Inner-layer matrix resin for cold-drawn sleeve packaging film, preparation method of inner-layer matrix resin and cold-drawn sleeve packaging film
By using vaterite-type calcium carbonate and activated dispersed components in the inner matrix resin of the cold stretched casing packaging film, the problems of high dynamic friction coefficient and high cost of the inner layer are solved, and a low-cost and low-oil-absorbing packaging film is achieved. Preparation improves packaging effect and environmental protection performance.
Patent Information
- Application Number
- CN202411455528.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-18
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The inner layer of the existing cold stretch casing packaging film has a high dynamic friction coefficient, high cost, and difficult to disperse functional agents, which affects the packaging effect and environmental protection performance.
Using vaterite calcium carbonate as the component of the inner matrix resin, the inner layer dynamic friction coefficient is reduced by mixing with activated dispersing components and dispersant, and a low-cost, low-oil absorption predispersion is prepared through extrusion granulation process. Masterbatch forms an efficient inner matrix resin.
It significantly reduces the dynamic friction coefficient of the inner layer of the cold stretched sleeve film, improves the smooth opening function, reduces the cost of raw materials, is suitable for environmentally friendly packaging, and does not affect the mechanical properties of the film.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyolefin film materials, and in particular to an inner layer matrix resin for a cold-stretch sleeve packaging film and a preparation method thereof, and a cold-stretch sleeve packaging film. Background Art
[0002] Cold stretch sleeve packaging film is mainly used for secondary container packaging of logistics and transportation products. Usually, the goods are stacked on pallets and then fixed with cold stretch sleeve packaging film to prevent the loosening of goods during handling, transportation and storage and the pollution of dust during storage. It also has a certain rainproof function. Cold stretch sleeve packaging film is mainly produced by a three-layer composite blown film method, and the main raw materials are metallocene linear low-density polyethylene (mLLDPE) and linear low-density polyethylene (LLDPE) blends. In order to meet the needs of low-cost packaging and environmentally friendly packaging process, people pay more attention to energy and material consumption, and require the inner film of cold stretch sleeve packaging film to have a smaller dynamic friction coefficient. Related technology In order to reduce the dynamic friction coefficient of the inner layer of cold stretch sleeve packaging film, erucic acid amide and silica-type open slippery functional agents are mainly added to the inner film. These substances are relatively expensive, and the migration speed of erucic acid amide is slow and the initial effect is poor. The silica-type open slippery functional agent has a high oil absorption value and is difficult to disperse, and there are different problems. Summary of the invention
[0003] In view of this, the object of the present invention is to provide an inner layer matrix resin for a cold stretch sleeve packaging film, a preparation method thereof, and a cold stretch sleeve packaging film. The inner layer matrix resin for the cold stretch sleeve packaging film of the present invention adds vaterite-type calcium carbonate to substantially reduce the dynamic friction coefficient of the inner layer of the cold stretch sleeve film, and has low cost, low oil absorption value, and is easy to disperse.
[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions: The present invention provides an inner layer matrix resin for a cold stretch sleeve packaging film, comprising the following components in parts by mass: 20 to 24 parts of metallocene linear low-density polyethylene, 75 parts of hexene copolymer LLDPE and 1 to 5 parts of a pre-dispersed masterbatch; The pre-dispersed masterbatch comprises the following components in percentage by mass: 70% of vaterite calcium carbonate, 0.5-1.5% of activated dispersing component and the balance of metallocene linear low-density polyethylene native polymer powder (mLLDPE native polymer powder).
[0005] Preferably, the fineness of the vaterite calcium carbonate is 600-1200 mesh.
[0006] Preferably, the activated dispersing component is a complex of ethylene-vinyl acetate copolymer wax and calcium stearate.
[0007] Preferably, the mass ratio of ethylene-vinyl acetate copolymer wax to calcium stearate in the activated dispersing component is 5:1 to 1:5.
[0008] Preferably, the weight average molecular weight of the ethylene-vinyl acetate copolymer wax is 500-1500.
[0009] Preferably, the melt flow rate of the metallocene linear low-density polyethylene raw polymer powder is 2.5-4.5 g / 10 min, and the density is 0.918-0.922 g / cm 3 , the average particle size is 50~300μm.
[0010] The present invention also provides a method for preparing the inner layer matrix resin for the cold stretch sleeve packaging film described in the above technical solution, comprising the following steps: Mixing vaterite calcium carbonate, an activated dispersing component and a dispersant to obtain a slurry; The slurry is mixed with metallocene linear low-density polyethylene raw polymer powder and extruded and granulated to obtain a pre-dispersed masterbatch; The pre-dispersed masterbatch, metallocene linear low-density polyethylene and hexene copolymer LLDPE are mixed to obtain the inner layer matrix resin for the cold stretch sleeve packaging film.
[0011] The present invention also provides a cold-stretch sleeve packaging film, comprising an outer matrix resin layer, a middle matrix resin layer and an inner matrix resin layer stacked in sequence, wherein the material of the inner matrix resin layer is the inner matrix resin for the cold-stretch sleeve packaging film described in the above technical solution.
[0012] Preferably, the thickness ratio of the outer matrix resin layer, the middle matrix resin layer and the inner matrix resin layer is 2:6:2.
[0013] Preferably, the outer layer matrix resin layer comprises the following components in mass proportions: 65 parts of hexene copolymer LLDPE resin particles and 35 parts of metallocene linear low-density polyethylene resin particles; the middle layer matrix resin layer comprises the following components in mass proportions: 80 parts of metallocene linear low-density polyethylene resin particles and 20 parts of hexene copolymer LLDPE resin particles.
[0014] The invention provides an inner layer matrix resin for a cold-stretch sleeve packaging film, comprising the following components in parts by mass: 20-24 parts of metallocene linear low-density polyethylene, 75 parts of hexene copolymer LLDPE and 1-5 parts of a pre-dispersed masterbatch; the pre-dispersed masterbatch comprises the following components in parts by mass: 70% of vaterite calcium carbonate, 0.5-1.5% of an activated dispersing component and the remainder of metallocene linear low-density polyethylene native polymer powder.
[0015] Compared with the prior art, the present invention has the following beneficial effects: Vaterite calcium carbonate is a polycrystalline vaterite composed of nano-sized microcrystalline spheroids. It is different from single crystals such as calcite calcium carbonate and aragonite calcium carbonate. Vaterite calcium carbonate often exists in the form of spherical aggregates, while calcite calcium carbonate often exists in the form of regular rhombohedrons, and aragonite calcium carbonate is easy to form needles. Vaterite calcium carbonate has the characteristics of large specific surface area, good dispersibility, uniform spherical size distribution, etc., and is significantly better than the other two crystalline calcium carbonates in improving the filling performance of plastic products, product fluidity and gloss. The present invention reduces the inner layer dynamic friction coefficient of the inner layer matrix resin by introducing vaterite calcium carbonate, improves the opening smoothness function, and the vaterite calcium carbonate has low cost, low oil absorption value, and is easy to disperse. The prepared cold stretch sleeve packaging film is used for secondary containerized packaging of synthetic resins, has the characteristics of easy packaging and green environmental protection, and provides a method for reducing the inner layer dynamic friction coefficient for consumers.
[0016] Furthermore, the activated dispersing component in the present invention fully infiltrates the surface of vaterite calcium carbonate, thereby organizing the surface of the vaterite calcium carbonate inorganic powder, promoting the dispersion of the vaterite calcium carbonate, and ensuring that the vaterite calcium carbonate does not affect the mechanical properties of the film.
[0017] The present invention also provides a cold-stretched sleeve packaging film, which is used for cold-drawn sleeves of ton pallets or two-ton pallets of synthetic resin products. It has the characteristics of improving the adaptability of film to mechanical sleeves and the flatness after sleeves, meeting the performance requirements of mechanical sleeves and reducing raw material costs. DETAILED DESCRIPTION
[0018] The present invention provides an inner layer matrix resin for a cold stretch sleeve packaging film, comprising the following components in parts by mass: 20 to 24 parts of metallocene linear low-density polyethylene, 75 parts of hexene copolymer LLDPE and 1 to 5 parts of a pre-dispersed masterbatch; The pre-dispersed masterbatch comprises the following components in percentage by mass: 70% of vaterite calcium carbonate, 0.5-1.5% of activated dispersing component and the balance of metallocene linear low-density polyethylene original polymer powder.
[0019] In the present invention, unless otherwise specified, the raw materials used are all commercially available products in the art.
[0020] The inner layer matrix resin for the cold stretch sleeve packaging film provided by the present invention comprises 20 to 24 parts by mass of metallocene linear low-density polyethylene, and in specific embodiments of the present invention, it can be 20, 21, 22.5, 23.5 and 24 parts.
[0021] In the present invention, the melt flow rate of the metallocene linear low-density polyethylene is preferably 1.0-2.0 g / 10 min, and the density is preferably 0.918-0.920 g / cm3 .
[0022] In the present invention, the melt flow rate of the hexene copolymer LLDPE is preferably 0.5-2.5 g / 10 min, and the density is preferably 0.916-0.922 g / cm 3 .
[0023] Based on 100 parts by mass of the inner layer matrix resin for the cold stretch sleeve packaging film, the mass fraction of the pre-dispersed masterbatch in the inner layer matrix resin for the cold stretch sleeve packaging film can be 1, 1.5, 2, 2.5, 3, 4 or 5 parts.
[0024] In the present invention, the particle size of the pre-dispersed masterbatch is preferably 2-3 mm×2-4 mm.
[0025] In the present invention, the fineness of the vaterite calcium carbonate is preferably 600-1200 meshes, more preferably 800-1000 meshes, and in a specific embodiment of the present invention, it can be 600, 700, 800, 900, 1000, 1100 or 1200 meshes. The present invention reduces the inner layer dynamic friction coefficient of the inner layer matrix resin by introducing vaterite calcium carbonate, improves the opening smooth function, and the vaterite calcium carbonate is easy to disperse, low in cost, and the obtained cold stretch sleeve packaging film is applied to the secondary containerized packaging of synthetic resin, has the characteristics of easy set and green environmental protection, and provides a method for reducing the inner layer dynamic friction coefficient for consumers.
[0026] In the present invention, the mass percentage of the activated dispersing component in the pre-dispersed masterbatch is preferably 0.8-1%. In specific embodiments of the present invention, it can be 0.5%, 0.8%, 1%, 1.3% and 1.5%.
[0027] In the present invention, the activated dispersing component is preferably a composite of ethylene-vinyl acetate copolymer wax (EVA-WAX) and calcium stearate.
[0028] In the present invention, the mass ratio of ethylene-vinyl acetate copolymer wax and calcium stearate in the activated dispersing component is preferably 5:1-1:5, more preferably 3:1-2:1. In a specific embodiment of the present invention, it can be 5:1, 3:1, 2:1, 1:5 or 5:2.
[0029] In the present invention, the weight average molecular weight (Mw) of the ethylene-vinyl acetate copolymer wax is preferably 500-1500, more preferably 800-1200. In a specific embodiment of the present invention, it can be 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400 or 1500.
[0030] In the present invention, the melt flow rate of the metallocene linear low-density polyethylene raw polymer powder is preferably 2.5-4.5 g / 10 min, and the density is preferably 0.918-0.922 g / cm 3 The average particle size is preferably 50-300 μm. In a specific embodiment of the present invention, it can be 50 μm, 100 μm, 150 μm, 200 μm, 250 μm or 300 μm.
[0031] The present invention also provides a method for preparing the inner layer matrix resin for the cold stretch sleeve packaging film described in the above technical solution, comprising the following steps: Mixing vaterite calcium carbonate, an activated dispersing component and a dispersant to obtain a slurry; The slurry is mixed with metallocene linear low-density polyethylene raw polymer powder and extruded and granulated to obtain a pre-dispersed masterbatch; The pre-dispersed masterbatch, metallocene linear low-density polyethylene and hexene copolymer LLDPE are mixed to obtain the inner layer matrix resin for the cold stretch sleeve packaging film.
[0032] The invention mixes vaterite calcium carbonate, an activated dispersing component and a dispersant to obtain slurry.
[0033] In the present invention, the dispersant is preferably cyclohexane. The present invention has no particular limitation on the amount of the dispersant, as long as the vaterite calcium carbonate and the activated dispersing component are uniformly dispersed.
[0034] In the present invention, the mixing temperature is preferably 60° C., and the mixing time is preferably 20 min.
[0035] After obtaining the slurry, the present invention mixes the slurry with metallocene linear low-density polyethylene native polymer powder to perform extrusion granulation to obtain a pre-dispersed masterbatch.
[0036] The present invention preferably adds metallocene linear low-density polyethylene native polymer powder to the slurry and continues mixing for 5 minutes, removes the dispersant to obtain a dry mixed powder, adds the mixed powder to a twin-screw compounding granulator, and compounds and granulates it at a melt processing temperature of 190° C. to obtain the pre-dispersed masterbatch.
[0037] After obtaining the pre-dispersed masterbatch, the present invention mixes the pre-dispersed masterbatch, metallocene linear low-density polyethylene and hexene copolymer LLDPE to obtain the inner layer matrix resin for the cold stretch sleeve packaging film.
[0038] The present invention has no particular limitation on the specific manner of mixing, and any manner familiar to those skilled in the art may be used.
[0039] The present invention also provides a cold-stretch sleeve packaging film, comprising an outer matrix resin layer, a middle matrix resin layer and an inner matrix resin layer stacked in sequence, wherein the material of the inner matrix resin layer is the inner matrix resin for the cold-stretch sleeve packaging film described in the above technical solution.
[0040] In the present invention, the thickness ratio of the outer matrix resin layer, the middle matrix resin layer and the inner matrix resin layer is preferably 2:6:2.
[0041] In the present invention, the outer matrix resin layer preferably comprises the following components in parts by mass: 65 parts of hexene copolymer LLDPE resin particles and 35 parts of metallocene linear low-density polyethylene resin particles.
[0042] In the present invention, the outer matrix resin layer preferably also includes antistatic masterbatch, and the mass of the antistatic masterbatch is preferably 2-4% of the sum of the mass of the hexene copolymer LLDPE resin particles and the metallocene linear low-density polyethylene resin particles in the outer matrix resin layer. In a specific embodiment of the present invention, it can be 2%, 3% or 4%. The present invention has no special limitation on the type and particle size of the electrostatic masterbatch, and the types familiar to those skilled in the art can be used. In a specific embodiment of the present invention, the antistatic masterbatch is purchased from Nanjing Special Plastics Technology Co., Ltd., and the product model is TJ510.
[0043] In the present invention, the middle base resin layer preferably comprises the following components in parts by mass: 80 parts of metallocene linear low-density polyethylene resin particles and 20 parts of hexene copolymer LLDPE resin particles.
[0044] In the present invention, the middle layer matrix resin layer preferably also includes extrusion-aid masterbatch, and the mass of the extrusion-aid masterbatch is preferably 1-4% of the sum of the mass of the metallocene linear low-density polyethylene resin particles and the hexene copolymer LLDPE resin particles in the middle layer matrix resin layer. In a specific embodiment of the present invention, it can be 2%, 3% or 4%. The present invention has no special limitation on the type and particle size of the extrusion-aid masterbatch, and the types familiar to those skilled in the art can be used. In a specific embodiment of the present invention, the extrusion-aid masterbatch is purchased from Nanjing Special Plastics Technology Co., Ltd., and the product model is EF220.
[0045] The present invention also provides a method for preparing the cold stretch sleeve packaging film described in the above technical solution, comprising the following steps: The outer layer matrix resin layer material, the middle layer matrix resin layer material and the inner layer matrix resin layer material are subjected to three-layer composite co-extrusion blow molding to obtain the cold stretch sleeve packaging film.
[0046] In the present invention, during the three-layer composite co-extrusion blowing process, the melt temperature of the outer layer matrix resin layer material is preferably 175~185°C, the melt temperature of the middle layer matrix resin layer material is preferably 180~190°C, and the melt temperature of the inner layer matrix resin layer material is preferably 170~180°C.
[0047] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0048] The present invention adopts national standards or industry standards for testing. The specific testing method is as follows: The tensile strength is tested in accordance with GB / T 1040.3-2006.
[0049] The elongation at break is carried out in accordance with GB / T 1040.3-2006.
[0050] The right-angle tear strength is tested in accordance with QB / T1130.
[0051] The dart impact strength is tested in accordance with GB / T 9639.1-2008.
[0052] The elastic recovery rate is determined according to the method specified in 5.6.6 of T / ZZB 1008-2019 standard.
[0053] The dynamic friction coefficient is carried out in accordance with GB / T 10006-2021.
[0054] Raw materials used in the examples: The fineness of vaterite calcium carbonate is 600~1200 mesh; Antistatic masterbatch was purchased from Nanjing Special Plastics Technology Co., Ltd., product model TJ510; The extrusion-aid masterbatch was purchased from Nanjing Special Plastics Technology Co., Ltd., product model EF220; The melt flow rate of mLLDPE original polymer powder is 2.5g / 10min and the density is 0.918g / cm 3 ; The melt flow rate of hexene copolymer LLDPE resin pellets is 0.5g / 10min and the density is 0.916g / cm 3 ; The melt flow rate of mLLDPE resin pellets is 1.0 g / 10 min and the density is 0.918 g / cm 3 .
[0055] Example 1 The thickness ratio of the outer matrix resin layer, the middle matrix resin layer and the inner matrix resin layer of the cold stretch sleeve packaging film is 2:6:2; the mass composition of the resin raw material of the outer matrix resin layer is hexene copolymer LLDPE resin particles: mLLDPE resin particles = 65:35, the mass percentage of the antistatic masterbatch to the mass percentage of the resin raw material of the outer matrix resin layer is 2.0%, and the melt temperature of the blown film processing is 175°C; the mass ratio of the resin raw material of the middle matrix resin layer is mLLDPE resin particles: hexene copolymer LLDPE resin particles = 80:20, the mass of the extrusion-aid masterbatch to the mass percentage of the resin raw material of the middle matrix resin layer is 1%, and the melt temperature of the blown film processing is 180℃; the raw materials of the inner matrix resin layer are 24 parts by mass of mLLDPE resin granules, 75 parts by mass of hexene copolymer LLDPE, and 1 part by mass of pre-dispersed masterbatch. Taking the pre-dispersed masterbatch as 100 parts by mass, the pre-dispersed masterbatch is composed of 70 parts by mass of 600-mesh vaterite calcium carbonate, 0.5 parts by mass of a composition of ethylene-vinyl acetate copolymer wax (weight-average molecular weight of 5 million) and calcium stearate (the mass ratio of ethylene-vinyl acetate copolymer wax to calcium stearate in the composition is 5:1), 29.5 parts by mass of mLLDPE native polymer powder (average particle size of 50μm), and the melt temperature of the blown film is 170℃.
[0056] The preparation method of the pre-dispersed masterbatch is as follows: first, a composition of ethylene-vinyl acetate copolymer wax and calcium stearate is mixed with vaterite-type calcium carbonate in a cyclohexane solvent at 60°C for 20 minutes, then mLLDPE native polymer powder is added and mixed for 5 minutes, cyclohexane is removed to obtain a dry mixed powder, and the mixed powder is added to a twin-screw compounding and granulating machine for compounding and granulating at a melt processing temperature of 190°C to prepare a pre-dispersed masterbatch.
[0057] After testing, the obtained cold stretch sleeve packaging film has a thickness of 130μm, a tensile strength (longitudinal / transverse) of 29.4 / 28.8MPa, an elongation at break (longitudinal / transverse) of 670 / 785%, and a tear strength (longitudinal / transverse) of 51.6 / 51.2N·mm -1 , the dart impact strength is 1050g, the lateral elastic recovery rate is 49%, and the inner layer dynamic friction coefficient is 0.31.
[0058] Example 2 The same as Example 1, except that: The raw materials of the inner matrix resin layer are 23.5 parts by mass of mLLDPE resin particles, 75 parts by mass of hexene copolymer LLDPE, and 1.5 parts by mass of pre-dispersed masterbatch. Taking the mass of the pre-dispersed masterbatch as 100, the pre-dispersed masterbatch is composed of 70 parts by mass of 800-mesh vaterite calcium carbonate, 0.8 parts by mass of a composition of ethylene-vinyl acetate copolymer wax (weight-average molecular weight of 8 million) and calcium stearate (the mass ratio of ethylene-vinyl acetate copolymer wax to calcium stearate in the composition is 3:1), and 29.2 parts by mass of mLLDPE native polymer powder (average particle size of 100 μm).
[0059] After testing, the obtained cold stretch sleeve packaging film has a thickness of 131μm, a tensile strength (longitudinal / transverse) of 29.1 / 28.9MPa, an elongation at break (longitudinal / transverse) of 660 / 790%, and a tear strength (longitudinal / transverse) of 51.1 / 51.3N·mm -1 , the dart impact strength is 990g, the lateral elastic recovery rate is 47%, and the inner layer dynamic friction coefficient is 0.29.
[0060] Example 3 The same as Example 1, except that: The raw materials of the inner matrix resin layer are 22.5 parts by mass of mLLDPE resin particles, 75 parts by mass of hexene copolymer LLDPE, and 2.5 parts by mass of pre-dispersed masterbatch. Taking the mass of the pre-dispersed masterbatch as 100, the pre-dispersed masterbatch is composed of 70 parts by mass of 1000-mesh vaterite calcium carbonate, 1 part by mass of a composition of ethylene-vinyl acetate copolymer wax (weight-average molecular weight of 12 million) and calcium stearate (the mass ratio of ethylene-vinyl acetate copolymer wax to calcium stearate in the composition is 3:1), and 29 parts by mass of mLLDPE native polymer powder (average particle size of 150 μm).
[0061] After testing, the obtained cold stretch sleeve packaging film has a thickness of 129μm, a tensile strength (longitudinal / transverse) of 28.6 / 28.4MPa, an elongation at break (longitudinal / transverse) of 640 / 750%, and a tear strength (longitudinal / transverse) of 50.7 / 50.6N·mm -1 , the dart impact strength is 965g, the lateral elastic recovery rate is 47%, and the inner layer dynamic friction coefficient is 0.26.
[0062] Example 4 The same as Example 1, except that: The raw materials of the inner matrix resin layer are 21 parts by mass of mLLDPE resin particles, 75 parts by mass of hexene copolymer LLDPE, and 4 parts by mass of pre-dispersed masterbatch. Taking the mass of the pre-dispersed masterbatch as 100, the pre-dispersed masterbatch is composed of 70 parts by mass of 1200-mesh vaterite calcium carbonate, 1.5 parts by mass of a composition of ethylene-vinyl acetate copolymer wax (weight-average molecular weight of 15 million) and calcium stearate (the mass ratio of ethylene-vinyl acetate copolymer wax to calcium stearate in the composition is 1:5), and 28.5 parts by mass of mLLDPE native polymer powder (average particle size of 200 μm).
[0063] After testing, the obtained cold stretch sleeve packaging film has a thickness of 130μm, a tensile strength (longitudinal / transverse) of 28.4 / 28.3MPa, an elongation at break (longitudinal / transverse) of 620 / 730%, and a tear strength (longitudinal / transverse) of 50.5 / 50.3N·mm -1 The dart impact strength is 938g, the lateral elastic recovery rate is 46%, and the inner layer dynamic friction coefficient is 0.22.
[0064] Example 5 The same as Example 1, except that: The raw materials of the inner matrix resin layer are 20 parts by mass of mLLDPE resin particles, 75 parts by mass of hexene copolymer LLDPE, and 5 parts by mass of pre-dispersed masterbatch. Taking the mass of the pre-dispersed masterbatch as 100, the pre-dispersed masterbatch is composed of 70 parts by mass of 900-mesh vaterite calcium carbonate, 1.3 parts by mass of a composition of ethylene-vinyl acetate copolymer wax (weight-average molecular weight of 10 million) and calcium stearate (the mass ratio of ethylene-vinyl acetate copolymer wax to calcium stearate in the composition is 5:2), and 28.7 parts by mass of mLLDPE native polymer powder (average particle size of 100 μm).
[0065] After testing, the obtained cold stretch sleeve packaging film has a thickness of 131μm, a tensile strength (longitudinal / transverse) of 28.2 / 28.1MPa, an elongation at break (longitudinal / transverse) of 620 / 710%, and a tear strength (longitudinal / transverse) of 50.3 / 50.1N·mm -1 , the dart impact strength is 920g, the lateral elastic recovery rate is 46%, and the inner layer dynamic friction coefficient is 0.20.
[0066] Comparative Example 1 The same as Example 1, the only difference is that the vaterite calcium carbonate in the pre-dispersed masterbatch is replaced by ordinary calcium carbonate.
[0067] After testing, the obtained cold stretch sleeve packaging film has a thickness of 130μm, a tensile strength (longitudinal / transverse) of 28.2 / 27.4MPa, an elongation at break (longitudinal / transverse) of 650 / 745%, and a tear strength (longitudinal / transverse) of 50.1 / 49.6N·mm -1 The dart impact strength is 950g, the lateral elastic recovery rate is 47%, and the inner layer dynamic friction coefficient is 0.39.
[0068] It can be seen that the present invention provides a cold-stretched sleeve packaging film with a low dynamic friction coefficient, which has the characteristics of improving the adaptability of the film to mechanical sheathing and the flatness after sheathing, can meet the performance requirements of mechanical sheathing and reduce the cost of raw materials.
[0069] Comparative Example 2 The same as Example 1, the only difference is that the activated dispersing component ethylene-vinyl acetate copolymer wax is not added in the preparation of the pre-dispersed masterbatch, and is replaced by an equal mass of mLLDPE original ecological polymer powder.
[0070] After testing, the obtained cold stretch sleeve packaging film has a thickness of 131μm, a tensile strength (longitudinal / transverse) of 28.6 / 28.1MPa, an elongation at break (longitudinal / transverse) of 665 / 750%, and a tear strength (longitudinal / transverse) of 50.7 / 50.8N·mm -1 The dart impact strength is 985g, the lateral elastic recovery rate is 49%, and the inner layer dynamic friction coefficient is 0.34.
[0071] It can be seen that the mechanical properties of the cold stretch sleeve packaging film decrease and the friction coefficient increases when no activated dispersing component is added, which is mainly caused by the influence of the dispersion uniformity and interface compatibility of vaterite calcium carbonate.
[0072] Comparative Example 3 The same as Example 1, the only difference is that the vaterite calcium carbonate in the pre-dispersed masterbatch is replaced by fumed silicon dioxide.
[0073] After testing, the obtained cold stretch sleeve packaging film has a thickness of 130μm, a tensile strength (longitudinal / transverse) of 28.4 / 27.8MPa, an elongation at break (longitudinal / transverse) of 670 / 745%, and a tear strength (longitudinal / transverse) of 50.1 / 49.9N·mm -1 , the dart impact strength is 990g, the lateral elastic recovery rate is 48%, and the inner layer dynamic friction coefficient is 0.36.
[0074] It can be seen that when silicon dioxide is used to replace vaterite calcium carbonate in the pre-dispersed masterbatch, the various properties of the obtained cold stretch sleeve packaging film cannot reach the effect of Example 1.
[0075] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. An inner layer matrix resin for a cold stretch sleeve packaging film, It is characterized in that The method comprises the following components in parts by weight: 20 to 24 parts of metallocene linear low-density polyethylene, 75 parts of hexene copolymer LLDPE and 1 to 5 parts of pre-dispersed masterbatch; The pre-dispersed masterbatch comprises the following components in percentage by mass: 70% of vaterite calcium carbonate, 0.5-1.5% of activated dispersing component and the balance of metallocene linear low-density polyethylene original polymer powder.
2. The inner layer matrix resin for the cold stretch hood packaging film according to claim 1, It is characterized in that The fineness of the vaterite calcium carbonate is 600-1200 meshes.
3. The inner layer matrix resin for the stretch hood packaging film according to claim 1, It is characterized in that The activated dispersing component is a complex of ethylene-vinyl acetate copolymer wax and calcium stearate.
4. The inner layer matrix resin for the cold stretch hood packaging film according to claim 3, It is characterized in that The mass ratio of ethylene-vinyl acetate copolymer wax to calcium stearate in the activated dispersing component is 5:1-1:
5.
5. The inner layer matrix resin for the stretch hood packaging film according to claim 3 or 4, It is characterized in that The weight average molecular weight of the ethylene-vinyl acetate copolymer wax is 500-1500.
6. The inner layer base resin for the stretch hood packaging film according to claim 1, It is characterized in that The melt flow rate of the metallocene linear low-density polyethylene raw polymer powder is 2.5-4.5 g / 10 min, and the density is 0.918-0.922 g / cm 3 , the average particle size is 50~300μm.
7. A method for preparing an inner layer matrix resin for a cold stretch hood packaging film according to any one of claims 1 to 6, It is characterized in that The following steps are involved: Mixing vaterite calcium carbonate, an activated dispersing component and a dispersant to obtain a slurry; The slurry is mixed with metallocene linear low-density polyethylene raw polymer powder and extruded and granulated to obtain a pre-dispersed masterbatch; The pre-dispersed masterbatch, metallocene linear low-density polyethylene and hexene copolymer LLDPE are mixed to obtain the inner layer matrix resin for the cold stretch sleeve packaging film.
8. A cold stretch hood packaging film, It is characterized in that The invention comprises an outer matrix resin layer, a middle matrix resin layer and an inner matrix resin layer which are stacked in sequence, wherein the material of the inner matrix resin layer is the inner matrix resin for the cold stretch sleeve packaging film according to any one of claims 1 to 6.
9. The stretch hood packaging film according to claim 8, It is characterized in that The thickness ratio of the outer matrix resin layer, the middle matrix resin layer and the inner matrix resin layer is 2:6:
2.
10. The stretch hood packaging film according to claim 8, It is characterized in that The outer layer matrix resin layer comprises the following components in mass fractions: 65 parts of hexene copolymer LLDPE resin particles and 35 parts of metallocene linear low-density polyethylene resin particles; the middle layer matrix resin layer comprises the following components in mass fractions: 80 parts of metallocene linear low-density polyethylene resin particles and 20 parts of hexene copolymer LLDPE resin particles.
Citation Information
Patent Citations
Plastic composite lubricating agent and preparation method thereof
CN102690440A
Three-layer coextrusion heavy packaging membrane and fabrication method thereof
CN103029388A
Plastic filling lubrication master batch
CN103044740A
Film masterbatch with micro-foaming and coloring composite function and preparation method thereof
CN107987366A
Damp-proof master batch for injection molding drainage opening material and preparation method thereof
CN108329576A