PBAT resin composite material and compound fertilizer composition
By adding calcium carbonate of specific particle size and amount and low molecular weight PBAT resin to PBAT resin, the problem of decreased mechanical properties of PBAT resin composites was solved, and high-performance and low-cost composite materials were prepared.
Patent Information
- Application Number
- CN202410944309.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-19
AI Technical Summary
In existing PBAT resin and calcium carbonate composite materials, the incompatibility between inorganic fillers and polymer resins leads to a decrease in the mechanical properties of the composite materials, especially a significant reduction in tensile strength and impact strength.
A PBAT resin composite material was prepared by using calcium carbonate with a particle size of 1800-2000 mesh, adding 25-28 parts of it, and maintaining a high content (not less than 90%) in PBAT resin, without surface treatment, and combining it with an appropriate amount of low molecular weight PBAT resin.
Without adding plasticizers or surface modifiers, the mechanical properties of PBAT resin are maintained, with tensile strength and impact strength retention rates not less than 90%, while reducing costs.
Smart Images

Figure BDA0004945162690000071 
Figure BDA0004945162690000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of compound fertilizers and relates to a PBAT resin composite material and a compound fertilizer composition. Background Art
[0002] Using degradable materials (such as PBAT resin, PLA resin, PBS resin, etc.) as carriers of elements such as N, P, and K and used as compound fertilizers, there are already disclosed technologies that can achieve the slow release of these elements and improve the fertilization effect. In addition, in order to reduce costs, some inorganic fillers are generally added to compound fertilizers, which can reduce costs and improve the modulus and rigidity of compound fertilizers. For example, Japanese patent JP2023060954A discloses a fertilizer particle, in which the fertilizer component is coated with a resin composition, and the resin composition includes a biodegradable resin (such as PBAT resin), an inorganic substance (such as calcium carbonate) and acetyl tributyl citrate. Among them, acetyl tributyl citrate can play a role in plasticizing and modifying the surface of inorganic fillers. However, from an environmental protection dimension, people tend to hope that the resin and surface modifier (or plasticizer) used in the compound fertilizer can be completely degraded, or less or no non-degradable or difficult to degrade organic components are added.
[0003] There are some existing technologies that have studied methods for modifying PBAT resin with calcium carbonate. For example, the journal article "Mechanical Properties and Crystallization Behavior of PBAT Modified with Calcium Carbonate" (Plastics, 2023, 52(6)) reported that calcium carbonate powder and PBAT resin were directly mixed and melt-extruded into granules without adding plasticizers or surface modifiers. It was found that the calcium carbonate content had a significant effect on the mechanical properties of the composite material. When the calcium carbonate content in PBAT was 20%, the tensile strength decreased by 6.3% and the impact strength decreased by 43.4%. When the calcium carbonate content in PBAT was 30%, the tensile strength decreased by 20% and the impact strength decreased by 76.1%. Summary of the invention
[0004] It is generally believed that inorganic fillers are added to polymer resins to prepare composite materials. Due to the incompatibility of inorganic fillers and polymer resins, the inorganic fillers have poor dispersibility in polymer resins, which affects the mechanical properties of the composite materials. For example, the tensile strength and impact strength of the composite materials are inferior to those of the polymer resin. The inorganic fillers are surface treated with organic substances so that the surface of the inorganic fillers is coated with organic substances, which can improve the compatibility with the polymer resin. However, it is surprisingly found that for a composite material composed of PBAT resin and calcium carbonate, when the particle size of calcium carbonate is within a certain range and the addition amount is within a certain range, there is no need to surface treat calcium carbonate. The composite material can basically achieve the mechanical properties of PBAT resin, and the performance retention rate of tensile strength and impact strength is not less than 90%. Based on this, the present invention provides a PBAT resin composite material and a composite fertilizer composition.
[0005] The technical solution of the present invention is as follows:
[0006] In one aspect, the present invention provides a PBAT resin composite material, which is composed of 100 parts of a degradable resin and 25-28 parts of calcium carbonate by weight;
[0007] The degradable resin contains PBAT resin, and the weight proportion of the PBAT resin in the degradable resin is not less than 90%;
[0008] The weight average molecular weight of the PBAT resin is not less than 60,000; the particle size of the calcium carbonate is 1800-2000 mesh.
[0009] The beneficial effects of the present invention are as follows: the PBAT resin composite material proposed by the present invention uses PBAT resin as the main degradable resin matrix, introduces a relatively high content of calcium carbonate, and limits the particle size range of calcium carbonate, so that the composite material can maintain the excellent mechanical properties of PBAT resin without the need for additional addition of plasticizers or surface modifiers, and does not cause too much reduction in the mechanical properties of PBAT resin such as tensile strength and impact strength after adding calcium carbonate.
[0010] Preferably, the weight proportion of the PBAT resin in the degradable resin is not less than 98%.
[0011] More preferably, the weight percentage of the PBAT resin in the degradable resin is 100%.
[0012] Preferably, the calcium carbonate is 27 parts.
[0013] Preferably, the particle size of the calcium carbonate is 1900 mesh.
[0014] More preferably, the particle size of the calcium carbonate is 2000 mesh.
[0015] Preferably, the degradable resin contains no more than 5% by weight of low molecular weight PBAT resin;
[0016] The weight average molecular weight of the low molecular weight PBAT resin is 3000-20000.
[0017] More preferably, the weight average molecular weight of the low molecular weight PBAT resin is 3000-15000.
[0018] Another aspect of the present invention provides a composite fertilizer composition, wherein the raw material components include the PBAT resin composite material and a fertilizer component as described in any one of the above technical solutions;
[0019] The fertilizer component accounts for no more than 30% by weight in the compound fertilizer composition.
[0020] Preferably, the fertilizer component is selected from one or a combination of urea, ammonium nitrate, ammonium sulfate, ammonium chloride, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, potassium nitrate, potassium chloride and potassium sulfate. DETAILED DESCRIPTION
[0021] The technical solution of the present invention is further illustrated and described below through specific implementation methods.
[0022] In one aspect, the present invention provides a PBAT resin composite material, which is composed of 100 parts of a degradable resin and 25-28 parts of calcium carbonate by weight;
[0023] The degradable resin contains PBAT resin, and the weight proportion of PBAT resin in the degradable resin is not less than 90%;
[0024] The weight average molecular weight of PBAT resin is not less than 60,000; the particle size of calcium carbonate is 1800-2000 mesh.
[0025] In the present invention, there is no particular limitation on the preparation method of the PBAT resin composite material. For example, the components are mixed according to a ratio, placed in a twin-screw extruder for melt extrusion granulation, the melt temperature is 150-180° C., the die temperature is 160-180° C., and the screw speed is 30-100 rpm to obtain a PBAT resin composite material.
[0026] The weight average molecular weight of PBAT resin is not less than 60,000, for example, it can be 60,000, 70,000, 80,000, 90,000, 100,000, 110,000, 120,000, etc., and has good mechanical strength. In the present invention, the weight proportion of PBAT resin in the biodegradable resin can be any value of 90%, 92%, 95%, 97%, 98%, 100%, etc., without special restrictions, and the balance can be other biodegradable resins, such as PLA.
[0027] The inventors found that when the particle size of calcium carbonate is 1800-2000 mesh, the composite material can maintain high mechanical properties without surface treatment of calcium carbonate, and the mechanical properties are not significantly reduced compared to PBAT resin; when calcium carbonate is 25-28 parts, the filling effect on PBAT resin is better, which can reduce the cost of the composite material and have little effect on its mechanical properties. In the present invention, calcium carbonate can be heavy calcium carbonate or light calcium carbonate, but light calcium carbonate is more preferred.
[0028] In a preferred embodiment of the present invention, the weight proportion of PBAT resin in the degradable resin is not less than 98%. For example, the weight proportion of PBAT resin in the degradable resin can be any value among 98%, 99%, 100%, etc., without special limitation.
[0029] In a more preferred embodiment of the present invention, the weight proportion of PBAT resin in the degradable resin is 100%.
[0030] In a preferred embodiment of the present invention, the calcium carbonate is 27 parts. The inventors found that when the content of calcium carbonate is 27 parts, the filling amount is large, and the impact on the mechanical properties of the PBAT resin is minimal, and the composite material can maintain good mechanical properties and low cost.
[0031] In a preferred embodiment of the present invention, the particle size of calcium carbonate is 1900 mesh. In the present invention, when calcium carbonate with a particle size of 1900 mesh is selected, the composite material can maintain higher mechanical properties, such as tensile strength, impact strength, etc., compared with PBAT resin.
[0032] In a more preferred embodiment of the present invention, the particle size of calcium carbonate is 2000 mesh. In the present invention, when calcium carbonate with a particle size of 2000 mesh is selected, it can ensure that a higher amount of calcium carbonate has higher filling and dispersibility in the PBAT resin, and the mechanical properties of the composite material are better.
[0033] In a preferred embodiment of the present invention, the degradable resin contains no more than 5% by weight of a low molecular weight PBAT resin;
[0034] The weight average molecular weight of the low molecular weight PBAT resin is 3000-20000.
[0035] The inventors have found that the introduction of an appropriate amount of low molecular weight PBAT resin into the composite material can improve the mechanical properties of the composite material. The possible reason is that the low molecular weight PBAT resin improves the compatibility of calcium carbonate and PBAT resin, thereby improving the dispersibility of calcium carbonate in the matrix PBAT resin, and the low molecular weight PBAT resin is also completely biodegradable. Therefore, no other types of surface treatment agents are introduced in the present invention. In addition, the addition amount of low molecular weight PBAT resin cannot be too large, otherwise it will cause the mechanical properties of the composite material to deteriorate, especially the tensile strength to deteriorate significantly. Further, the weight percentage of low molecular weight PBAT resin in the degradable resin is not less than 1%. For example, the weight percentage of low molecular weight PBAT resin in the degradable resin can be any value of 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, etc., without special restrictions.
[0036] In a more preferred embodiment of the present invention, the weight average molecular weight of the low molecular weight PBAT resin is 3000-15000. In the present invention, further screening the weight average molecular weight range of the low molecular weight PBAT resin can further improve the dispersibility and compatibility of calcium carbonate in the matrix PBAT resin. For example, the weight average molecular weight of the low molecular weight PBAT resin of the present invention can be any value of 3000, 4000, 5000, 6000, 7000, 8000, 9000, 10000, 11000, 12000, 13000, 14000, 15000, etc., without special restrictions.
[0037] Another aspect of the present invention provides a composite fertilizer composition, wherein the raw material components include the PBAT resin composite material of any of the above technical solutions and a fertilizer component;
[0038] The fertilizer component accounts for no more than 30% by weight in the compound fertilizer composition.
[0039] The composite fertilizer composition of the present invention uses a PBAT resin composite material as a carrier of the fertilizer component. During use, for example, when inserted into the soil of a flower pot, the PBAT resin composite material gradually degrades and gradually releases the loaded fertilizer component as time goes by and as microorganisms in the soil act. First, the fertilizer component can be released more evenly into the soil; second, there is no need to apply fertilizer frequently, and a rod-shaped composite fertilizer composition with a diameter of 1 cm and a height of 5 cm can be applied once every 4-6 months; third, the composite fertilizer composition can be clearly supplemented according to changes in the appearance of the composite fertilizer composition (for example, the size of the rod-shaped composite fertilizer composition will become smaller and smaller over time).
[0040] In a preferred embodiment of the present invention, the fertilizer component is selected from one or more combinations of urea, ammonium nitrate, ammonium sulfate, ammonium chloride, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, potassium nitrate, potassium chloride and potassium sulfate. In the present invention, by adding fertilizer components containing elements such as N, P, and K, it is possible to provide necessary nutrients for crops and improve the yield and quality of crops. However, the weight proportion of the fertilizer component in the composite fertilizer composition should not be too high, otherwise it will cause the mechanical properties of the composite fertilizer composition to be too poor, and it will not be easy to process and shape, or it will be easy to break after processing and shaping. For example, the weight proportion of the fertilizer component in the composite fertilizer composition can be any value of 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, 27%, 30%, etc., without special restrictions. In addition, the present invention has no particular limitation on the preparation method of the composite fertilizer composition. For example, it can be as follows: the components are mixed according to a ratio, placed in a twin-screw extruder for melt extrusion molding, the melt temperature is 130-170°C, the die temperature is 130-160°C, the screw speed is 30-100rpm, and the composite fertilizer composition is obtained. The product shape can be rods, granules, spheres, films, etc., without particular limitation.
[0041] The technical solution of the present invention is further described and illustrated according to various embodiments below. Unless otherwise specified, the parts described in the following embodiments are parts by weight.
[0042] Example 1
[0043] A PBAT resin composite material consists of 100 parts of PBAT resin (the weight average molecular weight of the PBAT resin is 110,000) and 27 parts of light calcium carbonate (the particle size is 2000 meshes) by weight.
[0044] It is prepared by the following method:
[0045] The components were mixed and blended according to a ratio, and placed in a twin-screw extruder for melt extrusion and granulation. The melt temperature was 150-180° C., the die temperature was 170° C., and the screw speed was 50 rpm to obtain a PBAT resin composite material.
[0046] Example 2
[0047] The difference between this embodiment and embodiment 1 is that the light calcium carbonate in embodiment 1 is replaced by light calcium carbonate with a particle size of 1900 mesh in equal amount. The other steps remain unchanged.
[0048] Example 3
[0049] The difference between this embodiment and embodiment 1 is that the light calcium carbonate in embodiment 1 is replaced by light calcium carbonate with a particle size of 1800 mesh in equal amount. The other steps remain unchanged.
[0050] Example 4
[0051] The difference between this embodiment and embodiment 1 is that the 100 parts of PBAT resin in embodiment 1 are replaced by a combination of 95 parts of PBAT resin with a weight average molecular weight of 110,000 and 5 parts of low molecular weight PBAT resin with a weight average molecular weight of 10,000. The remaining steps remain unchanged.
[0052] Example 5
[0053] The difference between this embodiment and embodiment 4 is that the low molecular weight PBAT resin in embodiment 4 is replaced by an equal amount of low molecular weight PBAT resin having a weight average molecular weight of 8000. The remaining steps remain unchanged.
[0054] Example 6
[0055] The difference between this embodiment and embodiment 1 is that the 100 parts of PBAT resin in embodiment 1 are replaced by a combination of 98 parts of PBAT resin with a weight average molecular weight of 110,000 and 2 parts of low molecular weight PBAT resin with a weight average molecular weight of 10,000. The remaining steps remain unchanged.
[0056] Example 7
[0057] The difference between this embodiment and embodiment 1 is that the light calcium carbonate in embodiment 1 is replaced by 25 parts of light calcium carbonate with the same particle size. The other steps remain unchanged.
[0058] Example 8
[0059] The difference between this embodiment and embodiment 1 is that the light calcium carbonate in embodiment 1 is replaced by 28 parts of light calcium carbonate with the same particle size. The other steps remain unchanged.
[0060] Comparative Example 1
[0061] The difference between this comparative example and Example 1 is that the light calcium carbonate in Example 1 is replaced by light calcium carbonate with a particle size of 2500 mesh in equal amounts. The remaining steps remain unchanged.
[0062] Comparative Example 2
[0063] The difference between this comparative example and Example 1 is that the light calcium carbonate in Example 1 is replaced by light calcium carbonate with a particle size of 5000 mesh in equal amounts. The remaining steps remain unchanged.
[0064] Comparative Example 3
[0065] The difference between this comparative example and Example 1 is that the light calcium carbonate in Example 1 is replaced by light calcium carbonate with a particle size of 1000 mesh in equal amounts. The remaining steps remain unchanged.
[0066] Comparative Example 4
[0067] The difference between this comparative example and Example 1 is that the light calcium carbonate in Example 1 is replaced by 32 parts of light calcium carbonate with the same particle size. The other steps remain unchanged.
[0068] Comparative Example 5
[0069] The difference between this comparative example and Example 4 is that the combination of 95 parts of PBAT resin with a weight average molecular weight of 110,000 and 5 parts of low molecular weight PBAT resin with a weight average molecular weight of 10,000 is adjusted to a combination of 92 parts of PBAT resin with a weight average molecular weight of 110,000 and 8 parts of low molecular weight PBAT resin with a weight average molecular weight of 10,000. The remaining steps remain unchanged.
[0070] Comparative Example 6
[0071] The difference between this comparative example and Example 1 is that calcium carbonate is not added. The remaining steps remain unchanged.
[0072] The mechanical properties of the formulations of Examples 1-8 and Comparative Examples 1-6 are shown in Table 1 below.
[0073] Tensile strength retention rate = composite material tensile strength / pure PBAT resin tensile strength × 100%;
[0074] Impact strength retention rate = composite material impact strength / pure PBAT resin impact strength × 100%;
[0075] The tensile strength of pure PBAT resin and the impact strength of pure PBAT resin shall be based on the data of Comparative Example 6.
[0076] Table 1
[0077]
[0078]
[0079] From the data in Table 1 above, it can be seen that the PBAT resin composite material of the present invention can still maintain high tensile strength and impact strength without surface treatment of calcium carbonate, and the retention rate is basically not less than 90%. When low molecular weight PBAT resin is further added to the composite material, the tensile strength and impact strength can be further improved. However, the increase or decrease of the particle size of calcium carbonate and the increase in the amount of addition are not conducive to the maintenance of mechanical properties.
[0080] Example 9
[0081] A composite fertilizer composition, the raw material components comprising the PBAT resin composite material prepared in the above Example 1 and a fertilizer component (a mixture of urea, diammonium phosphate and potassium nitrate, in a weight ratio of 1:2:1);
[0082] The fertilizer component accounts for 15% by weight in the compound fertilizer composition.
[0083] It is prepared by the following method:
[0084] The components were mixed in a proportion, placed in a twin-screw extruder for melt extrusion into a rod shape, the extrusion temperature was 130-170°C, the die temperature was 145°C, the screw speed was 60rpm, and a compound fertilizer rod was obtained. The bottom diameter of the compound fertilizer rod was 1cm and the length was 5cm.
[0085] Example 10
[0086] The difference between this embodiment and embodiment 9 is that the weight proportion of the fertilizer component in the compound fertilizer composition is 25%. The other steps remain unchanged.
[0087] 20 rod-shaped compound fertilizers of Example 9 and Example 10 were respectively inserted into the soil of 4 flower pots, with an exposed height of about 2 mm, and 5 rods were inserted into each flower pot. After 1 month, many holes appeared in the rod-shaped compound fertilizers, indicating that obvious degradation occurred. After 4-6 months, the rod-shaped compound fertilizers were basically completely degraded.
[0088] As described above, the basic principles, main features and advantages of the present invention are shown and described. Those skilled in the art should understand that the present invention is not limited by the above embodiments, which are only preferred embodiments of the present invention and cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the scope of the present invention and the content of the specification should still be within the scope of the present invention. The scope of protection required by the present invention is defined by the attached claims and their equivalents.
Claims
1. A PBAT resin composite material, characterized in that: By weight, it consists of 100 parts of biodegradable resin and 25-28 parts of calcium carbonate; The degradable resin contains PBAT resin, and the weight proportion of the PBAT resin in the degradable resin is not less than 90%; The weight average molecular weight of the PBAT resin is not less than 60,000; the particle size of the calcium carbonate is 1800-2000 mesh.
2. The PBAT resin composite material according to claim 1, characterized in that: The weight proportion of the PBAT resin in the degradable resin is not less than 98%.
3. The PBAT resin composite material according to claim 1, characterized in that: The weight percentage of the PBAT resin in the degradable resin is 100%.
4. The PBAT resin composite material according to claim 1, characterized in that: The calcium carbonate is 27 parts.
5. The PBAT resin composite material according to claim 1, characterized in that: The particle size of the calcium carbonate is 1900 mesh.
6. The PBAT resin composite material according to claim 1, characterized in that: The particle size of the calcium carbonate is 2000 mesh.
7. The PBAT resin composite material according to claim 1, characterized in that: The degradable resin contains no more than 5% by weight of low molecular weight PBAT resin; The weight average molecular weight of the low molecular weight PBAT resin is 3000-20000.
8. The PBAT resin composite material according to claim 7, characterized in that: The weight average molecular weight of the low molecular weight PBAT resin is 3000-15000.
9. A composite fertilizer composition, characterized in that: The raw material component comprises the PBAT resin composite material according to any one of claims 1 to 8 and a fertilizer component; The fertilizer component accounts for no more than 30% by weight in the compound fertilizer composition.
10. The compound fertilizer composition according to claim 9, characterized in that: The fertilizer component is selected from one or a combination of urea, ammonium nitrate, ammonium sulfate, ammonium chloride, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, potassium nitrate, potassium chloride and potassium sulfate.
Citation Information
Cited By
Modified material and preparation method thereof, and polycaproic acid butylene terephthalate film
CN119684761A