Flexible infrared stealth phase change material as well as preparation and application thereof

By using a mixing technology of polymer polymer and low-infrared radiation metal particles in composite shaped phase change materials, flexible infrared stealth materials are formed, which solves the problems of material rigidity and high infrared emissivity, and achieves low infrared emissivity and shape stability The effect is suitable for wearable infrared stealth intelligent equipment.

CN118978742AInactive Publication Date: 2024-11-19CHINA UNIV OF MINING & TECH

Patent Information

Application Number
CN202411057335.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing composite shaped phase change materials are difficult to meet the actual application needs due to their inherent rigidity and high infrared emissivity, and there are leakage problems during the phase change, which affects the infrared stealth effect.

Method used

The polymer is mixed with low infrared radiation metal particles to form a flexible carrier, and the phase change material is fully entered into the substrate structure through vacuum impregnation, and a flexible infrared stealth phase change material is produced, reducing its infrared radiation rate and maintaining its shape stable sex.

Benefits of technology

The obtained flexible phase change material has low infrared emissivity and good shape stability, and can be bent above 180° without leakage. It is suitable for wearable infrared stealth intelligent equipment to achieve efficient infrared stealth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978742A_ABST
    Figure CN118978742A_ABST
Patent Text Reader

Abstract

The invention discloses a flexible infrared stealth phase change material as well as preparation and application thereof. A high-molecular polymer is used as a supporting material, low-infrared radiation metal particles are loaded through physical mixing, and a flexible carrier is obtained through freeze drying treatment; and immersing the phase-change material into a flexible carrier through vacuum impregnation to finally prepare the flexible infrared stealth phase-change material. The phase change material has relatively high heat storage density and low infrared radiance, can realize efficient infrared stealth through double ways of reducing target temperature and infrared radiation, and is expected to be applied to the field of wearable infrared stealth intelligent equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of flexible composite shaped phase change materials, and in particular to a flexible infrared stealth phase change material and its preparation and application. Background Art

[0002] The continuous improvement of the intelligence and accuracy of detection equipment has put higher and higher requirements on the stealth of military targets. Improving the stealth ability of targets has always been an important focus of researchers. According to the Stefan-Boltzmann law, the infrared radiation energy of an object is determined by the infrared emissivity and temperature. Therefore, reducing the infrared emissivity and temperature of the target is the basic way to achieve infrared stealth.

[0003] Phase change materials can absorb / release a large amount of latent heat and keep the temperature relatively constant during the phase change process. Based on this, they can be used as infrared stealth materials to absorb the heat generated by the target and control its temperature, thereby achieving the effect of infrared stealth. As a highly potential temperature-controlled infrared stealth material, the research on phase change materials has received more and more attention. However, this type of material has the problem of leakage during phase change, so the phase change material is often loaded into a carrier material to prepare a composite shaped phase change material so that it remains stable during the phase change process. However, in this process, the prepared composite shaped phase change material often has rigidity, which reduces its operability and makes it difficult to meet the application of many practical scenarios. Therefore, the preparation of flexible composite shaped phase change materials has important practical value. At the same time, the phase change system often has a high saturation of organic functional groups, so the infrared emissivity is high, so its infrared stealth effect is still limited. If its infrared emissivity can be effectively reduced, its infrared stealth effect will be further improved. Summary of the invention

[0004] In view of the shortcomings of inherent rigidity, phase change leakage and high infrared emissivity of phase change materials, the present invention proposes a flexible infrared stealth phase change material and its preparation and application.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] In a first aspect, the present invention provides a method for preparing a flexible infrared stealth phase change material, comprising the following process steps:

[0007] (1) mixing a polymer and an organic solvent in proportion to obtain a transparent solution, wherein the mass fraction of the polymer is 3-15 wt %; then adding low infrared radiation metal particles and stirring to obtain a mixed solution, wherein the mass ratio of the polymer to the low infrared radiation metal particles is 4-10; scraping the mixed solution onto a substrate to form a uniform layer of a certain thickness, placing it in water for displacement at room temperature, and then freeze-drying it to obtain a flexible carrier;

[0008] (2) Mixing the phase change material with the flexible carrier in step (1), vacuum impregnating the phase change material so that it fully enters the substrate structure, and finally removing excess phase change material on the surface to obtain a flexible infrared stealth phase change material.

[0009] Preferably, the mass fraction of the high molecular weight polymer in step (1) is 5-10wt%, and optimally 8wt%.

[0010] Preferably, in step (1), the mass ratio of the high molecular weight polymer to the low infrared radiation metal particles is 8, at which point the infrared radiation rate is optimal.

[0011] Preferably, the low infrared radiation metal particles in step (1) are one or more of gold, silver, aluminum and copper; and the average particle size is 300-800 nm.

[0012] More preferably, the average particle size of the low infrared radiation metal particles in step (1) is 500 nm, at which point the distribution effect is optimal.

[0013] Preferably, the high molecular polymer in step (1) is one or more of cellulose acetate, polyvinylidene fluoride, polyether sulfone, polyvinylidene fluoride-hexafluoropropylene copolymer, and polyvinyl alcohol; and the organic solvent is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, acetone, N-methylpyrrolidone, and dimethyl sulfoxide.

[0014] Preferably, the solution is coated with a thickness of 500-600 μm in step (1), at which point the composite membrane has the best energy storage effect.

[0015] Preferably, the time for replacement in water in step (1) is 2-3 hours, and the best effect is achieved when the time is 3 hours.

[0016] Preferably, the freeze-drying temperature in step (1) is -20°C-10°C, and the time is 48-60h.

[0017] More preferably, the freeze-drying temperature in step (1) is -15°C-10°C and the time is 48-55h, at which time the freeze-drying effect is best.

[0018] Preferably, the phase change material in step (2) is one or more of paraffin, polyethylene glycol (molecular weight 1000-20000), fatty alcohol (carbon number 14-18), fatty acid (carbon number 14-18);

[0019] Preferably, the temperature during the vacuum impregnation in step (2) is 80-110° C., the vacuum degree is -0.1 MPa, and the time is 2-4 hours.

[0020] In a second aspect, the present invention provides a flexible infrared stealth phase change material prepared by the above preparation method.

[0021] The flexible phase change material prepared by the invention has good flexibility and can be bent over 180 degrees while still maintaining its shape without breaking. The infrared radiation rate of the flexible phase change material prepared can be reduced to 0.2-0.7.

[0022] In a third aspect, the present invention provides an application of the above-mentioned flexible infrared stealth phase change material, and the phase change material product can be used in the field of wearable infrared stealth intelligent equipment.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The reaction conditions designed in the present invention have low requirements for preparation conditions and equipment, and are easy to operate. The prepared composite shaped phase change material has good heat storage performance, flexibility and shape stability (no leakage), and can be bent over 180° and still maintain its shape without breaking;

[0025] 2. The infrared emissivity of the phase change material prepared by the present invention can be effectively reduced to 0.2-0.7, so efficient infrared stealth can be achieved through dual approaches of lowering the target temperature and reducing infrared radiation. The system can be applied to the field of wearable infrared stealth intelligent equipment. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a physical picture of the flexible infrared stealth phase change material prepared in Example 1 of the present invention.

[0027] Figure 2 This is a differential scanning calorimetry curve of the flexible infrared stealth phase change material prepared in Example 2 of the present invention.

[0028] Figure 3 This is an infrared reflectivity spectrum of the flexible infrared stealth phase change material prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0029] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0030] Example 1

[0031] (1) Weigh 0.5 g of polyvinylidene fluoride and 9.5 g of N,N-dimethylformamide and mix them for 1 h to obtain a transparent solution; then weigh 0.1 g of aluminum particles (average diameter 500 nm) and add them to the transparent solution and stir for 2.5 h to obtain a mixed solution. The liquid was scraped onto a glass plate to a thickness of 600 μm, the solvent was replaced in a water bath for 3 h, and freeze-dried at -10°C for 55 h to obtain a flexible carrier;

[0032] (2) The flexible carrier and polyethylene glycol (molecular weight 6000) were placed in a vacuum oven and immersed for 3 h at a vacuum degree of -0.1 MPa and a temperature of 80°C. Finally, the excess phase change material on the surface was removed to obtain a flexible infrared stealth phase change material.

[0033] The melting enthalpy of the flexible infrared stealth phase change material prepared by the present invention is about 110 J·g -1 , indicating that the material has a high heat storage density; the infrared emissivity of the material can be reduced to about 0.6, indicating that the material has a low infrared emissivity; and the material can be bent about 180 degrees without breaking, indicating that the material has good flexibility and shape stability (no leakage), as shown in the actual picture Figure 1 shown.

[0034] Example 2

[0035] (1) Weigh 0.8 g of polyvinylidene fluoride-hexafluoropropylene copolymer and 9.2 g of N,N-dimethylacetamide and mix and stir for 1 h to obtain a transparent solution; then weigh 0.2 g of silver particles (average diameter 300 nm) and add them to the transparent solution and stir for 2 h to obtain a mixed solution. The liquid is scraped onto a glass plate to a thickness of 500 μm, the solvent is replaced in a water bath for 3 h, and freeze-dried at -10°C for 50 h to obtain a flexible carrier;

[0036] (2) The carrier and paraffin are placed in a vacuum oven and immersed for 3 hours at a vacuum degree of -0.1 MPa and a temperature of 80°C. Finally, the excess phase change material on the surface is removed to obtain a flexible infrared stealth phase change material.

[0037] The melting enthalpy of the flexible infrared stealth phase change material prepared by the present invention is about 100 J·g -1 The differential scanning calorimetry curve is as follows Figure 2 As shown, it indicates that the material has a higher heat storage density; the infrared emissivity of the material can be reduced to about 0.4, indicating that the material has low infrared radiation rate; and the material can be bent about 180 degrees without breaking, indicating that the material has good flexibility and shape stability (no leakage).

[0038] Example 3

[0039] (1) Weigh 1 g of cellulose acetate and 9 g of N-methylpyrrolidoneamine and mix and stir for 1 h to obtain a transparent solution; then weigh 0.1 g of copper particles (average diameter 800 nm) and add them to the transparent solution and stir for 2 h to obtain a mixed solution. The liquid is scraped onto a glass plate to a thickness of 500 μm, the solvent is replaced in a water bath for 3 h, and freeze-dried at -10°C for 48 h onto a flexible carrier;

[0040] (2) The above-mentioned carrier and tetradecanoic acid are placed in a vacuum oven together, and immersed for 3 hours under the conditions of vacuum degree -0.1 MPa and temperature 80°C. Finally, the excess phase change material on the surface is removed to obtain a flexible infrared stealth phase change material.

[0041] The melting enthalpy of the flexible infrared stealth phase change material prepared by the present invention is about 120 J·g -1 , indicating that the material has a high heat storage density; the infrared emissivity of the material can be reduced to about 0.7, and its infrared reflectivity spectrum is shown in Figure 3 As shown, it indicates that the material has low infrared emissivity; and the material can be bent about 180 degrees without breaking, indicating that the material has good flexibility and shape stability (no leakage).

[0042] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a flexible infrared stealth phase change material, characterized in that: The process steps include: (1) mixing a polymer and an organic solvent in proportion to obtain a transparent solution, wherein the mass fraction of the polymer is 3-15 wt %; then adding low infrared radiation metal particles and stirring to obtain a mixed solution, wherein the mass ratio of the polymer to the low infrared radiation metal particles is 4-10; scraping the mixed solution onto a substrate to form a uniform layer of a certain thickness, placing it in water for displacement at room temperature, and then freeze-drying it to obtain a flexible carrier; (2) Mixing the phase change material with the flexible carrier in step (1), vacuum impregnating the phase change material so that it fully enters the substrate structure, and finally removing excess phase change material on the surface to obtain a flexible infrared stealth phase change material.

2. The method for preparing a flexible infrared stealth phase change material according to claim 1, characterized in that: The mass fraction of the high molecular weight polymer in step (1) is 5-10wt%; The mass ratio of the high molecular polymer to the low infrared radiation metal particles is 8; The low infrared radiation metal particles are one or more of gold, silver, aluminum and copper; and the average particle size is 300-800nm.

3. The method for preparing a flexible infrared stealth phase change material according to claim 1, characterized in that: The high molecular polymer in step (1) is one or more of cellulose acetate, polyvinylidene fluoride, polyether sulfone, polyvinylidene fluoride-hexafluoropropylene copolymer, and polyvinyl alcohol; The organic solvent is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, acetone, N-methylpyrrolidone and dimethyl sulfoxide.

4. The method for preparing a flexible infrared stealth phase change material according to claim 1, characterized in that: The thickness of the solution applied by scraping in step (1) is 500-600 μm.

5. The method for preparing a flexible infrared stealth phase change material according to claim 1, characterized in that: The freeze-drying temperature in step (1) is -20°C-10°C, and the time is 48-60h.

6. The method for preparing a flexible infrared stealth phase change material according to claim 5, characterized in that: The freeze-drying temperature in step (1) is -15°C-10°C and the time is 48-55h.

7. The method for preparing a flexible infrared stealth phase change material according to claim 1, characterized in that: The phase change material in step (2) is one or more of paraffin, polyethylene glycol with a molecular weight of 1000-20000, fatty alcohol with a carbon number of 14-18, and fatty acid with a carbon number of 14-18.

8. The method for preparing a flexible infrared stealth phase change material according to claim 1, characterized in that: The vacuum impregnation temperature in step (2) is 80-110° C., the vacuum degree is -0.1 MPa, and the time is 2-4 hours.

9. A flexible phase change material obtained by the preparation method according to any one of claims 1 to 8.

10. An application of the flexible phase change material according to claim 9 in the field of wearable infrared stealth intelligent equipment.

Citation Information

Patent Citations

  • Preparation method of radar wave absorption composite material with infrared stealth

    CN111286079A

  • Infrared stealth material taking leather as base material, and preparation method thereof

    CN111286562A

  • Infrared stealth polyformaldehyde powder coating based on low-emissivity phase change microcapsules and preparation method

    CN115722160A

  • Infrared stealth and wave transmission integrated metamaterial coating and preparation method thereof

    CN117567782A

  • Flexible vanadium dioxide film and preparation method and application thereof

    CN117987086A

Cited By

  • Integrated ordered structure material as well as preparation method and application thereof

    CN119758490A