Crosslinked fluorine-containing polyarylether membrane material as well as preparation method and application thereof

By introducing trifluoroisopropyl and perfluorobiphenyl structures into the polymer and carrying out allyl crosslinking reaction, the problem of insufficient dielectric constant of traditional polyarylether is solved, and low dielectric constant and high mechanical properties are achieved The crosslinked fluorine-containing polyarylether film material is suitable for the fifth generation of communications and microelectronics fields.

CN118978689AActive Publication Date: 2024-11-19CHANGZHOU UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411070438.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The traditional polyarylether dielectric constant cannot meet the needs of fifth-generation communication technology and ultra-large-scale integrated circuits, resulting in increased delay and power consumption in electronic devices during miniaturization.

Method used

By introducing large free volumes of low polar trifluoroisopropyl and perfluorobiphenyl structures into the polymer structure, and crosslinking reactions are carried out using crosslinkable allyl side groups to form a crosslinking network to reduce dielectric Constant and dielectric loss improve dimensional stability and thermal stability.

Benefits of technology

It achieves a low dielectric constant and dielectric loss, improves hydrophobic performance and mechanical properties, is suitable for membrane materials in the fields of communications and microelectronics, and is easy to prepare and the products are easy to be used in industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978689A_ABST
    Figure CN118978689A_ABST
Patent Text Reader

Abstract

The invention provides a cross-linked fluorine-containing polyarylether membrane material, the molecular formula of the cross-linked fluorine-containing polyarylether membrane material is as shown in the formula 1: # imgabs0 #, in the structural formula 1, the content x is 0.1-0.4, the content 1-x is 0.6-0.9, and the content n is 40-70, the cross-linked fluorine-containing polyarylether membrane material has low dielectric constant, low dielectric loss and low water absorption rate, has excellent thermodynamic property, and can be used for preparing a high-temperature-resistant material. The method has potential application value in the fields of communication and microelectronics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polyarylether membrane materials and preparation thereof, and in particular relates to a cross-linked fluorine-containing polyarylether membrane material and a preparation method and application thereof. Background Art

[0002] With the advent of the fifth generation of communication technology and the rapid development of ultra-large-scale integrated circuits, the size of electronic devices in circuits has gradually become smaller and even miniaturized. However, the miniaturization of circuits leads to increased delays and power consumption of resistance and capacitance. Therefore, there is an urgent need to develop high-performance low dielectric constant materials to reduce these adverse effects and improve the performance of electronic equipment. Traditional polyarylether resins contain a large number of aromatic rings in their structure, and the rigidity of the molecular chain is very strong, so they have excellent dimensional stability, friction resistance, thermal stability and excellent mechanical properties; the aromatic ether bonds in the structure can guarantee the flexibility of the molecular chain to a certain extent. Moreover, polyarylether has a low dielectric constant and dielectric loss in a wide frequency range, which is suitable for application in low dielectric materials.

[0003] However, with the development of communication and microelectronics technology, the dielectric constant of traditional polyarylether is about 3 to 5, and the dielectric constant of traditional polyarylether can no longer meet the demand. Therefore, in order to further develop polyarylether interlayer dielectric materials, it is necessary to optimize the molecular structure to improve its dielectric properties. Summary of the invention

[0004] The purpose of the present invention is to provide a cross-linked fluorinated polyarylether membrane material and a preparation method and application thereof in view of the above shortcomings. By introducing low-polarity trifluoroisopropyl and perfluorobiphenyl structures with large free volume into the polymer structure, the polymer has lower surface free energy, dielectric constant and stronger dimensional stability and thermal stability; at the same time, cross-linkable allyl side groups are also introduced into the polymer structure. The allyl groups serve as cross-linking sites, undergo cross-linking reactions, form a cross-linked network, restrict the movement of chain segments, further reduce the dielectric constant, and improve the dielectric properties. The polyarylether polymer has important potential application value in the fields of communications and microelectronics.

[0005] In one aspect, the present invention provides a cross-linked fluorinated polyarylether membrane material, wherein the molecular formula of the cross-linked fluorinated polyarylether membrane material is as shown in Formula 1:

[0006]

[0007] In the structural formula 1, the content x=0.1-0.4, 1-x=0.6-0.9, and n=40-70.

[0008] The cross-linked fluorinated polyarylether membrane material is prepared by high-temperature cross-linking of a cross-linkable fluorinated polyarylether containing an allyl structure. The molecular structure of the cross-linkable fluorinated polyarylether containing an allyl structure is shown in Formula 2:

[0009]

[0010] The structural formula 2 is divided into a cross-linkable structural unit and a non-cross-linkable structural unit, the content of the cross-linkable structural unit is x=0.1-0.4, the content of the non-cross-linkable structural unit is 1-x=0.6-0.9, and n=40-70.

[0011] The second aspect of the present invention provides a method for preparing a cross-linked fluorinated polyarylether membrane material, and the synthesis route is as follows:

[0012]

[0013] The specific steps are as follows:

[0014] Step (1) Preparation of cross-linkable fluorinated polyarylether containing allyl structure: adding perfluorobiphenyl, bisphenol AF, 2,2'-diallyl bisphenol A, potassium carbonate and N-methyl-2-pyrrolidone into a three-necked flask equipped with a mechanical stirrer, a water condenser and a nitrogen inlet and outlet, stirring for reaction. After the reaction is completed, a viscous polymer solution is obtained. The polymer solution is slowly poured into ethanol for sedimentation, and a fibrous cross-linkable fluorinated polyarylether containing allyl structure is obtained by filtering, washing and drying.

[0015] Step (2) Preparation of a cross-linkable fluorinated polyarylether film containing an allyl structure: The polyarylether obtained in step (1) is heated and fully dissolved in N-methyl-2-pyrrolidone, and then filtered with a sand core funnel to obtain a uniform solution, the solution is cast on a glass substrate, and then placed in an oven, dried, and after natural cooling, the film is peeled off from the glass substrate to obtain a cross-linkable fluorinated polyarylether film containing an allyl structure;

[0016] Step (3) Preparation of cross-linked fluorinated polyarylether membrane material: The cross-linked fluorinated polyarylether film containing an allyl structure obtained in step (2) is vacuum dried at high temperature to obtain a cross-linked fluorinated polyarylether membrane material after a cross-linking reaction.

[0017] Furthermore, the molar amount of the perfluorobiphenyl is equal to the sum of the molar amounts of 2,2'-diallyl bisphenol A and bisphenol AF, and the molar ratio of 2,2'-diallyl bisphenol A to bisphenol AF is 1:9 to 4:6.

[0018] Furthermore, the molar amount of potassium carbonate is 1 to 2 times the molar amount of perfluorobiphenyl.

[0019] Furthermore, the amount of N-methyl-2-pyrrolidone used is 3 to 5 times the total mass of perfluorobiphenyl, bisphenol AF and 2,2'-diallylbisphenol A.

[0020] Furthermore, the reaction conditions are: reaction temperature 100-120° C., reaction time 4-6 hours.

[0021] Furthermore, the oven drying conditions are: drying at 80°C, 100°C, 120°C, 140°C, 160°C, 180°C, and 200°C for 2h respectively.

[0022] Furthermore, in the step (2), the amount of N-methyl-2-pyrrolidone used is 10-15 times the amount of the cross-linkable fluorinated polyarylether containing an allyl structure.

[0023] Furthermore, in the step (3), the cross-linking conditions are: under vacuum and at a temperature of 250-260°C.

[0024] The third aspect of the present invention further provides an application of a cross-linked fluorinated polyarylether membrane material, wherein the cross-linked fluorinated polyarylether membrane material can be used as a membrane material in the fields of communications and microelectronics.

[0025] Beneficial effects of the present invention:

[0026] (1) The cross-linkable fluorinated polyarylether containing an allyl structure provided by the present invention reduces the polarity and surface free energy of the polymer material by introducing trifluoroisopropyl and perfluorobiphenyl structures, thereby reducing the dielectric constant and dielectric loss of the polymer material and improving the hydrophobicity;

[0027] (2) The cross-linkable fluorinated polyarylether containing an allyl structure provided by the present invention introduces a cross-linkable allyl structure, and the allyl group acts as a cross-linking site to cause a cross-linking reaction to form a cross-linked network, thereby restricting the movement of chain segments and further reducing the dielectric constant, dielectric loss and water absorption rate;

[0028] (3) The polyarylether polymer prepared by the present invention uses readily available starting materials and a relatively simple synthetic route. The product is easy to purify and separate, has a high yield, is stable at room temperature, and is easy to industrialize. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The cross-linkable fluorinated polyarylether (PAE10) containing allyl structure in Example 1 1 H NMR spectrum;

[0030] Figure 2 The cross-linkable fluorinated polyarylether (PAE20) containing allyl structure in Example 2 1 H NMR spectrum;

[0031] Figure 3 The cross-linkable fluorinated polyarylether (PAE30) containing allyl structure in Example 3 1 H NMR spectrum;

[0032] Figure 4 The cross-linkable fluorinated polyarylether (PAE40) containing allyl structure in Example 4 1 H NMR spectrum;

[0033] Figure 5 is the infrared spectrum of the cross-linkable fluorinated polyarylether (UCL-PAE10-40) containing an allyl structure in Examples 1-4;

[0034] Figure 6 The infrared spectra of the cross-linkable fluorinated polyarylether (UCL-PAE40) containing allyl structure and the cross-linked fluorinated polyarylether membrane material (CL-PAE40) in Example 4 are compared;

[0035] Figure 7 is a relationship diagram between the dielectric constant and the electric field frequency change of the cross-linkable fluorinated polyarylether film containing allyl structure (UCL-PAE10-40) and the cross-linked fluorinated polyarylether film material (CL-PAE10-40) in Examples 1-4;

[0036] Figure 8 is the C1s XPS spectrum of the cross-linkable fluorinated polyarylether film (UCL-PAE40) containing an allyl structure in Example 4;

[0037] Fig. 9 It is the C1s XPS spectrum of the cross-linked fluorinated polyarylether membrane material (CL-PAE40) in Example 4. DETAILED DESCRIPTION

[0038] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification. The methods described are all conventional methods unless otherwise specified, and the raw materials described can be obtained from public commercial channels unless otherwise specified.

[0039] The term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0040] The sources of the drugs and reagents described in the examples are as follows:

[0041] 2,2-Bis(4-hydroxyphenyl)hexafluoropropane (bisphenol AF): Tokyo Chemical Industry Co., Ltd., purity>98%.

[0042] 2,2'-Diallylbisphenol A: Shanghai MacLean Biochemical Technology Co., Ltd., purity 90%.

[0043] Perfluorobiphenyl: Wuhan Changcheng Chemical Technology Development Co., Ltd., purity >98%.

[0044] N-Methyl-2-pyrrolidone (NMP): Shanghai Lingfeng Chemical Reagent Co., Ltd., purity ≥99%.

[0045] Anhydrous potassium carbonate (K2CO3): Shanghai Lingfeng Chemical Reagent Co., Ltd., purity ≥99%.

[0046] The specific preparation method is as follows:

[0047] Step (1) Preparation of cross-linkable fluorinated polyarylether containing allyl structure: adding perfluorobiphenyl, bisphenol AF, 2,2'-diallyl bisphenol A, potassium carbonate and N-methyl-2-pyrrolidone into a three-necked flask equipped with a mechanical stirrer, a water condenser and a nitrogen inlet and outlet, stirring for reaction. After the reaction is completed, a viscous polymer solution is obtained. The polymer solution is slowly poured into ethanol for sedimentation, and a fibrous cross-linkable fluorinated polyarylether containing allyl structure is obtained by filtering, washing and drying.

[0048] Step (2) Preparation of a cross-linkable fluorinated polyarylether film containing an allyl structure: The polyarylether obtained in step (1) is heated and fully dissolved in N-methyl-2-pyrrolidone, and then filtered with a sand core funnel to obtain a uniform solution, the solution is cast on a glass substrate, and then placed in an oven, dried, and after natural cooling, the film is peeled off from the glass substrate to obtain a cross-linkable fluorinated polyarylether film containing an allyl structure.

[0049] Step (3) Preparation of cross-linked fluorinated polyarylether membrane material: The cross-linked fluorinated polyarylether film containing an allyl structure obtained in step (2) is vacuum dried at high temperature to obtain a cross-linked fluorinated polyarylether membrane material after a cross-linking reaction.

[0050] Preferably, the molar amount of the perfluorobiphenyl is equal to the sum of the molar amounts of 2,2'-diallyl bisphenol A and bisphenol AF, and the molar ratio of 2,2'-diallyl bisphenol A to bisphenol AF is 1:9 to 4:6; the molar amount of potassium carbonate is 1 to 2 times the molar amount of perfluorobiphenyl; the amount of N-methyl-2-pyrrolidone is 3 to 5 times the total mass of perfluorobiphenyl, bisphenol AF and 2,2'-diallyl bisphenol A; the reaction conditions are: The reaction temperature is 100-120°C and the reaction time is 4-6 hours; the oven drying conditions are: drying for 2 hours at 80°C, 100°C, 120°C, 140°C, 160°C, 180°C and 200°C respectively; in the step (2), the amount of N-methyl-2-pyrrolidone is 10-15 times the amount of the cross-linkable fluorinated polyarylether containing an allyl structure; in the step (3), the cross-linking conditions are: under vacuum, the temperature is 250-260°C.

[0051] The following is a detailed description of the raw material feeding amount and the specific reaction conditions in the examples.

[0052] Example 1

[0053] Step (1) Preparation of cross-linkable fluorinated polyarylether (PAE10) containing allyl structure

[0054] Perfluorobiphenyl (4.0093 g, 12 mmol), bisphenol AF (3.6313 g, 10.8 mmol), 2,2'-diallylbisphenol A (0.3701 g, 1.2 mmol), potassium carbonate (2.6536 g, 19.2 mmol), and 26 mL of N-methyl-2-pyrrolidone were added to a 100 mL three-necked flask equipped with a mechanical stirrer, a water condenser, and a nitrogen inlet and outlet. The reaction was stirred at 100 ° C for 4 hours, and the reaction was terminated. The polymer solution was poured into ethanol for precipitation, and further filtered, washed, and dried to obtain a fibrous allyl-structured cross-linkable fluorinated polyarylether (PAE10). The molar yield was 87%; 1H-NMR (CDCl3, 400 MHz) was as shown in the attached figure. Figure 1 As shown, the data were recorded by Bruker AVANCE III 400M digital NMR spectrometer using CDCl3 as solvent. 1 H NMR spectrum; FT-IR Figure 5 shown.

[0055] Step (2) Preparation of cross-linkable fluorinated polyarylether film (UCL-PAE10) containing allyl structure The obtained dry polymer (2 g) was heated and fully dissolved in N-methyl-2-pyrrolidone (20 mL), and then filtered with a sand core funnel to obtain a uniform solution. The uniform solution was cast on a glass substrate (inner diameter of about 8 cm×8 cm), and then placed in a flat-bottom oven and dried at 80°C, 100°C, 120°C, 140°C, 160°C, 180°C, and 200°C for 2 h. After natural cooling, the film (thickness of about 0.25 mm) was peeled off from the glass substrate to obtain a cross-linkable fluorinated polyarylether film (UCL-PAE10) containing allyl structure. The prepared 0.25 mm (UCL-PAE10) film was used for thermal and dielectric properties tests, and the prepared 0.2 mm (UCL-PAE10) film was used for infrared characterization. The preparation method was consistent with the above.

[0056] Step (3) Preparation of cross-linked fluorinated polyarylether membrane material (CL-PAE10)

[0057] The film was vacuum dried at 260° C. for 2 hours to perform a cross-linking reaction, thereby preparing a cross-linked fluorinated polyarylether membrane material (CL-PAE10).

[0058] Example 2

[0059] Step (1) Preparation of cross-linkable fluorinated polyarylether (PAE20) containing allyl structure

[0060] Perfluorobiphenyl (4.0093 g, 12 mmol), bisphenol AF (3.2278 g, 9.6 mmol), 2,2'-diallylbisphenol A (0.7402 g, 2.4 mmol), potassium carbonate (2.6536 g, 19.2 mmol), and 26 mL of N-methyl-2-pyrrolidone were added to a 100 mL three-necked flask with a mechanical stirrer, a water condenser, and a nitrogen inlet and outlet. The reaction was stirred at 110 ° C for 4 hours, and the reaction was terminated. The polymer solution was poured into ethanol for sedimentation, and further filtered, washed, and dried to obtain a fibrous allyl-structured cross-linkable fluorinated polyarylether (PAE20). The molar yield was 88%; 1 H-NMR (CDCl3, 400MHz) as attached Figure 2 As shown; FT-IR as Figure 5 shown.

[0061] Step (2) Preparation of cross-linkable fluorinated polyarylether film (UCL-PAE20) containing allyl structure The obtained dry polymer (2 g) was heated and fully dissolved in N-methyl-2-pyrrolidone (20 mL), and then filtered with a sand core funnel to obtain a uniform solution. The uniform solution was cast on a glass substrate (inner diameter of about 8 cm×8 cm), and then placed in a flat-bottom oven and dried at 80°C, 100°C, 120°C, 140°C, 160°C, 180°C, and 200°C for 2 h. After natural cooling, the film (thickness of about 0.25 mm) was peeled off from the glass substrate to obtain a cross-linkable fluorinated polyarylether film (UCL-PAE20) containing allyl structure. The prepared 0.25 mm (UCL-PAE20) film was used for thermal and dielectric properties tests, and the prepared 0.2 mm (UCL-PAE20) film was used for infrared characterization. The preparation method was consistent with the above.

[0062] Step (3) Preparation of cross-linked polymer film (CL-PAE20)

[0063] The film was vacuum dried at 260° C. for 2 hours and further heat treated to prepare a cross-linked fluorinated polyarylether membrane material (CL-PAE20).

[0064] Example 3

[0065] Step (1) Preparation of cross-linkable fluorinated polyarylether (PAE30) containing allyl structure

[0066] Perfluorobiphenyl (4.0093 g, 12 mmol), bisphenol AF (2.8243 g, 8.4 mmol), 2,2'-diallylbisphenol A (1.1103 g, 3.6 mmol), potassium carbonate (2.6536 g, 19.2 mmol), and 26 mL of N-methyl-2-pyrrolidone were added to a 100 mL three-necked flask with a mechanical stirrer, a water condenser, and a nitrogen inlet and outlet. The reaction was stirred at 110 ° C for 5 hours, and the reaction was terminated. The polymer solution was poured into ethanol for precipitation, and further filtered, washed, and dried to obtain a fibrous allyl-structured cross-linkable fluorinated polyarylether (PAE30). The molar yield was 87%; 1 H-NMR (CDCl3, 400MHz) as attached Figure 3 As shown; FT-IR as Figure 5 shown.

[0067] Step (2) Preparation of cross-linkable fluorinated polyarylether film (UCL-PAE30) containing allyl structure The obtained dry polymer (2 g) was heated and fully dissolved in N-methyl-2-pyrrolidone (20 mL), and then filtered with a sand core funnel to obtain a uniform solution. The uniform solution was cast on a glass substrate (inner diameter of about 8 cm×8 cm), and then placed in a flat-bottom oven and dried at 80°C, 100°C, 120°C, 140°C, 160°C, 180°C, and 200°C for 2 h. After natural cooling, the film (thickness of about 0.25 mm) was peeled off from the glass substrate to obtain a cross-linkable fluorinated polyarylether film (UCL-PAE30) containing allyl structure. The prepared 0.25 mm (UCL-PAE30) film was used for thermal and dielectric properties tests, and the prepared 0.2 mm (UCL-PAE30) film was used for infrared characterization. The preparation method was consistent with the above.

[0068] Step (3) Preparation of cross-linked fluorinated polyarylether membrane material (CL-PAE30)

[0069] The film was vacuum dried at 260° C. for 2 hours and further heat treated to prepare a cross-linked fluorinated polyarylether film material (CL-PAE30).

[0070] Example 4

[0071] Step (1) Preparation of cross-linkable fluorinated polyarylether (PAE40) containing allyl structure

[0072] Perfluorobiphenyl (4.0093g, 12mmol), bisphenol AF (2.4208g, 7.2mmol), 2,2'-diallylbisphenol A (1.4804g, 4.8mmol), potassium carbonate (2.6536g, 19.2mmol), and 26mL N-methyl-2-pyrrolidone were added to a 100mL three-necked flask with a mechanical stirrer, a water condenser, and a nitrogen inlet and outlet. The reaction was stirred at 120°C for 6 hours, and the reaction was terminated. The polymer solution was poured into ethanol for sedimentation, and further filtered, washed, and dried to obtain a fibrous allyl-structured cross-linkable fluorinated polyarylether (PAE40). The molar yield was 86%; 1 H-NMR (CDCl3, 400MHz) as attached Figure 4 As shown; FT-IR as Figure 5 shown.

[0073] Step (2) Preparation of cross-linkable fluorinated polyarylether film (UCL-PAE40) containing allyl structure The obtained dry polymer (2 g) was heated and fully dissolved in N-methyl-2-pyrrolidone (20 mL), and then filtered with a sand core funnel to obtain a uniform solution. The uniform solution was cast on a glass substrate (inner diameter of about 8 cm×8 cm), and then placed in a flat-bottom oven and dried at 80°C, 100°C, 120°C, 140°C, 160°C, 180°C, and 200°C for 2 h. After natural cooling, the film (thickness of about 0.25 mm) was peeled off from the glass substrate to obtain a cross-linkable fluorinated polyarylether film (UCL-PAE40) containing allyl structure. The prepared 0.25 mm (UCL-PAE40) film was used for thermal and dielectric properties tests, and the prepared 0.2 mm (UCL-PAE40) film was used for infrared characterization. The preparation method was consistent with the above.

[0074] Step (3) Preparation of cross-linked fluorinated polyarylether membrane material (CL-PAE40)

[0075] The film was vacuum dried at 260° C. for 2 hours and further heat treated to prepare a cross-linked fluorinated polyarylether membrane material (CL-PAE40).

[0076] NMR analysis: Figure 1-4 In the above, the chemical shifts at 6.5-8.0 ppm are attributed to the protons on the aromatic rings. The chemical shifts at 6.01 ppm, 5.07 ppm and 3.53 ppm are characteristic peaks of allyl groups. The chemical shift at 1.65 ppm is a characteristic peak of methyl groups.

[0077] Figure 5 Shown are infrared spectra of the cross-linkable fluorinated polyarylether membranes (UCL-PAE10-40) containing an allyl structure in Examples 1-4.

[0078] Analysis: at 1695cm -1 Typical C=C bond vibration absorption peaks appeared at 1607, 1649, 1506, 1480 cm -1 The absorption peak of the skeleton vibration of the benzene ring appears at 1223cm -1 and 1070cm -1 The asymmetric and symmetric vibration peaks of the aromatic ether bond appeared. 1172cm -1 The characteristic peak at 978cm is attributed to the trifluoromethyl group. -1 The peak at 724 cm is attributed to the CF bond; -1 The peak at is attributed to the out-of-plane bending of the aromatic -CH bonds.

[0079] Figure 6 The figure shows the infrared spectrum comparison of the cross-linkable fluorinated polyarylether containing allyl structure (UCL-PAE40) and the cross-linked fluorinated polyarylether membrane material (CL-PAE40) in Example 4.

[0080] Test method: FTIR spectra were recorded on a Nicolet iS 50 Fourier transform infrared spectrometer (4000-400 cm -1 ).

[0081] Analysis: UCL-PAE40 at 1695cm -1 A vibration absorption peak of the C=C bond appeared at , and the absorption peak of the cross-linked polymer CL-PAE40 at this position completely disappeared, indicating that the double bonds had completely undergone cross-linking reaction after high-temperature thermal curing.

[0082] Figure 7 4 is a graph showing the relationship between the dielectric constant and the electric field frequency of the cross-linkable fluorinated polyarylether film containing an allyl structure (UCL-PAE10-40) and the cross-linked film (CL-PAE10-40) in Examples 1-4.

[0083] Figure 8 is the C1s XPS spectrum of the cross-linkable fluorinated polyarylether (UCL-PAE40) containing an allyl structure in Example 4;

[0084] Fig. 9 This is the C1s XPS spectrum of the cross-linked fluorinated polyarylether membrane material (CL-PAE40) in Example 4.

[0085] pass Figure 8 and Fig. 9Comparison and analysis: For UCL-PAE40 before cross-linking, the characteristic peaks are located at 292.3, 286.6, 284.8, and 284.2 eV, which are attributed to CF, COC, CC, and C=C bonds, respectively. The characteristic peak at 288.2 eV is attributed to the C=O bond, which may be due to the long-term exposure of the sample to air and the adsorption of CO2 on the surface. The disappearance of the C=C bond peak in the C1s core energy level spectrum of CL-PAE40 further indicates the success of cross-linking.

[0086] Test method: PHI 5000VersaProbe III X-ray photoelectron spectrometer was used to test the elemental composition of the film surface.

[0087] Table 1 Molecular weight of cross-linkable fluorinated polyarylether containing allyl structure

[0088]

[0089]

[0090] Table 1 shows the number average molecular weight, weight average molecular weight and polydispersity index (PDI) of crosslinkable fluorinated polyarylether PAE10-40 containing allyl structure dissolved in tetrahydrofuran. Table 1 lists the molecular weight data of polyarylether PAE10-40, and their number average molecular weight values ​​and polydispersity index are in the range of 3.11×104-4.02×104 g / mol and 4.15-4.68, respectively. The results show that crosslinkable fluorinated polyarylether containing allyl structure with moderate molecular weight and molecular weight distribution was successfully prepared.

[0091] The molecular weight of the polymer was measured by a WATERS 515 gel permeation chromatograph. Tetrahydrofuran was used as the solvent at a flow rate of 1.0 mL / min.

[0092] Table 2 Dissolution performance

[0093]

[0094] Note: “++” indicates complete dissolution under room temperature; “+” indicates complete dissolution under heating

[0095] "+-" means partially dissolved under heating; "-" means not dissolved under heating

[0096] Dissolve.

[0097] Table 2 shows the solubility of the cross-linked fluorinated polyarylether membrane UCL-PAE10-40 and the cross-linked fluorinated polyarylether membrane material CL-PAE10-40 containing allyl structure. 0.1g of the cross-linked fluorinated polyarylether containing allyl structure was placed in 10mL of solvent (NMP, DMF, DMSO, THF, CHCl3 and Acetone) to determine the solubility. The cross-linked fluorinated polyarylether showed strong solubility in both strong polar solvents (NMP, DMF, DMSO and THF) and weak polar solvents (CHCl3 and acetone). Before cross-linking, the large free volume of fluorinated isopropyl and allyl groups destroyed the regularity of the polymer chain, increased the distance between the polymer molecular chains, and reduced the interaction between the polymer chains, thus having strong solubility. The cross-linked fluorinated polyarylether membrane materials were insoluble in the solvent, which was attributed to the formation of the cross-linked network, and also indirectly proved the successful cross-linking and curing reaction of the polymer.

[0098] Table 3 Thermal properties

[0099]

[0100] Table 3 shows the thermal properties of the cross-linkable fluorinated polyarylether membrane UCL-PAE10-40 containing allyl structure and the cross-linked fluorinated polyarylether membrane material CL-PAE10-40.

[0101] T 5% is the temperature at which the weight loss is 5%; T max is the temperature at which the decomposition rate is maximum; T g Glass transition temperature.

[0102] Thermogravimetric analysis was recorded on a TG 209F3 thermogravimetric analyzer. The test was carried out under nitrogen atmosphere, with a heating rate of 20°C / min and a temperature range of 50°C to 800°C. The glass transition temperature was measured on a Pyris 1 differential scanning calorimeter produced by Perkin Elmer. The test environment was under nitrogen atmosphere, with a heating rate of 10°C / min and a temperature range of 50°C to 300°C.

[0103] As shown in Table 3, the glass transition temperature of the polymer film before cross-linking decreases with the increase of 2,2'-diallyl bisphenol A content, because the increase of 2,2'-diallyl bisphenol A content increases the allyl content of the polymer side chain, destroys the regularity of the polymer chain, increases the free volume, and reduces the glass transition temperature. On the contrary, the glass transition temperature of the cross-linked fluorinated polyarylether film material increases with the increase of 2,2'-diallyl bisphenol A content, because the increase of allyl content increases the cross-linking network, greatly restricts the movement of the polymer chain segments, and increases the glass transition temperature.

[0104] It can be seen from Table 3 that the T5% of the film before and after cross-linking decreases with the increase of 2,2'-diallyl bisphenol A content. Thermal stability mainly depends on the polymer main chain and side groups. Before cross-linking, the thermal stability of the side chain allyl group is lower than that of the main chain containing rigid benzene rings; after cross-linking, the bond energy of the CC bond of the cross-linked network is lower than that of the main chain containing rigid benzene rings. It can also be seen from Table 3 that the T5% of UCL-PAE10, UCL-PAE20, UCL-PAE30, and UCL-PAE40 increased by 17, 42, 13, and 6 °C respectively after cross-linking, indicating that cross-linking can improve thermal stability. In addition, the maximum thermal decomposition temperature of all samples is higher than 550 °C, and the residual carbon rate at 800 °C is higher than 50%, showing excellent thermal properties.

[0105] Table 4 Mechanical properties

[0106]

[0107] Table 4 shows the mechanical properties of cross-linkable fluorinated polyarylether UCL-PAE10-40 containing allyl structure and cross-linked film CL-PAE10-40.

[0108] The stress-strain curve was obtained from a WDT-10 electronic universal testing machine. The mechanical properties were evaluated by the stress-strain curve. The film was cut into a size of 5 cm × 1 cm. The tensile rate during the test was 5 mm / min, and the experiment was repeated 5 times and the average value was taken.

[0109] It can be seen from Table 4 that the cross-linked network improves the rigidity of the cross-linked fluorinated polyarylether film material chain, so that the elongation at break of the cross-linked film is lower than that of the film before cross-linking, and decreases with the increase of the cross-linked network, from 6.8% to 4.3%. The tensile strength and tensile modulus of all cross-linked fluorinated polyarylether films containing allyl structures are improved after cross-linking, which is due to the formation of the cross-linked network. In addition, the tensile strength and tensile modulus of the cross-linked film (CL-PAEn) show a trend of first increasing and then decreasing with the increase of the allyl content. The improvement of mechanical properties is due to the cross-linking reaction at high temperature, while the decline in performance is attributed to excessive cross-linking. It is worth noting that CL-PAE20 exhibits the best mechanical properties, with a tensile strength of 146.7MPa and a tensile modulus of 4.5GPa. It can be seen from this that moderate cross-linking can improve mechanical properties, and excessive cross-linking will increase the brittleness of the material, thereby reducing the mechanical properties.

[0110] Table 5 Dielectric properties and water absorption

[0111]

[0112] Table 5 shows the dielectric properties and water absorption of the cross-linkable fluorinated polyarylether UCL-PAE10-40 containing allyl structure and the cross-linked fluorinated polyarylether membrane material CL-PAE10-40.

[0113] The dielectric constant and dielectric loss related tests are performed using the TH2826 LCR digital bridge. The test is performed at room temperature with a frequency range of 10Hz-10 6 Hz.

[0114] After the film is immersed in deionized water for a certain period of time, the water absorption rate is obtained according to the formula: W = (m2-m1) / m1×100%, where W is the water absorption rate, m1 is the weight of the sample when it is dry, and m2 is the weight of the sample after being immersed in water for a certain period of time.

[0115] As can be seen from Table 5, the dielectric constant of the uncrosslinked allyl-containing crosslinkable fluorinated polyarylether film at 1MHz is in the range of 2.47-2.97, and increases with the increase of 2,2'-diallylbisphenol A content. This is because the content of 2,2'-diallylbisphenol A increases, the fluorine content decreases, the electronic polarization increases, and the dielectric constant increases. On the contrary, the dielectric constant of the crosslinked fluorinated polyarylether film material decreases with the increase of 2,2'-diallylbisphenol A content, and the dielectric constant at 1MHz is in the range of 1.93-2.24. The crosslinked network structure limits the migration of polymer segments, reduces the dipole orientation, limits the polarization of the polymer electron cloud under the applied electric field, and limits the orientation of the polymer segments in the direction of the external electric field. Therefore, the dielectric constant of the crosslinked film is lower than that of the film before crosslinking. At 1MHz, the dielectric constant of CL-PAE40 is the lowest, only 1.93.

[0116] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Without departing from the scope and technical principles of the described embodiments, many modifications and changes are obvious to those of ordinary skill in the art, and these modifications and changes should also be regarded as the scope of protection of the present invention.

Claims

1. A cross-linked fluorinated polyarylether membrane material, characterized in that: The molecular formula of the cross-linked fluorinated polyarylether membrane material is shown in Formula 1: In the structural formula 1, the content x=0.1-0.4, 1-x=0.6-0.9, and n=40-70.

2. A method for synthesizing the cross-linked fluorinated polyarylether membrane material according to claim 1, characterized in that: The specific steps are as follows: Step (1) Preparation of cross-linkable fluorinated polyarylether containing allyl structure: adding perfluorobiphenyl, bisphenol AF, 2,2'-diallyl bisphenol A, potassium carbonate and N-methyl-2-pyrrolidone into a three-necked flask equipped with a mechanical stirrer, a water condenser and a nitrogen inlet and outlet, stirring for reaction, after the reaction is completed, a viscous polymer solution is obtained, the polymer solution is slowly poured into ethanol for sedimentation, and a fibrous cross-linkable fluorinated polyarylether containing allyl structure is obtained by filtering, washing and drying; Step (2) Preparation of a cross-linkable fluorinated polyarylether film containing an allyl structure: The polyarylether obtained in step (1) is heated and fully dissolved in N-methyl-2-pyrrolidone, and then filtered with a sand core funnel to obtain a uniform solution, the solution is cast on a glass substrate, and then placed in an oven, dried, and after natural cooling, the film is peeled off from the glass substrate to obtain a cross-linkable fluorinated polyarylether film containing an allyl structure. Step (3) Preparation of cross-linked fluorinated polyarylether membrane material: The cross-linked fluorinated polyarylether film containing an allyl structure obtained in step (2) is vacuum dried at high temperature to obtain a cross-linked fluorinated polyarylether membrane material after a cross-linking reaction.

3. The method for synthesizing the cross-linked fluorinated polyarylether membrane material according to claim 2, characterized in that: In the step (1), the molar amount of the perfluorobiphenyl is equal to the sum of the molar amounts of 2,2'-diallyl bisphenol A and bisphenol AF, and the molar ratio of 2,2'-diallyl bisphenol A to bisphenol AF is 1:9 to 4:

6.

4. The method for synthesizing a cross-linked fluorinated polyarylether membrane material according to claim 2, characterized in that: In the step (1), the molar amount of potassium carbonate is 1 to 2 times the molar amount of perfluorobiphenyl.

5. The method for synthesizing a cross-linked fluorinated polyarylether membrane material according to claim 2, characterized in that: In the step (1), the amount of N-methyl-2-pyrrolidone used is 3 to 5 times the total mass of perfluorobiphenyl, bisphenol AF and 2,2'-diallylbisphenol A.

6. The method for synthesizing a cross-linked fluorinated polyarylether membrane material according to claim 2, characterized in that: In the step (1), the reaction conditions are: reaction temperature 100-120° C., reaction time 4-6 hours.

7. The method for synthesizing a cross-linked fluorinated polyarylether membrane material according to claim 2, characterized in that: In the step (2), the oven drying conditions are: drying at 80°C, 100°C, 120°C, 140°C, 160°C, 180°C, and 200°C for 2 hours respectively.

8. The method for synthesizing a cross-linked fluorinated polyarylether membrane material according to claim 2, characterized in that: In the step (2), the amount of N-methyl-2-pyrrolidone used is 10-15 times the amount of the cross-linkable fluorinated polyarylether containing an allyl structure.

9. The method for synthesizing a cross-linked fluorinated polyarylether membrane material according to claim 2, characterized in that: In the step (3), the cross-linking conditions are: under vacuum and at a temperature of 250-260°C.

10. An application of the cross-linked fluorinated polyarylether membrane material as claimed in claim 1, characterized in that: The cross-linked fluorinated polyarylether membrane material can be used as a membrane material in the fields of communications and microelectronics.

Citation Information

Patent Citations

  • High-fluorine content heat-resistant polyarylether resin and preparation method thereof

    CN106750257A

  • Cross-linkable fluorine-containing sulphonated polyarylether compound and preparation method thereof

    CN107573501A

  • Crosslinked or non-crosslinked aromatic (CO)polymers as proton conductors for use in high temperature PEM fuel cells

    US20120202129A1