the magnetic composite oxide and using an external magnetic field to form stable magnetic composite oxide, the problems of unstable and loss of catalyst active center are solved, and the synthesis efficiency and stability of polycarbonate diol are improved , suitable for the preparation of polyurethane materials.

CN118978682APending Publication Date: 2024-11-19CHINA CHEM TECH RES INST
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411080844.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the prior art, the active center of the potassium fluoride-supported magnetic magnesium-ferrous oxide catalyst is unstable, and is easily lost in liquid phase reactions and is not easy to separate, which affects the synthesis efficiency of polycarbonate diol.

Method used

Using a composition with a magnetic composite oxide-supported potassium salt, a stable magnetic composite oxide is formed through co-precipitation reaction and external magnetic field co-deposition, and calcination at high temperatures to form oxides with strong alkalinity and stability, thereby improving catalytic activity. and stability.

Benefits of technology

The stability and reaction performance of the catalyst are improved, so that the polycarbonate diol is not easily lost in liquid phase reaction, has high activity and strong active center, is easy to separate and recover, and is suitable for transesterification and polycondensation reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978682A_ABST
    Figure CN118978682A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of polymer synthesis, particularly provides a composition as well as a preparation method and application thereof, and aims to solve the problems that an active center of a catalyst is unstable, is easy to lose in a liquid phase reaction and is difficult to separate. The composition comprises a magnetic composite oxide and sylvite loaded on the magnetic composite oxide, the sylvite comprises at least one of potassium nitrate, potassium hydroxide and potassium carbonate, and the mass ratio of the potassium element contained in the sylvite to the composition is (0.0001-0.3): 1. The magnetic composite oxide includes a first component metal oxide and a second component metal oxide. The preparation method of the composition comprises the steps of coprecipitation reaction, magnetic composite oxide preparation, potassium salt loading and composition preparation. The composition or a product obtained by the preparation method of the composition is applied to ester exchange reaction and / or polycondensation reaction. The composition and the preparation method and application thereof provided by the invention are used for preparing polycarbonate diol.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of polymer synthesis, and in particular to a composition, a preparation method and application thereof. Background Art

[0002] Polycarbonate diols are a type of polymer that contains repeated carbonate groups in the main chain of the molecule and a hydroxyl group at the end of the chain. Polycarbonate diols can be divided into aliphatic polycarbonate diols and aromatic polycarbonate diols according to the structure of the polymer. Among them, aliphatic polycarbonate diols can be used as soft segments of polyurethanes because of the greater flexibility of the molecular chain, making polyurethanes have excellent mechanical properties, hydrolysis resistance, heat resistance, oxidation resistance and wear resistance. At present, aliphatic polycarbonate diols have been widely used in polyurethane materials such as synthetic leather, adhesives, and coatings.

[0003] At present, potassium fluoride is often loaded on magnetic magnesium-iron oxide to obtain a magnetic solid base catalyst, which is used to prepare aliphatic polycarbonate diols. Although this type of catalyst can be used to synthesize aliphatic polycarbonate diols, the active center is mainly formed by potassium fluoride and magnesium oxide, the active center is not stable, and is easily lost in the liquid phase reaction and difficult to separate. Summary of the invention

[0004] The present disclosure is proposed in view of the above problems. The present disclosure provides a composition and a preparation method and application thereof.

[0005] According to one aspect of the present disclosure, a composition is provided, wherein the raw materials of the composition include:

[0006] A magnetic composite oxide and a potassium salt supported on the magnetic composite oxide, wherein the mass ratio of the potassium element contained in the potassium salt to the composition is (0.0001-0.3):1; the potassium salt comprises at least one of potassium chloride, potassium nitrate, potassium hydroxide and potassium carbonate;

[0007] The magnetic composite oxide comprises a first component metal oxide and a second component metal oxide, the first component metal oxide comprises at least one of aluminum oxide, zirconium oxide and cerium oxide, and the second component metal oxide is iron oxide.

[0008] Compared with the prior art, the raw materials of the composition in the present application include a magnetic composite oxide and a potassium salt loaded on the magnetic composite oxide, and the mass ratio of the potassium element contained in the potassium salt to the composition is (0.0001-0.3):1. Within this ratio range, the potassium element of the potassium salt can produce a good anchoring and dispersion effect with the components in the magnetic composite oxide, improve the dispersion and fixity of the potassium element, and help improve the stability and reaction performance of the composition. When the potassium salt includes at least one of potassium chloride, potassium nitrate, potassium hydroxide and potassium carbonate, it is easy to decompose on the surface of the magnetic composite oxide in a high temperature environment to form an oxide with strong alkalinity and stability. Compared with the composition composed of potassium fluoride and magnesium oxide, the composition in the present application is not easy to lose in the liquid phase reaction, and not only has a higher activity, but also has a stronger stability of the active center.

[0009] On this basis, the magnetic composite oxide in the present application includes a first component metal oxide and a second component metal oxide, wherein the first component metal oxide includes at least one of aluminum oxide, zirconium oxide and cerium oxide, and the second component metal oxide is iron oxide. The metal oxide of the first component is mainly used as a carrier of the active component and forms a new active component with potassium salt, wherein the iron oxide can make the composite oxide magnetic.

[0010] According to another aspect of the present disclosure, there is provided a method for preparing a composition, comprising:

[0011] Step 1, coprecipitation reaction: adding a weak base to the prepared raw material premix of the magnetic composite oxide to carry out a coprecipitation reaction until the pH value of the raw material premix reaches 11.0, thereby obtaining a suspension including the magnetic composite oxide;

[0012] Step 2, preparing a magnetic composite oxide: applying an external magnetic field to cause the suspension to precipitate, and then sequentially performing a washing treatment, a drying treatment and a first calcination treatment to obtain a composite oxide;

[0013] Step 3, loading potassium salt: immersing the composite oxide in a potassium salt solution, and drying after immersion to obtain a composite intermediate;

[0014] Step 4, preparing the composition: performing a second calcination treatment on the composition intermediate to obtain the composition.

[0015] Compared with the prior art, in the preparation method of the composition provided by the present application, a weak base is first added to the prepared raw material premix of the magnetic composite oxide to carry out a coprecipitation reaction until the pH value of the raw material premix reaches 11.0, thereby obtaining a suspension including the magnetic composite oxide. Next, an external magnetic field is applied to cause the suspension to precipitate, and then washing, drying and first calcination are performed in sequence to obtain a composite oxide. Then, the composite oxide is immersed in a potassium salt solution, dried after immersion, and a composite intermediate is obtained. Finally, the composite intermediate is subjected to a second calcination treatment to obtain a composition. Based on this, in the process of preparing the magnetic composite oxide, the external magnetic field can aggregate the colloid particles in the suspension, and under the action of gravity, the aggregated colloid particles are precipitated, which can enhance the magnetism of the colloid particles, thereby being able to prepare a composite oxide with strong magnetism. That is to say, under the action of an external magnetic field, the magnetic composite oxide can be moved, thereby ensuring that it is easy to separate after the chemical reaction is completed. In addition, by impregnating the magnetic composite oxide with potassium salt and roasting it, potassium can be decomposed during the roasting process to form an oxide with strong alkalinity and stability. It can be seen that the composition prepared by the preparation method of the composition of the present application can not only improve the activity and stability of the composition, but also make the composition easy to separate after the chemical reaction is completed.

[0016] According to another aspect of the present disclosure, there is provided a composition or a product obtained by the method for preparing the composition, and the use of the composition in an ester exchange reaction and / or a polycondensation reaction.

[0017] Compared with the prior art, the beneficial effects of the composition or the product obtained by the preparation method of the composition provided in the present application in the ester exchange reaction and / or polycondensation reaction are the same as the beneficial effects of the above-mentioned composition and its preparation method, which will not be repeated here.

[0018] It is to be understood that both the foregoing general description and the following detailed description are exemplary, and are intended to provide further explanation of the technology as claimed. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The above and other purposes, features and advantages of the present disclosure will become more apparent by describing the embodiments of the present disclosure in more detail in conjunction with the accompanying drawings. The accompanying drawings are used to provide a further understanding of the embodiments of the present disclosure and constitute a part of the specification. Together with the embodiments of the present disclosure, they are used to explain the present disclosure and do not constitute a limitation of the present disclosure. In the accompanying drawings, the same reference numerals generally represent the same components or steps.

[0020] Figure 1 is a flow chart illustrating a method for preparing a composition according to an embodiment of the present disclosure;

[0021] Figure 2is a flow chart illustrating a method for synthesizing a polycarbonate diol according to an embodiment of the present disclosure. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solution and advantages of the present disclosure more obvious, the exemplary embodiments according to the present disclosure will be described in detail with reference to the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present disclosure, rather than all the embodiments of the present disclosure, and it should be understood that the present disclosure is not limited to the exemplary embodiments described here.

[0023] In view of the problem that the active center of the catalyst in the prior art is unstable, easily lost in the liquid phase reaction, and difficult to separate, the present application provides a composition, the raw materials of the composition include: a magnetic composite oxide and a potassium salt supported on the magnetic composite oxide, the potassium salt used in the present application includes at least one of potassium chloride, potassium nitrate, potassium hydroxide and potassium carbonate, and the mass ratio of the potassium element contained in the potassium salt to the composition is (0.0001-0.3):1.

[0024] The magnetic composite oxide comprises a first component metal oxide and a second component metal oxide, wherein the first component metal oxide comprises at least one of aluminum oxide, zirconium oxide and cerium oxide, and the second component metal oxide is iron oxide.

[0025] For example, when the mass ratio of potassium element contained in potassium salt to the composition is (0.0001-0.3):1, the potassium element of potassium salt can produce good anchoring and dispersion effect with the components in the magnetic composite oxide, improve the dispersion and fixation of potassium element, and help improve the stability and reaction performance of the composition. Among them, when the mass ratio of potassium element contained in potassium salt to the composition is (0.01-0.1):1, the effect is best.

[0026] When the potassium salt includes at least one of potassium chloride, potassium nitrate, potassium hydroxide and potassium carbonate, it is easy to decompose on the surface of the magnetic composite oxide in a high temperature environment to form an oxide with strong alkalinity and stability. Compared with the composition composed of potassium fluoride and magnesium oxide, the composition in the present application is not easy to be lost in the liquid phase reaction, and not only has higher activity, but also has stronger stability of the active center.

[0027] On this basis, the magnetic composite oxide in the present application includes a first component metal oxide and a second component metal oxide, wherein the first component metal oxide includes at least one of aluminum oxide, zirconium oxide and cerium oxide, and the second component metal oxide is iron oxide. When the molar ratio of the metal element contained in the first component metal oxide and the iron element contained in the iron oxide is (0.3-0.5):1, the metal element contained in the first component metal oxide can promote the uniform distribution of potassium elements and improve the catalytic activity of the catalyst, and the iron element contained in the iron oxide can not only make the composite oxide magnetic, but also give full play to the reaction selectivity. Among them, when the first component metal oxide is aluminum oxide, it can not only ensure that the composition has good reaction performance, but also reduce production costs.

[0028] Exemplarily, for the iron source, the iron source of the iron oxide in the present application includes at least one of ferric chloride and ferrous chloride. For the aluminum source, the aluminum source of the aluminum oxide in the present application includes at least one of aluminum chloride, aluminum sulfate and aluminum nitrate. For the zirconium source, the zirconium source of the zirconium oxide in the present application includes at least one of zirconium oxychloride octahydrate and zirconium chloride. For the aluminum source, the cerium source of the cerium oxide in the present application includes at least one of cerium chloride, cerium nitrate and cerium sulfate.

[0029] The present application also provides a method for preparing the composition. Figure 1 is a flow chart illustrating a method for preparing a composition according to an embodiment of the present disclosure. Figure 1 As shown, the preparation method comprises:

[0030] Step 1, coprecipitation reaction: a weak base is added dropwise to the prepared raw material premix of the magnetic composite oxide to carry out a coprecipitation reaction until the pH value of the raw material premix reaches 11.0, thereby obtaining a suspension containing the magnetic composite oxide.

[0031] Exemplarily, in order to prepare the raw material premix, it is necessary to mix the iron source, the first component metal source and deionized water to obtain the raw material premix, wherein the first component metal source includes at least one of an aluminum source, a zirconium source and a cerium source.

[0032] Exemplary, in the coprecipitation reaction process of the present invention, it is necessary to control the raw material premix pH value to 11.0, so that the metal ions (e.g., iron ions and aluminum ions) in the raw material premix are precipitated simultaneously to obtain a suspension comprising a composite oxide. At this time, the uniform distribution of the first component metal element in the iron oxide lattice can be achieved, so that the surface active sites of the composite oxide are increased. If the pH value is too low, the metal ion precipitation in the raw material premix will be delayed, and if the pH value is too high, the metal ion precipitation in the raw material premix will end in advance, thereby affecting the reactivity of the composition.

[0033] Step 2, preparing magnetic composite oxides: applying an external magnetic field to cause the suspension to precipitate, and then sequentially performing washing treatment, drying treatment and first calcination treatment to obtain composite oxides.

[0034] Exemplarily, before applying an external magnetic field to cause the suspension to precipitate, an aging step is also included. The aging step includes leaving the suspension to stand for 1 to 4 hours, so that the various components in the suspension slowly interact and combine with each other, so that the first component metal element is evenly distributed in the iron oxide lattice, thereby increasing the surface active sites of the composite oxide.

[0035] Exemplarily, in the process of preparing magnetic composite oxides, an external magnetic field can aggregate the colloid particles in the suspension, and under the action of gravity, the aggregated colloid particles are precipitated, which can enhance the magnetism of the colloid particles, thereby preparing composite oxides with strong magnetism. In other words, under the action of an external magnetic field, the magnetic composite oxide can be moved, thereby ensuring that it is easy to separate after the chemical reaction. Then, after the suspension is precipitated, it is repeatedly washed with deionized water, dried, and calcined at 400 to 600°C for 0.5 to 2h to obtain a magnetic composite oxide. Among them, the drying method is freeze drying, the drying temperature is -20 to -40°C, and the drying time is 5 to 10h.

[0036] Step three, loading potassium salt: immersing the magnetic composite oxide in a potassium salt solution, and drying after immersion to obtain a composite intermediate.

[0037] Exemplarily, potassium salt is first formulated into a potassium salt solution, and then the magnetic composite oxide is immersed in the potassium salt solution, which can not only promote the interaction between the potassium element and the main active component of the composition and improve the dispersion of the potassium element, but also simplify the composition preparation process, avoid composition loss, and improve the operation stability and life of the composition. Subsequently, the impregnated magnetic composite oxide is dried to obtain a composition intermediate. The drying temperature is 120 to 160 ° C, and the drying time is 6 to 12 hours. It should be understood that the drying method here can be vacuum drying or normal pressure drying, or other drying methods, which are not limited here.

[0038] Step 4, preparing the composition: performing a second calcination treatment on the composition intermediate to obtain the composition.

[0039] Exemplarily, the temperature of the second calcination treatment is 300-1000°C, and the time of the second calcination treatment is 3-12 hours. Within this range, the potassium salt supported on the magnetic composite oxide can decompose to form an oxide with strong alkalinity and stability. Compared with the composition composed of potassium fluoride and magnesium oxide, the composition in the present application is not easy to lose in the liquid phase reaction, and not only has high activity, but also has strong stability of the active center. When the temperature of the second calcination treatment is 600-800°C and the time of the second calcination treatment is 4-8 hours, the calcination effect is best.

[0040] The present application also provides an application of the above composition or the product obtained by the preparation method of the above composition in transesterification reaction and / or polycondensation reaction. When the above composition is used in transesterification reaction and / or polycondensation reaction, it can not only show good reaction performance, but also can be completely recovered from the reaction product after the reaction is completed, reducing the probability of product purity decreasing due to the composition remaining in the reaction product. In addition, the composition can be recycled and has a high economic value. Specifically, the application is the application in the catalyst for preparing polycarbonate diol.

[0041] Figure 2 FIG. 1 is a flow chart illustrating a method for synthesizing a polycarbonate diol according to an embodiment of the present disclosure. Figure 2 As shown, the synthesis method comprises:

[0042] Step 1, transesterification reaction and polycondensation reaction: under the action of the composition and an inert atmosphere, the diol and the carbonate are sequentially subjected to transesterification reaction and polycondensation reaction to obtain a crude product.

[0043] Exemplarily, in step 1, the amount of the composition is 0.001wt% to 1wt%. Within this range, a crude product with a desired molecular weight distribution and excellent performance can be obtained. Among them, when the amount of the composition is 0.01wt% to 0.5wt%, the reaction performance of the combination is the best. When the amount of the composition is less than 0.001wt%, the reaction time will be prolonged and the conversion rate of the product will be adversely affected; when the amount of the composition is higher than 1wt%, too many basic centers will cause saponification reaction in the transesterification reaction and adversely affect the conversion rate of the product.

[0044] Exemplarily, in step one, for the inert atmosphere, it can be at least one of helium, neon and argon. The pressure of the inert atmosphere is 30-100KPa, and the temperature of the transesterification reaction is 140-220°C. When the temperature of the transesterification reaction is lower than 140°C, the reaction rate of the transesterification reaction is slow; when the temperature of the transesterification reaction is higher than 220°C, the diol is easily volatilized and lost. The time of the transesterification reaction is 1-4h. Within the above reaction parameter range, it can be ensured that the reaction can proceed smoothly. Among them, when the pressure of the inert atmosphere is 50-80KPa, the temperature of the transesterification reaction is 150-180°C, and the reaction time of the transesterification reaction is 2-3h, the reaction effect is best.

[0045] For example, as for the diol, the diol used in the present application includes aliphatic diols of C3 to C15.

[0046] Specifically, the aliphatic diol used in the present application includes at least one of 1,3-propylene glycol, 1,4-propylene glycol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, tricyclodecane dimethanol, pentacyclopentadecanedimethanol, 2,6-decahydronaphtalene dimethanol, 1,5-decahydronaphtalene dimethanol, 2,3-decahydronaphtalene dimethanol, 2,3-norbornane dimethanol, 2,5-norbornane dimethanol and 1,3-adamantanedimethanol.

[0047] As for carbonate, the carbonate used in the present application includes at least one of dimethyl carbonate, diethyl carbonate and dibutyl carbonate. When dimethyl carbonate is selected, the reaction effect is the best.

[0048] On this basis, the molar ratio of diol to carbonate is 1:(1-1.6), and when the molar ratio of diol to carbonate is 1:(1.1-1.3), the reaction effect is best.

[0049] Exemplarily, the polycondensation reaction in the present application includes: using a gradient pressure reduction method to carry out a polycondensation reaction on the product after the transesterification reaction. Specifically, the pressure reduction rate of the gradient pressure reduction is 0.001-0.01KPa / s, the pressure of the polycondensation reaction is 1-50KPa, the temperature of the polycondensation reaction is 180-220°C, and the time of the polycondensation reaction is 1-5h. Within this range, it is beneficial to reduce the content of small molecules in the reaction system, which is beneficial to the forward progress of the polycondensation reaction and effectively improves the conversion rate. Among them, when the pressure reduction rate of the gradient pressure reduction is 0.01KPa / s, the pressure of the polycondensation reaction is 5-10KPa, the temperature of the polycondensation reaction is 180-220°C, and the time of the polycondensation reaction is 2-4h, the reaction effect is best.

[0050] Step 2, recovering the composition: dissolving the crude product in an organic solvent, recovering the composition in the crude product by using a magnetic field, and separating the polycarbonate diol.

[0051] Exemplarily, for the organic solvent, it includes at least one of dichloromethane, dichloroethane, dichloropropane and trichloroethane. In this process, the polycarbonate diol in the crude product is dissolved in the organic solvent, and the composition can be separated from the polycarbonate diol with a higher viscosity by a magnetic field (for example, a magnet), and the recovered composition can be recycled and has a high economic value. Step three also includes: a post-treatment step; the post-treatment step includes: refining the polycarbonate diol by a precipitation method. The molecular weight of the polycarbonate diol synthesized in the present application is 800-1200g / mol; the hydroxyl value of the diol is 80-1200mg KOH / g, the acid value is less than 0.05mg KOH / g, the product quality is high, and it is suitable for the synthesis of high-quality polyurethane.

[0052] In order to verify the effect of the composition provided in the examples of the present invention as a catalyst in the preparation of polycarbonate diol, the examples of the present invention are demonstrated by comparing the examples with the comparative examples.

[0053] The following are the steps for preparing the composition:

[0054] Composition Example 1

[0055] Step 1, coprecipitation reaction: dissolve ferric chloride and ferrous chloride in 1000 mL of deionized water to prepare a solution, add aluminum chloride thereto, add 10 wt % ammonia solution dropwise to the mixed metal salt solution under stirring, adjust the pH value to 11.0, and obtain a suspension including a magnetic composite oxide.

[0056] Wherein, the molar ratio of ferric chloride, ferrous chloride and aluminum chloride is 2:1:3.

[0057] Step 2, preparing magnetic composite oxides: allowing the suspension including the magnetic composite oxides to stand for 4 hours, sucking it at the bottom of the beaker with a magnet, repeatedly washing it with deionized water after flocculation, and then freeze-drying it at -20°C for 5 hours, and calcining it at 500°C for 1 hour to obtain Al2O3-Fe3O4 magnetic composite oxides.

[0058] Step 3, loading potassium salt: put Al2O3-Fe3O4 magnetic composite oxide into a beaker, add potassium hydroxide solid and 500 mL of deionized water, immerse and stir for 4 hours, and then dry at 80°C to obtain a composite intermediate.

[0059] Wherein, the mass ratio of Al2O3-Fe3O4 magnetic composite oxide to potassium hydroxide solid is 0.7:0.3.

[0060] Step 4, preparing the composition: calcining the composition intermediate at 500° C. for 4 h to obtain a K-Al2O3-Fe3O4 composition.

[0061] Composition Example 2

[0062] Step 1, coprecipitation reaction: dissolve ferric chloride and ferrous chloride in 1000 mL of deionized water to prepare a solution, add zirconium oxychloride octahydrate thereto, add 10 wt % ammonia solution dropwise to the mixed metal salt solution under stirring, adjust the pH value to 11.0, and obtain a suspension including a magnetic composite oxide.

[0063] The molar ratio of ferric chloride, ferrous chloride and zirconium oxychloride octahydrate is 2:1:0.15.

[0064] Step 2, preparing magnetic composite oxides: allowing the suspension including the magnetic composite oxides to stand for 4 hours, sucking it at the bottom of the beaker with a magnet, repeatedly washing it with deionized water after flocculation, and then freeze-drying it at -20°C for 5 hours, and calcining it at 500°C for 1 hour to obtain ZrO2-Fe3O4 magnetic composite oxides.

[0065] Step 3, loading potassium salt: put the magnetic composite oxide including ZrO2-Fe3O4 into a beaker, add potassium hydroxide solid and 500 mL of deionized water, immerse and stir for 4 hours, and then dry at 80°C to obtain a composite intermediate.

[0066] Wherein, the mass ratio of ZrO2-Fe3O4 magnetic composite oxide to potassium hydroxide solid is 0.7:0.3.

[0067] Step 4, preparing the composition: calcining the composition intermediate at 500° C. for 4 h to obtain a K-ZrO2-Fe3O4 composition.

[0068] Composition Example 3

[0069] Step 1, coprecipitation reaction: dissolve ferric chloride and ferrous chloride in 1000 mL of deionized water to prepare a solution, add cerium chloride thereto, add 10 wt % ammonia solution dropwise to the mixed metal salt solution under stirring, adjust the pH value to 11.0, and obtain a suspension including a magnetic composite oxide.

[0070] The molar ratio of ferric chloride, ferrous chloride and cerium chloride is 2:1:0.5.

[0071] Step 2, preparing magnetic composite oxides: allowing the suspension including the magnetic composite oxides to stand for 4 hours, sucking it at the bottom of the beaker with a magnet, repeatedly washing it with deionized water after flocculation, and then freeze-drying it at -20°C for 5 hours, and calcining it at 500°C for 1 hour to obtain CeO2-Fe3O4 magnetic composite oxides.

[0072] Step 3, loading potassium salt: put the magnetic composite oxide including CeO2-Fe3O4 into a beaker, add potassium carbonate solid and 500 mL of deionized water, immerse and stir for 4 hours, and then dry at 80°C to obtain a composite intermediate.

[0073] Wherein, the mass ratio of CeO2-Fe3O4 magnetic composite oxide to potassium hydroxide solid is 0.7:0.3.

[0074] Step 4, preparing the composition: calcining the composition intermediate at 800° C. for 4 h to obtain a K-CeO2-Fe3O4 composition.

[0075] The following are the steps for the synthesis of polycarbonate diol:

[0076] Embodiment 1

[0077] Step 1, transesterification and polycondensation: add dimethyl carbonate and 1,4-butanediol in a molar ratio of 1.2:1 to the reactor, add 0.1wt% of K-Al2O3-Fe3O4 composition to the reactor, introduce nitrogen at a pressure of 30KPa, heat to 140°C for 2h, then gradually heat to 180°C for 2h, until no fraction is produced. At this point, the transesterification reaction is over. Then, the reaction pressure is gradually reduced at a pressure reduction rate of 0.01KPa / s to 10KPa for 4h of polycondensation to obtain a crude product.

[0078] Step 2, recovering the composition: dissolving the crude product in dichloromethane, using a magnet to adsorb the K-Al2O3-Fe3O4 composition, and separating the polycarbonate diol. Then, the polycarbonate diol is placed in ethanol and purified by a precipitation method to obtain the purified polycarbonate diol.

[0079] Embodiment 2

[0080] Step 1, transesterification reaction and polycondensation reaction: add dimethyl carbonate and 1,6-hexanediol in a molar ratio of 1.2:1 to a reactor, add 0.2wt% of K-Al2O3-Fe3O4 composition to the reactor, introduce nitrogen at a pressure of 30KPa, heat to 140°C for 2h, then gradually heat to 180°C for 2h, until no fraction is produced. At this point, the transesterification reaction is completed. Then, the reaction pressure is gradually reduced at a pressure reduction rate of 0.01KPa / s to 10KPa for 4h of polycondensation reaction to obtain a crude product.

[0081] Step 2, recovering the composition: dissolving the crude product in dichloromethane, using a magnet to adsorb the K-Al2O3-Fe3O4 composition, and separating the polycarbonate diol. Then, the polycarbonate diol is placed in ethanol and purified by a precipitation method to obtain the purified polycarbonate diol.

[0082] Embodiment 3

[0083] Step 1, transesterification reaction and polycondensation reaction: add dimethyl carbonate, 1,6-butanediol and 1,4-butanediol to a reactor, add 0.2wt% of K-Al2O3-Fe3O4 composition to the reactor, introduce nitrogen at a pressure of 30KPa, heat to 140°C for 2h, then gradually increase the temperature to 180°C for 2h, until no fraction is produced. At this point, the transesterification reaction is completed. Then, the reaction pressure is gradually reduced at a pressure reduction rate of 0.01KPa / s to 8KPa for polycondensation reaction for 3.5h to obtain a crude product.

[0084] The molar ratio of dimethyl carbonate, 1,6-hexanediol and 1,4-butanediol is 1.3:0.5:0.5.

[0085] Step 2, recovering the composition: dissolving the crude product in dichloromethane, using a magnet to adsorb the K-Al2O3-Fe3O4 composition, and separating the polycarbonate diol. Then, the polycarbonate diol is placed in ethanol and purified by a precipitation method to obtain the purified polycarbonate diol.

[0086] Embodiment 4

[0087] Step 1, transesterification reaction and polycondensation reaction: add dimethyl carbonate and 1,4-butanediol in a molar ratio of 1.2:1 to a reactor, add 0.1wt% of K-ZrO2-Fe3O4 composition to the reactor, introduce nitrogen at a pressure of 30KPa, heat to 140°C for 2h, then gradually heat to 180°C for 2h, until no fraction is produced. At this point, the transesterification reaction is complete. Then, the reaction pressure is gradually reduced at a pressure reduction rate of 0.005KPa / s to 10KPa for 4h of polycondensation reaction to obtain a crude product.

[0088] Step 2, recovering the composition: dissolving the crude product in dichloromethane, using a magnet to adsorb the K-ZrO2-Fe3O4 composition, and separating the polycarbonate diol. Then, the polycarbonate diol is placed in ethanol and purified by a precipitation method to obtain the purified polycarbonate diol.

[0089] Embodiment 5

[0090] Step 1, transesterification reaction and polycondensation reaction: add dimethyl carbonate and 1,4-butanediol in a molar ratio of 1.2:1 to a reactor, add 0.1wt% of K-CeO2-Fe3O4 composition to the reactor, introduce nitrogen at a pressure of 40KPa, heat to 140°C for 2h, then gradually heat to 180°C for 2h, until no fraction is produced. At this point, the transesterification reaction is completed. Then, the reaction pressure is gradually reduced at a pressure reduction rate of 0.01KPa / s to 10KPa for 4h of polycondensation reaction to obtain a crude product.

[0091] Step 2, recovering the composition: dissolving the crude product in dichloromethane, using a magnet to adsorb the K-CeO2-Fe3O4 composition, and separating the polycarbonate diol. Then, the polycarbonate diol is placed in ethanol and purified by a precipitation method to obtain the purified polycarbonate diol.

[0092] Embodiment 6

[0093] Step 1, transesterification reaction and polycondensation reaction: dimethyl carbonate, 1,4-butanediol and 1,6-hexanediol are added to the reactor, 0.2wt% of K-CeO2-Fe3O4 composition is added to the reactor, nitrogen with a pressure of 40KPa is introduced, the temperature is raised to 150°C for 2h, and then gradually raised to 190°C for 2h until no fraction is produced. At this point, the transesterification reaction is completed. Then, the reaction pressure is gradually reduced at a pressure reduction rate of 0.01KPa / s to 15KPa for polycondensation reaction for 3.5h to obtain a crude product.

[0094] The molar ratio of dimethyl carbonate, 1,4-butanediol and 1,6-hexanediol is 1.3:0.5:0.5.

[0095] Step 2, recovering the composition: dissolving the crude product in dichloromethane, using a magnet to adsorb the K-CeO2-Fe3O4 composition, and separating the polycarbonate diol. Then, the polycarbonate diol is placed in ethanol and purified by a precipitation method to obtain the purified polycarbonate diol.

[0096] Embodiment 7

[0097] Step 1, transesterification reaction and polycondensation reaction: add dimethyl carbonate and 1,4-butanediol in a molar ratio of 1.2:1 to the reactor, add 0.1wt% of K-Al2O3-Fe3O4 composition to the reactor, introduce nitrogen at a pressure of 40KPa, heat to 140°C for 2h, then gradually heat to 180°C for 2h, until no fraction is produced. At this point, the transesterification reaction is completed. Then, the reaction pressure is gradually reduced at a pressure reduction rate of 0.01KPa / s to 10KPa for 4h of polycondensation reaction to obtain a crude product.

[0098] Step 2, recovering the composition: dissolving the crude product in dichloromethane, using a magnet to adsorb the K-Al2O3-Fe3O4 composition, and separating the polycarbonate diol. Then, the polycarbonate diol is placed in ethanol and purified by a precipitation method to obtain the purified polycarbonate diol.

[0099] Comparative Example 1

[0100] The solution of Example 1 was adopted, except that Al2O3-Fe3O4 was directly used as a catalyst. Finally, no transesterification reaction and polycondensation reaction were observed.

[0101] Comparative Example 2

[0102] The solution of Example 2 is adopted, except that sodium methoxide is used as the catalyst.

[0103] Table 1 shows the product performance results of Examples 1 to 7 and Comparative Examples 1 to 2.

[0104] Table 1

[0105]

[0106] 1. As can be seen from Table 1, the diol hydroxyl value and acid value of the polycarbonate diol prepared in Examples 1 to 7 are much higher than those of the polycarbonate diol prepared in Comparative Example 2. It can be seen that the composition in the present application has a strong reaction activity and a large amount of polycarbonate diol is generated.

[0107] 2. As can be seen from Table 1, the number average molecular weight of the polycarbonate diol prepared in Comparative Example 2 is much higher than the number average molecular weight of the polycarbonate diol prepared in Examples 1 to 7, but its hydroxyl value and acid value do not increase significantly, indicating that when sodium methoxide is used as a catalyst, a certain amount of catalyst is bound to remain in the polycarbonate diol after the reaction is completed. It can be seen that the composition used in this application not only has high activity and stability, but is also easy to separate.

[0108] The above is only a specific implementation of the present application. Obviously, various modifications and combinations can be made without departing from the spirit and scope of the present application. Accordingly, this specification and the drawings are only exemplary illustrations of the present application as defined by the attached claims, and are deemed to have covered any and all modifications, changes, combinations or equivalents within the scope of the present application. Obviously, those skilled in the art can make various changes and modifications to the present application without departing from the spirit and scope of the present application. Thus, if these modifications and variations of the present application fall within the scope of the claims of the present application and their equivalents, the present application is intended to include these changes and variations. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be covered within the scope of protection of the present application. Therefore, the scope of protection of the present application shall be based on the scope of protection of the claims.

[0109] It should also be noted that in the system and method of the present disclosure, each component or each step can be decomposed and / or recombined. Such decomposition and / or recombination should be regarded as equivalent solutions of the present disclosure.

[0110] The above description of the disclosed aspects is provided to enable any person skilled in the art to make or use the present disclosure. Various modifications to these aspects will be readily apparent to those skilled in the art, and the general principles defined herein may be applied to other aspects without departing from the scope of the present disclosure. Therefore, the present disclosure is not intended to be limited to the aspects shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

[0111] The above description has been given for the purpose of illustration and description. In addition, this description is not intended to limit the embodiments of the present disclosure to the forms disclosed herein. Although multiple example aspects and embodiments have been discussed above, those skilled in the art will recognize certain variations, modifications, changes, additions and sub-combinations thereof.

Claims

1. A composition, characterized in that The raw materials of the composition include: a magnetic composite oxide and a potassium salt supported on the magnetic composite oxide, wherein the mass ratio of the potassium element contained in the potassium salt to the composition is (0.0001-0.3):1; the potassium salt includes at least one of potassium nitrate, potassium hydroxide and potassium carbonate; The magnetic composite oxide comprises a first component metal oxide and a second component metal oxide, the first component metal oxide comprises at least one of aluminum oxide, zirconium oxide and cerium oxide, and the second component metal oxide is iron oxide.

2. The composition according to claim 1, characterized in that The molar ratio of the metal element contained in the first component metal oxide to the iron element contained in the iron oxide is (0.05-1):

1.

3. The composition according to claim 1 or 2, characterized in that The iron source of the iron oxide includes at least one of ferric chloride and ferrous chloride, the aluminum source of the aluminum oxide includes at least one of aluminum chloride, aluminum sulfate and aluminum nitrate, the zirconium source of the zirconium oxide includes at least one of zirconium oxychloride octahydrate and zirconium chloride, and the cerium source of the cerium oxide includes at least one of cerium chloride, cerium nitrate and cerium sulfate.

4. A method for preparing the composition according to any one of claims 1 to 3, characterized in that: include: Step 1, coprecipitation reaction: adding a weak base to the prepared raw material premix of the magnetic composite oxide to carry out a coprecipitation reaction until the pH value of the raw material premix reaches 11.0, thereby obtaining a suspension including the magnetic composite oxide; Step 2, preparing a magnetic composite oxide: applying an external magnetic field to cause the suspension to precipitate, and then sequentially performing a washing treatment, a drying treatment and a first calcination treatment to obtain a magnetic composite oxide; Step 3, loading potassium salt: immersing the magnetic composite oxide in a potassium salt solution, and drying after immersion to obtain a composite intermediate; Step 4, preparing the composition: performing a second calcination treatment on the composition intermediate to obtain the composition.

5. The method for preparing the composition according to claim 4, characterized in that: Step 1 also includes: preparing a raw material premix solution step; the step of preparing a raw material premix solution includes: The iron source, the first component metal source and deionized water are mixed to obtain a raw material premix solution; the first component metal source includes at least one of an aluminum source, a zirconium source and a cerium source.

6. The method for preparing the composition according to claim 4, characterized in that: In step 2, before applying an external magnetic field to cause the suspension to precipitate, an aging step is also included; the aging step includes: The suspension is allowed to stand for 1 to 4 hours.

7. The method for preparing the composition according to claim 4, characterized in that: In step 2, the temperature of the first calcination treatment is 400-600° C., and the time of the first calcination treatment is 0.5-2 h.

8. The method for preparing the composition according to claim 4, characterized in that: In step 4, the temperature of the second calcination treatment is 300-1000° C., and the time of the second calcination treatment is 3-12 hours.

9. Use of a product obtained by the method for preparing the composition according to any one of claims 1 to 3 or the composition according to any one of claims 4 to 8 in transesterification reaction and / or polycondensation reaction.

10. The use according to claim 9, characterized in that The application is application in a catalyst for preparing polycarbonate diol.

11. The use according to claim 10, characterized in that The synthesis method of the polycarbonate diol comprises: Step 1, transesterification reaction and polycondensation reaction: in the presence of the composition of any one of claims 1 to 3 and an inert atmosphere, sequentially subjecting a diol to a transesterification reaction and a polycondensation reaction with a carbonate to obtain a crude product; Step 2, recovering the composition: dissolving the crude product in an organic solvent, recovering the composition in the crude product by using a magnetic field, and separating the polycarbonate diol.

12. The use according to claim 11, characterized in that In step 1, the dosage of the composition is 0.001 wt% to 1 wt%.

13. The use according to claim 11, characterized in that In step 1, the pressure of the inert atmosphere is 30 to 100 KPa, the temperature of the transesterification reaction is 140 to 220° C., and the time of the transesterification reaction is 1 to 4 hours.

14. The use according to claim 11, characterized in that In step 1, the diol includes aliphatic diol of C3 to C15.

15. The use according to claim 14, characterized in that The aliphatic diol includes at least one of 1,3-propylene glycol, 1,4-propylene glycol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, tricyclodecane dimethanol, pentacyclopentadecanedimethanol, 2,6-decahydronaphtalene dimethanol, 1,5-decahydronaphtalene dimethanol, 2,3-decahydronaphtalene dimethanol, 2,3-norbornane dimethanol, 2,5-norbornane dimethanol and 1,3-adamantanedimethanol.

16. The use according to claim 11, characterized in that In step 1, the carbonate includes at least one of dimethyl carbonate, diethyl carbonate and dibutyl carbonate.

17. The use according to any one of claims 11 to 16, characterized in that: The molar ratio of the diol to the carbonate is 1:(1-1.6).

18. The use according to claim 11, characterized in that In step 1, the polycondensation reaction includes: performing a polycondensation reaction on the product after the ester exchange reaction by adopting a gradient pressure reduction method.

19. The use according to claim 18, characterized in that The gradient pressure reduction rate is 0.001-0.01 KPa / s, the polycondensation reaction pressure is 1-50 KPa, the polycondensation reaction temperature is 180-220° C., and the polycondensation reaction time is 1-5 hours.

20. The use according to claim 11, characterized in that Step 2 also includes: a post-processing step; the post-processing step includes: The polycarbonate diol is purified by a precipitation method.

Citation Information

Cited By

  • Method for appreciation conversion of polycarbonate into phenol

    CN119775105A

  • A method for upgrading polycarbonate to phenol

    CN119775105B