Partially degradable antibacterial composite material for playing cards and preparation method of partially degradable antibacterial composite material

By using antibacterial agents to load cellulose in PVC playing cards, combined with melt blending process of polyvinyl chloride and other materials, the problems of antibacteriality and degradability of PVC playing cards are solved, and efficient antibacterial, environmentally friendly and safe are achieved And the elution-resistant playing card materials improve the durability and safety of playing cards.

CN118978773APending Publication Date: 2024-11-19YANGZHOU JINYI COMMERCIAL PRINTING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411093635.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing PVC playing cards are difficult to meet the needs of antibacterial, degradable and environmental protection. The antibacterial coating is prone to fall off and commonly used antibacterial agents contain heavy metal ions, which pose a risk of pathogenicity.

Method used

Using composite fibers loaded in cellulose with antibacterial agents, combined with polyvinyl chloride, matting agent, stabilizer and plasticizer, composite materials are prepared by melt blending process to provide highly efficient antibacterial, environmentally friendly, safe and elution-resistant partially degraded poker Composite materials for brand use.

Benefits of technology

It achieves the provision of partial biodegradable properties and efficient antibacterial properties while maintaining printing performance, mechanical properties and feel, and improves the durability and safety of playing cards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978773A_ABST
    Figure CN118978773A_ABST
Patent Text Reader

Abstract

The invention discloses a partially degradable antibacterial playing card composite material which comprises the following components in parts by mass: 80-90 parts of polyvinyl chloride, 10-20 parts of composite fibers, 7-8 parts of a delustering agent, 2-3 parts of a stabilizer and 2-3 parts of a plasticizer, the composite fiber is an antibacterial agent / cellulose composite fiber, and the content of the antibacterial agent is 15-20wt%. In the composite fiber, the antibacterial agent is loaded in the cellulose, so that the composite fiber has an antibacterial property and also has excellent elution resistance which is not possessed by a coating method. The cellulose is low in price and high in molecular polarity, cannot generate adverse effects on the printing performance of the PVC, and can improve the coloring firmness of the PVC material. The antibacterial agent / cellulose composite fiber is added, so that the hand feeling of the PVC playing card can be improved, the PVC playing card is firmer, and the PVC playing card has antibacterial and partial degradable properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer composite materials, and in particular to a partially degradable composite material for antibacterial playing cards and a preparation method thereof. Background Art

[0002] Polyvinyl chloride (PVC) playing cards are a type of playing cards that have become increasingly popular in the market in recent years. Compared with traditional paper playing cards, PVC playing cards have the advantages of strong durability, waterproof and anti-fouling, and comfortable feel. However, as consumers pay more and more attention to environmental protection and health, PVC playing cards also have requirements for antibacterial and biodegradable properties, but the PVC playing cards currently sold on the market are difficult to meet the above requirements.

[0003] Traditional antimicrobial coating methods are difficult to meet the needs of playing cards, mainly because playing cards will inevitably rub against each other or the user's hands during use, causing the antimicrobial coating to fall off. In addition, most commonly used silver ion antimicrobial agents contain heavy metal ions, which have a potential risk of causing disease when in contact with the human body for a long time. Therefore, it is very necessary to research and develop composite materials for playing cards that are resistant to elution, highly effective and safe, and biodegradable. Summary of the invention

[0004] In view of the problems that the above-mentioned PVC playing card material has no antibacterial property and is non-degradable, the present invention provides a partially degradable antibacterial playing card composite material and a preparation method thereof. The composite material has partial biodegradability while maintaining printing performance, mechanical properties and hand feel similar to those of PVC playing card materials, and introduces an antibacterial agent. It has the characteristics of high efficiency antibacterial, environmental protection and safety, and also has excellent wash-off resistance that the coating method does not have.

[0005] In order to achieve the above-mentioned object, the present invention provides a partially degradable antibacterial composite material for playing cards. The composite material comprises the following components by weight: 80-90 parts of polyvinyl chloride, 10-20 parts of composite fiber, 7-8 parts of matting agent, 2-3 parts of stabilizer, and 2-3 parts of plasticizer; the composite fiber is an antibacterial agent / cellulose composite fiber, and the content of the antibacterial agent is 15-20wt% (the mass percentage of the antibacterial agent in the composite fiber).

[0006] In the composite fiber, the antibacterial agent is loaded in cellulose, which has antibacterial properties and excellent wash-off resistance that the coating method does not have. Cellulose is cheap and has high molecular polarity, which will not adversely affect the printing performance of PVC and can improve the color fastness of PVC materials.

[0007] In the above composite material, the addition of antibacterial agent / cellulose composite fiber can not only improve the feel of PVC playing cards and make them firmer, but also make them have antibacterial and partially degradable properties.

[0008] Preferably, the antibacterial agent is nano zinc oxide.

[0009] Cellulose has many hydroxyl groups on its surface, and zinc oxide is also a polar substance with a certain amount of polar groups such as hydroxyl groups on its surface. The two are closely combined, mainly including electrostatic force, physical adsorption and a small amount of possible chemical reactions. Nano zinc oxide is used as an antibacterial agent with the characteristics of high efficiency, environmental protection and safety.

[0010] Preferably, the matting agent is titanium dioxide.

[0011] Preferably, the stabilizer is stabilizer 181.

[0012] Preferably, the plasticizer is plasticizer 488.

[0013] Another aspect of the present invention provides a method for preparing the composite material, which comprises the following steps:

[0014] S1. Preparation of composite fiber: dispersing cellulose and antimicrobial agent in ionic liquid, and spinning to obtain the composite fiber;

[0015] S2, melt blending: melt blending the polyvinyl chloride, matting agent, stabilizer, plasticizer and the composite fiber prepared in step S1 in a screw extruder, followed by cooling, granulation and drying to obtain the composite material.

[0016] In the above preparation method, the antibacterial agent is loaded into cellulose through step S1 to form an antibacterial agent / cellulose composite fiber, which has good thermal stability and can be used in the melt blending process of PVC and the like. The addition of the composite fiber can improve the bending modulus and strength of the material, and maintain a certain elongation at break, indicating that the material has good toughness and can ensure that the prepared playing cards do not break during use. More importantly, the material is given certain antibacterial properties. At the same time, cellulose, as a degradable material, can also provide partial degradability for the product.

[0017] Specifically, in step S1, the antibacterial agent is nano zinc oxide, and the mass ratio of cellulose to nano zinc oxide is 5:1-2.

[0018] Nano zinc oxide can provide certain antibacterial properties as an antibacterial agent, and cellulose fibers loaded with nano zinc oxide have good thermal stability, with no obvious thermal decomposition at around 400°C, and can be safely used in the melt blending process of PVC.

[0019] Specifically, in step S1, the dispersion is ultrasonic dispersion for 3 to 6 hours.

[0020] Specifically, in step S1, the spinning is dry-wet spinning, with an air gap of 4 to 8 cm, a spinning rate of 2 to 6 m / min, an extrusion pressure of 0.2 to 0.5 MPa, and an extrusion rate of 1 to 6 mL / min.

[0021] Specifically, in step S2, the temperature of the melt blending is 185-195°C, the screw length-to-diameter ratio of the screw extruder is 40-45, and the rotation speed is 120-180 rpm.

[0022] Through the above technical solution, the present invention achieves the following beneficial effects:

[0023] 1. The present invention provides a composite material formula for partially degradable antibacterial playing cards. The addition of composite fibers gives the material certain antibacterial properties and degradability, and can improve the mechanical properties of PVC playing card materials and maintain good toughness, thereby improving the feel of PVC playing cards.

[0024] 2. The present invention uses nano zinc oxide as an antibacterial agent loaded in the fiber, which not only has antibacterial properties but also has excellent wash-off resistance that the coating method does not have. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a SEM photograph of composite fiber B prepared in Example 2 of the present invention;

[0026] Figure 2 is the TGA curve of the composite fiber B prepared in Example 2 of the present invention;

[0027] Figure 3 is a SEM photograph of the composite material D prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0028] The specific implementation of the present invention is described in detail below in conjunction with the examples. It should be understood that the specific implementation described herein is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0029] Example 1

[0030] S1. Disperse 20g of nano zinc oxide in 1kg of ionic liquid and use ultrasonic dispersion for 4 hours. Take 100g of wood pulp cellulose and disperse it in the above mixture, and ultrasonically treat until the cellulose is completely dissolved. Use a homemade spinning machine for dry-wet spinning, with an air gap of 6cm and a coagulation bath of deionized water. The spinning rate is 3m / min, the extrusion pressure is 0.35MPa, and the solution extrusion rate is 3mL / min, and finally composite fiber A is obtained.

[0031] S2, 100g of the composite fiber A obtained in step S1 was uniformly mixed with 900g of PVC powder, 75g of titanium dioxide, 25g of stabilizer 181, and 25g of plasticizer 488, and melt-blended in a twin-screw extruder, with a screw length-diameter ratio of 42, a blending temperature of 190°C, and a screw speed of 150rpm. Then, the mixture was water-cooled, granulated, and dried to obtain a composite material C.

[0032] Example 2

[0033] S1. Disperse 40g of nano zinc oxide in 1kg of ionic liquid and use ultrasonic dispersion for 5 hours. Take 100g of wood pulp cellulose and disperse it in the above mixture, and ultrasonicate until the cellulose is completely dissolved. Use a homemade spinning machine for dry-wet spinning, with an air gap of 8cm and a coagulation bath of deionized water. The spinning rate is 6m / min, the extrusion pressure is 0.45MPa, and the solution extrusion rate is 6mL / min, and finally composite fiber B is obtained.

[0034] S2, 100g of the composite fiber B obtained in step S1 was uniformly mixed with 900g of PVC powder, 80g of titanium dioxide, 30g of stabilizer 181, and 20g of plasticizer 488, and melt-blended in a twin-screw extruder, with a screw aspect ratio of 45, a blending temperature of 195°C, and a screw speed of 180rpm. Then, the composite material D was obtained by water cooling, granulation, and drying.

[0035] Example 3

[0036] S1, preparing composite fiber B by the same method as in Example 2;

[0037] S2, 200g of the composite fiber B obtained in step S1 was uniformly mixed with 800g of PVC powder, 75g of titanium dioxide, 25g of stabilizer 181, and 25g of plasticizer 488, and melt-blended in a twin-screw extruder, with a screw length-diameter ratio of 42, a blending temperature of 190°C, and a screw speed of 150rpm. After that, the composite material E was obtained by water cooling, granulation, and drying.

[0038] Comparative Example

[0039] 800g PVC powder, 75g titanium dioxide, 25g stabilizer 181 and 25g plasticizer 488 were uniformly mixed and melt-blended in a twin-screw extruder with a screw length-diameter ratio of 42, a blending temperature of 190°C and a screw speed of 150rpm. The mixture was then water-cooled, granulated and dried to obtain a composite material F.

[0040] Performance Testing

[0041] The composite fiber B prepared in Example 2 was observed for microstructure under a scanning electron microscope (SEM). Figure 1 As shown. Figure 1It can be seen that a large number of granular substances are evenly distributed on the surface of composite fiber B, indicating that nano zinc oxide has been loaded in the fiber.

[0042] The composite fiber B prepared in Example 2 was subjected to thermogravimetric analysis (TGA), and its TGA curve is as follows: Figure 2 As shown. Figure 2 It can be seen that the cellulose fiber loaded with nano zinc oxide has good thermal stability, no obvious thermal decomposition is observed at about 400°C, and can be safely used in the melt blending process of PVC. The slight weight loss at about 200°C should be caused by the loss of water in cellulose. At the same time, the zinc oxide content can be calculated from the final residual weight to be about 18.2wt%, which is consistent with the initial feed ratio.

[0043] The composite material D prepared in Example 2 was observed for microstructure under a scanning electron microscope (SEM), and its SEM photo is as follows: Figure 3 As shown. Figure 3 It can be seen that the composite fiber is dispersed more evenly in PVC, and the fiber area size is about 500-1000nm. Good dispersion can provide guarantee for the mechanical properties of the material.

[0044] The composite materials C to E prepared in Examples 1 to 3 and the composite material F prepared in the comparative example were tested for flexural modulus, flexural strength, elongation at break and antibacterial rate. The results are shown in Table 1.

[0045] Table 1 Summary of properties of composite materials C~F

[0046]

[0047]

[0048] The following conclusions can be drawn from the data in Table 1:

[0049] After adding the antimicrobial agent / cellulose composite fiber, the mechanical properties and antibacterial properties of the material were affected to a certain extent. Compared with composite material F, after adding the composite fiber, the bending modulus and bending strength of composite materials C, D, and E are higher. Correspondingly, the prepared playing cards will appear more "firm" and feel better. At the same time, the elongation at break of composite materials C, D, and E has not decreased significantly, indicating that they still maintain sufficient toughness to ensure that the playing cards do not break during use. More importantly, due to the loading of nano zinc oxide, it has certain antibacterial properties. After testing, its antibacterial rate against Escherichia coli reached more than 86%, while the control sample F did not show any antibacterial effect.

[0050] The preferred implementation modes of the present invention are described in detail above in combination with the embodiments; however, the present invention is not limited to the specific details in the above implementation modes. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical scheme of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0051] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0052] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A partially degradable antibacterial composite material for playing cards, characterized in that: The invention comprises the following components by weight: 80-90 parts of polyvinyl chloride, 10-20 parts of composite fiber, 7-8 parts of matting agent, 2-3 parts of stabilizer and 2-3 parts of plasticizer; the composite fiber is an antibacterial agent / cellulose composite fiber, and the content of the antibacterial agent is 15-20wt%.

2. The composite material according to claim 1, characterized in that The antibacterial agent is nano zinc oxide.

3. The composite material according to claim 1, characterized in that The matting agent is titanium dioxide.

4. The composite material according to claim 1, characterized in that The stabilizer is stabilizer 181.

5. The composite material according to claim 1, characterized in that The plasticizer is plasticizer 488.

6. A method for preparing a composite material according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Preparation of composite fiber: dispersing cellulose and antimicrobial agent in ionic liquid, and spinning to obtain the composite fiber; S2, melt blending: melt blending the polyvinyl chloride, matting agent, stabilizer, plasticizer and the composite fiber prepared in step S1 in a screw extruder, followed by cooling, granulation and drying to obtain the composite material.

7. The preparation method according to claim 6, characterized in that: In step S1, the antibacterial agent is nano zinc oxide, and the mass ratio of cellulose to nano zinc oxide is 5:1-2.

8. The preparation method according to claim 6, characterized in that: In step S1, the dispersion is ultrasonic dispersion for 3 to 6 hours.

9. The preparation method according to claim 6, characterized in that: In step S1, the spinning is dry-wet spinning, with an air gap of 4 to 8 cm, a spinning rate of 2 to 6 m / min, an extrusion pressure of 0.2 to 0.5 MPa, and an extrusion rate of 1 to 6 mL / min.

10. The preparation method according to claim 6, characterized in that: In step S2, the temperature of the melt blending is 185-195°C, the screw length-diameter ratio of the screw extruder is 40-45, and the rotation speed is 120-180 rpm.