Intumescent halogen-free flame retardant and application thereof
By using an expanded halogen-free flame retardant composed of melamine cyanurate, diethyl aluminum hypophosphate and red phosphorus, the problems of degradation of flammability and mechanical properties of ethylene propylene rubber are solved, and efficient Flame retardant modification meets application needs in the fields of wires, cables and automobiles.
Patent Information
- Application Number
- CN202410997495.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-19
AI Technical Summary
The existing ethylene propylene ternary rubber has a low oxygen index and is flammable. The existing flame retardants such as bromine antimony and hydroxide flame retardants will produce toxic substances or cause the mechanical properties of the materials to decline, and the flame retardant efficiency will be Low, it is difficult to meet the requirements of FV-0 flame retardant level.
The expanded halogen-free flame retardant consisting of melamine cyanurate, diethyl aluminum hypophosphate and coated red phosphorus are used to improve flame retardant efficiency by preferably coating the phosphorus content and coating material of the red phosphorus, and Combined with melamine formaldehyde resin, red phosphorus is coated with red phosphorus to improve mechanical properties and dispersion effect, and ethylene propylene ternary rubber with excellent flame retardant properties was prepared.
It has achieved low usage and good flame retardant performance of EPDM rubber, excellent mechanical properties, can meet the application requirements of wires, cables and automobiles, and maintains the elongation and tear of the material during the flame retardant modification process. Cracking strength.
Smart Images

Figure BDA0004960652090000031 
Figure BDA0004960652090000041 
Figure BDA0004960652090000042
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flame retardants, and in particular to an intumescent halogen-free flame retardant and application thereof. Background Art
[0002] Ethylene propylene diene monomer (EPDM) is widely used in wires, cables, seals, auto parts, etc. due to its good weather resistance, electrical insulation, ozone resistance and other properties. However, the oxygen index of EPDM is only about 19%, which is flammable. In order to ensure its safe application, it often needs to be flame-retardant modified.
[0003] At present, the flame retardants for commercial EPDM are mainly bromine antimony flame retardants and hydroxide flame retardants. Bromine antimony flame retardants will produce toxic and harmful substances to the human body and the environment during combustion; hydroxide flame retardants have low flame retardant efficiency, and when EPDM reaches the FV-0 flame retardant level, there is a problem of large usage, which seriously damages the mechanical properties of the material such as elongation at break. CN106967230A discloses an intumescent halogen-free flame retardant, containing melamine cyanurate and aluminum diethylphosphinate and / or aluminum hydroxide mixed with each other. Melamine cyanurate and aluminum diethylphosphinate cooperate with each other to improve the flame retardant properties of the material, but there are still problems such as large usage of flame retardant and decrease in mechanical properties of the material caused by flame retardant. Summary of the invention
[0004] The present invention aims to solve at least one of the above-mentioned technical problems existing in the prior art. To this end, one of the purposes of the present invention is to provide an intumescent halogen-free flame retardant; the second purpose of the present invention is to provide an EPDM rubber; the third purpose of the present invention is to provide a method for preparing the EPDM rubber; the fourth purpose of the present invention is to provide an application of the EPDM rubber.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] The first aspect of the present invention provides an intumescent halogen-free flame retardant, which comprises the following components by weight: 30 to 80 parts of melamine cyanurate, 15 to 45 parts of diethyl aluminum hypophosphite, and 5 to 40 parts of coated red phosphorus.
[0007] Preferably, the intumescent halogen-free flame retardant is composed of the following components in parts by mass: 50 to 65 parts of melamine cyanurate (MCA), 20 to 30 parts of diethyl aluminum hypophosphite (ADP), and 10 to 20 parts of coated red phosphorus.
[0008] Preferably, the phosphorus content of the coated red phosphorus is 70-80wt%.
[0009] Specifically, the phosphorus content of the coated red phosphorus will affect the flame retardant efficiency, so choosing coated red phosphorus with a higher phosphorus content is beneficial to improving the flame retardant efficiency and reducing the amount of flame retardant used.
[0010] Preferably, the coated red phosphorus includes at least one of melamine formaldehyde resin coated red phosphorus and phenolic resin coated red phosphorus; further preferably, the coated red phosphorus is melamine formaldehyde resin coated red phosphorus.
[0011] Specifically, the coating material has a diluting effect on the phosphorus content of the coated red phosphorus and has a great influence on the flame retardant properties; and different coating materials have different compatibilities with polymer materials, and the coating effects on red phosphorus will also be different, so the coating material will affect the dispersion effect of the coated red phosphorus in the polymer. Therefore, melamine formaldehyde resin with good compatibility with the polymer is preferably used as the coating layer; in addition, melamine formaldehyde resin coated red phosphorus is a smooth powder, which can not only improve the mechanical properties of the material, but also act as a lubricant to improve the appearance of the material.
[0012] The second aspect of the present invention provides an EPDM rubber, comprising the following preparation raw materials: the intumescent halogen-free flame retardant described in the first aspect of the present invention, EPDM rubber raw rubber, and additives.
[0013] Preferably, the mass ratio of the intumescent halogen-free flame retardant, EPDM rubber and additive is (40-120):100:(70-98); further preferably, the mass ratio of the intumescent halogen-free flame retardant, EPDM rubber and additive is (80-95):100:(73-97.5).
[0014] Preferably, the Mooney viscosity of the EPDM raw rubber is 20-100.
[0015] Preferably, the EPDM raw rubber is obtained by copolymerizing the following raw materials in percentage by mass: 45-80% ethylene, 10-50% propylene, and 1-10% a third monomer.
[0016] Preferably, the third monomer includes at least one of ethylidene norbornene (ENB), 1,4-hexadiene (1,4-HD), and dicyclopentadiene (DCDP).
[0017] Preferably, the additives include the following components: zinc oxide, stearic acid, carbon black, paraffin oil, vulcanizing agent, and vulcanization accelerator.
[0018] Preferably, the vulcanizing agent includes at least one of sulfur, peroxide, and resin vulcanization system.
[0019] Preferably, the vulcanization accelerator includes at least one of dibenzothiazyl disulfide (DM), N-cyclohexyl-2-benzothiazole sulfenamide (CZ), thiocarbamoyl sulfenamide, and sulfur phosphoryl accelerator; further preferably, the vulcanization accelerator is a compound of dibenzothiazyl disulfide and N-cyclohexyl-2-benzothiazole sulfenamide, and the mass ratio of dibenzothiazyl disulfide to N-cyclohexyl-2-benzothiazole sulfenamide is 1:(1 to 1.5).
[0020] Preferably, the additive comprises the following components in parts by mass: 2 to 8 parts of zinc oxide, 0.5 to 3 parts of stearic acid, 35 to 40 parts of carbon black, 30 to 40 parts of paraffin oil, 1 to 4 parts of vulcanizing agent, and 1.5 to 3 parts of vulcanization accelerator; further preferably, the additive comprises the following components in parts by mass: 2 to 8 parts of zinc oxide, 0.5 to 2.5 parts of stearic acid, 38 to 40 parts of carbon black, 30 to 40 parts of paraffin oil, 1 to 4 parts of vulcanizing agent, and 1.5 to 3 parts of vulcanization accelerator.
[0021] In some embodiments of the present invention, the oxygen index of the EPDM rubber is 25-35%.
[0022] In some embodiments of the present invention, the Shore A hardness of the EPDM rubber is 80-85.
[0023] In some embodiments of the present invention, the elongation at break of the EPDM rubber is 340-355%.
[0024] In some embodiments of the present invention, the tear strength of the EPDM rubber is 24-26 kN / m.
[0025] The third aspect of the present invention provides a method for preparing the EPDM rubber according to the second aspect of the present invention, comprising the following steps:
[0026] The intumescent halogen-free flame retardant, EPDM rubber and additives are mixed and vulcanized to obtain the EPDM rubber.
[0027] Preferably, the preparation method specifically comprises the following steps:
[0028] The EPDM raw rubber is thinned on an open mill for 4 to 6 times, and after rolling, the roller distance is adjusted to 0.5 to 1 mm, zinc oxide, stearic acid, carbon black, paraffin oil and intumescent halogen-free flame retardant are added, and mixed for 15 to 20 minutes, and a vulcanizing agent and a vulcanization accelerator are added. The rubber is mixed evenly, triangularly wrapped for 6 to 10 times, rolled for 6 to 8 times, and then produced into a sheet, which is vulcanized at 160° C.×12 minutes to obtain the EPDM rubber.
[0029] The fourth aspect of the present invention provides the use of the EPDM rubber described in the second aspect of the present invention in the fields of wires, cables and automobiles.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] 1) The intumescent halogen-free flame retardant provided by the present invention has a small dosage and little effect on the mechanical properties of the material;
[0032] 2) The EPDM rubber provided by the present invention contains an intumescent halogen-free flame retardant, has good flame retardancy, excellent mechanical properties, and can meet the application requirements in the fields of wires, cables, and automobiles;
[0033] 3) The method for preparing EPDM rubber provided by the present invention has simple steps and mild process conditions and is suitable for industrial application. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a sample photo of EPDM rubber in Example 1. DETAILED DESCRIPTION
[0035] The present invention is further described in detail below by specific examples. Unless otherwise specified, the raw materials, reagents or devices used in the examples and comparative examples can be obtained from conventional commercial sources or can be obtained by prior art methods. Unless otherwise specified, the experiments or test methods are conventional methods in the art.
[0036] The specific information of the raw materials used in the following examples and comparative examples is shown in Table 1 below:
[0037] Table 1 Raw material information table in Examples and Comparative Examples
[0038]
[0039]
[0040] Unless otherwise specified, "parts" in the following examples and comparative examples refer to "parts by mass".
[0041] Example 1
[0042] This embodiment provides an intumescent halogen-free flame retardant and an EPDM rubber. The intumescent halogen-free flame retardant is composed of 50 parts of melamine cyanurate, 25 parts of diethyl aluminum hypophosphite and 5 parts of melamine formaldehyde resin coated red phosphorus. The raw materials and contents of the EPDM rubber are shown in Table 2:
[0043] Table 2 Preparation raw materials and content of EPDM rubber in Example 1
[0044]
[0045]
[0046] EPDM rubber is prepared by the following steps:
[0047] The EPDM raw rubber was thinned on an open mixing mill for 5 times, and after being rolled, the roller distance was adjusted to 1 mm, zinc oxide, stearic acid, carbon black, paraffin oil and intumescent halogen-free flame retardant were added, and mixed for 15 minutes, sulfur, dibenzothiazyl disulfide and N-cyclohexyl-2-benzothiazolesulfenamide were added, mixed evenly, triangularly wrapped 6 times, and rolled 6 times before being produced into sheets, which were vulcanized at 160°C × 12 minutes to obtain EPDM rubber.
[0048] Example 2
[0049] This embodiment provides an intumescent halogen-free flame retardant and an EPDM rubber. The intumescent halogen-free flame retardant is composed of 50 parts of melamine cyanurate, 20 parts of diethyl aluminum hypophosphite and 10 parts of melamine formaldehyde resin coated red phosphorus. The raw materials and contents of the EPDM rubber are shown in Table 3:
[0050] Table 3 Preparation raw materials and content of EPDM rubber in Example 2
[0051]
[0052] EPDM rubber is prepared by the following steps:
[0053] The EPDM raw rubber is thinned on an open mixing mill for 4 to 6 times, and after being rolled, the roller distance is adjusted to 0.5 to 1 mm, zinc oxide, stearic acid, carbon black, paraffin oil and intumescent halogen-free flame retardant are added, and mixed for 15 to 20 minutes, sulfur, dibenzothiazole disulfide and N-cyclohexyl-2-benzothiazolesulfenamide are added, and mixed evenly, and triangularly wrapped for 6 to 10 times, rolled for 6 to 8 times, and then sheets are produced, and vulcanized at 160°C × 12 minutes to obtain EPDM rubber.
[0054] Example 3
[0055] This embodiment provides an intumescent halogen-free flame retardant and an EPDM rubber. The intumescent halogen-free flame retardant is composed of 50 parts of melamine cyanurate, 15 parts of diethyl aluminum hypophosphite and 15 parts of melamine formaldehyde resin-coated red phosphorus. The raw materials and contents of the EPDM rubber are shown in Table 2:
[0056] Table 4 Preparation raw materials and content of EPDM rubber in Example 3
[0057]
[0058] EPDM rubber is prepared by the following steps:
[0059] The EPDM raw rubber is thinned on an open mixing mill for 4 to 6 times, and after being rolled, the roller distance is adjusted to 0.5 to 1 mm, zinc oxide, stearic acid, carbon black, paraffin oil and intumescent halogen-free flame retardant are added, and mixed for 15 to 20 minutes, sulfur, dibenzothiazole disulfide and N-cyclohexyl-2-benzothiazolesulfenamide are added, and mixed evenly, and triangularly wrapped for 6 to 10 times, rolled for 6 to 8 times, and then sheets are produced, and vulcanized at 160°C × 12 minutes to obtain EPDM rubber.
[0060] Comparative Example 1
[0061] This comparative example provides an EPDM rubber, which is different from Example 1 in that aluminum hydroxide is used instead of the intumescent halogen-free flame retardant. The raw materials and contents of the EPDM rubber are shown in Table 5:
[0062] Table 5 Preparation raw materials and content of EPDM rubber in comparative example 1
[0063]
[0064]
[0065] EPDM rubber is prepared by the following steps:
[0066] The EPDM raw rubber is thinned on an open mixing mill for 4 to 6 times, and after rolling, the roller distance is adjusted to 0.5 to 1 mm, zinc oxide, stearic acid, carbon black, paraffin oil and aluminum hydroxide are added, and mixed for 15 to 20 minutes, sulfur, dibenzothiazole disulfide and N-cyclohexyl-2-benzothiazolesulfenamide are added, and mixed evenly, triangle wrapped for 6 to 10 times, rolled for 6 to 8 times, and then the sheet is produced, and vulcanized at 160°C × 12 minutes to obtain the EPDM rubber.
[0067] Comparative Example 2
[0068] This comparative example provides an EPDM rubber, which is different from Example 1 in that aluminum hydroxide is used to replace the intumescent halogen-free flame retardant and the amount of the flame retardant is increased. The raw materials and contents of the EPDM rubber are shown in Table 6:
[0069] Table 6 Preparation raw materials and content of EPDM rubber in comparative example 2
[0070]
[0071] EPDM rubber is prepared by the following steps:
[0072] The EPDM raw rubber is thinned on an open mixing mill for 4 to 6 times, and after rolling, the roller distance is adjusted to 0.5 to 1 mm, zinc oxide, stearic acid, carbon black, paraffin oil and aluminum hydroxide are added, and mixed for 15 to 20 minutes, sulfur, dibenzothiazole disulfide and N-cyclohexyl-2-benzothiazolesulfenamide are added, and mixed evenly, triangle wrapped for 6 to 10 times, rolled for 6 to 8 times, and then the sheet is produced, and vulcanized at 160°C × 12 minutes to obtain the EPDM rubber.
[0073] Comparative Example 3
[0074] This comparative example provides an EPDM rubber, which is different from Example 1 in that a flame retardant composed of 50 parts of melamine cyanurate and 30 parts of diethyl aluminum hypophosphite is used, and the flame retardant does not contain coated red phosphorus. The raw materials and contents of the EPDM rubber are shown in Table 7:
[0075] Table 7 Preparation raw materials and content of EPDM rubber in comparative example 3
[0076]
[0077] EPDM rubber is prepared by the following steps:
[0078] The EPDM raw rubber is thinned on an open mixing mill for 4 to 6 times, and after being rolled, the roller distance is adjusted to 0.5 to 1 mm, zinc oxide, stearic acid, carbon black, paraffin oil, melamine cyanurate and diethyl aluminum hypophosphite are added, and mixed for 15 to 20 minutes, sulfur, dibenzothiazole disulfide and N-cyclohexyl-2-benzothiazolesulfenamide are added, and mixed evenly, triangle wrapped for 6 to 10 times, rolled for 6 to 8 times, and then sheets are produced, and vulcanized at 160°C × 12 minutes to obtain EPDM rubber.
[0079] Comparative Example 4
[0080] This comparative example provides an EPDM rubber, which is different from Example 1 in that no flame retardant is added. The raw materials and contents of the EPDM rubber are shown in Table 8:
[0081] Table 8 Preparation raw materials and content of EPDM rubber in comparative example 4
[0082]
[0083] EPDM rubber is prepared by the following steps:
[0084] The EPDM raw rubber is thinned on an open mixing mill for 4 to 6 times, and after rolling, the roller distance is adjusted to 0.5 to 1 mm, zinc oxide, stearic acid, carbon black and paraffin oil are added, and mixed for 15 to 20 minutes, sulfur, dibenzothiazole disulfide and N-cyclohexyl-2-benzothiazolesulfenamide are added, and mixed evenly, triangle wrapped for 6 to 10 times, rolled for 6 to 8 times, and then sheets are produced, and vulcanized at 160°C × 12 minutes to obtain EPDM rubber.
[0085] Performance Testing
[0086] The EPDM rubbers in Examples 1-3 and Comparative Examples 1-4 were tested as follows:
[0087] 1) Vertical burning time and flame retardant level: Tested according to GB / T 2408-1996, sample size is 125mm×12.5mm×1.6mm;
[0088] 2) Oxygen index: Tested according to GB / T2406-1993, sample size 85mm×10mm×3.2mm;
[0089] 3) Shore A hardness: Tested in accordance with GB / T531-1992;
[0090] 4) Elongation at break and tear strength: tested according to method GB / T528-1998, with a tensile rate of 500 mm / min.
[0091] The performance test results of the EPDM rubber in Examples 1-3 and Comparative Examples 1-4 are shown in Table 9 below:
[0092] Table 9 Performance test results of EPDM rubber in Examples 1-3 and Comparative Examples 1-4
[0093]
[0094] Table 9 shows the performance test results of EPDM rubber in Examples 1-3 and Comparative Examples 1-4. It can be seen from Table 9 that after adding the intumescent halogen-free flame retardant composed of melamine cyanurate, diethyl aluminum hypophosphite and coated red phosphorus in Examples 1-3, the vertical burning time of the EPDM rubber sample is 3 to 5s, the oxygen index is greater than or equal to 28%, the flame retardant level can reach FV-0 grade, and the flame retardant performance is excellent; the Shore A hardness of the EPDM rubber sample can reach more than 82, and the hardness is relatively high; the elongation at break of the EPDM rubber sample is greater than or equal to 340%, the tear strength is greater than or equal to 24.5kN / m, and the mechanical properties are good. Compared with the performance of EPDM rubber in Comparative Example 4 when no flame retardant is added, the intumescent halogen-free flame retardant improves the flame retardant performance without causing a significant decline in the mechanical properties of the material. Figure 1 is a sample photo of EPDM rubber in Example 1, Figure 1 It can be seen that after using the coated red phosphorus, the EPDM rubber sample is black and has a smooth surface, which solves the problem that the purple-red color of red phosphorus itself easily affects the color of the material. It can be seen that the use of the intumescent halogen-free flame retardant provided by the present invention can not only make the EPDM rubber have better flame retardant properties, but also ensure that the mechanical properties of the EPDM rubber are not affected, so that it can be better used in the fields of wires, cables and automobiles.
[0095] In Comparative Examples 1 and 2, the use of traditional aluminum hydroxide flame retardant, when the same amount as the intumescent halogen-free flame retardant, can not achieve the purpose of improving the flame retardant performance, and the hardness, elongation at break and tear strength of EPDM rubber are affected, and the mechanical properties deteriorate; when the amount of aluminum hydroxide flame retardant is increased to 1.5 times the amount of intumescent halogen-free flame retardant, the flame retardancy of EPDM rubber is improved, but still not as good as Examples 1-3, and the mechanical properties of the material are seriously deteriorated. In Comparative Example 3, a flame retardant composed of melamine cyanurate and diethyl aluminum hypophosphite is used. When the amount is the same as in Example 1, the flame retardant performance improvement effect is not ideal. It can be seen that the intumescent halogen-free flame retardant composed of melamine cyanurate, diethyl aluminum hypophosphite and coated red phosphorus can achieve a better flame retardant performance improvement effect with a smaller amount.
[0096] The intumescent halogen-free flame retardant provided by the present invention includes melamine cyanurate, diethyl aluminum hypophosphite and red phosphorus. The composite use of the three can improve the flame retardant performance of EPDM rubber with a small amount of addition, while ensuring that its mechanical properties are not seriously affected. The EPDM rubber with the intumescent halogen-free flame retardant added has good flame retardancy and mechanical properties, excellent overall performance, and can meet the application requirements in the fields of wires, cables, and automobiles.
Claims
1. An intumescent halogen-free flame retardant, characterized in that: The invention comprises the following components by weight: 30 to 80 parts of melamine cyanurate, 15 to 45 parts of diethyl aluminum hypophosphite, and 5 to 40 parts of coated red phosphorus.
2. The intumescent halogen-free flame retardant according to claim 1, characterized in that: The phosphorus content of the coated red phosphorus is 70-80wt%.
3. The intumescent halogen-free flame retardant according to claim 1, characterized in that: The coated red phosphorus includes at least one of melamine formaldehyde resin coated red phosphorus and phenolic resin coated red phosphorus.
4. An EPDM rubber, characterized in that: The preparation method comprises the following raw materials: the intumescent halogen-free flame retardant according to any one of claims 1 to 3, EPDM raw rubber, and additives.
5. The EPDM rubber according to claim 4, characterized in that: The mass ratio of the intumescent halogen-free flame retardant, the EPDM rubber raw rubber and the additive is (40-120):100:(70-98).
6. The EPDM rubber according to claim 4, characterized in that: The EPDM raw rubber is obtained by copolymerizing the following raw materials in percentage by mass: 45-80% ethylene, 10-50% propylene, and 1-10% a third monomer; Preferably, the third monomer includes at least one of ethylidene norbornene, 1,4-hexadiene, and dicyclopentadiene.
7. The EPDM rubber according to claim 4, characterized in that: The additives include the following components: zinc oxide, stearic acid, carbon black, paraffin oil, vulcanizing agent and vulcanization accelerator.
8. The EPDM rubber according to claim 7, characterized in that: The additive comprises the following components in parts by mass: 2 to 8 parts of zinc oxide, 0.5 to 3 parts of stearic acid, 35 to 40 parts of carbon black, 30 to 40 parts of paraffin oil, 1 to 4 parts of vulcanizing agent, and 1.5 to 3 parts of vulcanization accelerator.
9. The method for preparing the EPDM rubber according to any one of claims 4 to 8, characterized in that: The following steps are involved: The intumescent halogen-free flame retardant, EPDM rubber and additives are mixed and vulcanized to obtain the EPDM rubber.
10. Use of the EPDM rubber according to any one of claims 4 to 8 in the fields of wires, cables and automobiles.