Transparent antistatic polyurethane elastomer and preparation method thereof
By introducing antistatic additives into polyurethane materials, the safety problems caused by the accumulation of electrostatic electricity of polyurethane materials are solved, and its antistatic stability and safety are improved.
Patent Information
- Application Number
- CN202411114388.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-19
AI Technical Summary
Polyurethane materials are prone to static electricity after friction with external objects, resulting in poor safety, which may absorb dust or cause fire and explosion accidents.
The preparation method of transparent antistatic polyurethane elastomer includes isocyanate, polyol/amine, chain extender and antistatic additive. The steps of heating and stirring in vacuum environment, mechanical stirring and heating curing are introduced to reduce the generation of static electricity and accumulation.
It effectively improves the antistatic stability of transparent antistatic polyurethane elastomers, enhances safety, and reduces the safety risks caused by static electricity.
Smart Images

Figure CN118978806A_ABST
Abstract
Description
Technical Field
[0001] The disclosed embodiments relate to the field of material technology, and in particular, to a transparent antistatic polyurethane elastomer and a method for preparing the transparent antistatic polyurethane elastomer. Background Art
[0002] Polyurethane, or PU for short, is an organic polymer material with great potential. Polyurethane began to be used in building insulation materials. In the 1980s, high-performance polyurethane coatings and elastomers began to be widely used. Since the end of the 20th century, the application scope of polyurethane materials has continued to expand, including automotive manufacturing, medical equipment, electronic products, construction, sporting goods, and aerospace.
[0003] Polyurethane has good elasticity and can quickly return to its original shape after deformation. This is due to the special structure of its molecular chain, which contains carbamate groups (-NHCOO-). The presence of carbamate groups enables polyurethane to effectively isolate charges and prevent current flow under electric fields, and it exhibits good electrical insulation properties as a whole. However, after friction with foreign objects, its surface may easily absorb dust in the air or cause electric shock during product processing or use, and even generate sparks that ignite flammable items, leading to fires and explosions, so its safety is poor. Summary of the invention
[0004] The purpose of the present disclosure is to provide a transparent antistatic polyurethane elastomer and a method for preparing the transparent antistatic polyurethane elastomer, thereby overcoming the problem of poor safety of the transparent antistatic polyurethane elastomer caused by the limitations and defects of the relevant technology at least to a certain extent.
[0005] According to one aspect of the present disclosure, a transparent antistatic polyurethane elastomer is provided, wherein components of the transparent antistatic polyurethane elastomer include isocyanate, polyol / amine, chain extender and antistatic additive.
[0006] In an exemplary embodiment of the present disclosure, the antistatic additive comprises: 60% of a quaternary ammonium cationic surfactant with a terminal hydroxyl functional group, 20% of tri-n-butylmethylammonium bis(trifluoromethanesulfonyl)imide salt and 20% of polyethylene glycol with a molecular weight of 600.
[0007] In an exemplary embodiment of the present disclosure, the isocyanate is a six-membered ring diisocyanate.
[0008] In an exemplary embodiment of the present disclosure, the polyol / amine is hydroxy-terminated polytetrahydrofuran of different molecular weights.
[0009] In an exemplary embodiment of the present disclosure, the chain extender is adipic acid dihydrazide.
[0010] According to one aspect of the present disclosure, there is provided a method for preparing a transparent antistatic polyurethane elastomer, comprising:
[0011] Add polyol / amine into the flask, heat and stir in a vacuum environment to remove water vapor in the solvent;
[0012] After the reaction system is cooled to the first temperature, a mixture of isocyanate and dibutyltin dilaurate is dissolved in N,N-dimethylacetamide solution and added to the flask through a syringe, the reaction system is heated and stirred under a nitrogen environment, and then cooled to a second temperature after heating and stirring;
[0013] Dissolve the chain extender in N,N-dimethylacetamide solution, add it into the reaction system, react and stir under nitrogen environment to obtain a viscous transparent solution;
[0014] adding an antistatic additive to the viscous transparent solution, and mechanically stirring at room temperature to obtain a polymer solution;
[0015] The polymer solution is poured into an organic glass mold, vacuumed to remove bubbles, and heated and cured to obtain a transparent antistatic polyurethane elastomer sample.
[0016] In an exemplary embodiment of the present disclosure, the heating temperature of the polyol / amine is 90° C.-110° C., and the stirring time is 20-30 minutes.
[0017] In an exemplary embodiment of the present disclosure, the first temperature is 75°C-85°C, and the second temperature is 35°C-45°C.
[0018] In an exemplary embodiment of the present disclosure, the mechanical stirring time is 12-15 hours.
[0019] In an exemplary embodiment of the present disclosure, the time for vacuuming and removing bubbles is 5-10 minutes, the heating temperature during the heating and curing process is 70° C.-80° C., and the curing time is 2-3 hours.
[0020] In the technical solution provided in the embodiments of the present invention, since the components of the transparent antistatic polyurethane elastomer include antistatic additives, the introduction of internally mixed antistatic additives can effectively reduce the generation and accumulation of static electricity on the surface of the transparent antistatic polyurethane elastomer, avoid safety problems caused by static electricity accumulation, improve the antistatic stability of the transparent antistatic polyurethane elastomer, and improve the safety of the elastomer.
[0021] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The accompanying drawings herein are incorporated into the specification and constitute a part of the specification, illustrate embodiments consistent with the present disclosure, and together with the specification are used to explain the principles of the present disclosure. Obviously, the accompanying drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without creative work.
[0023] Figure 1 A flow chart schematically shows a method for preparing a transparent antistatic polyurethane elastomer in an embodiment of the present disclosure.
[0024] Figure 2 The test results of the transparent antistatic polyurethane elastomer prepared according to Example 1 are schematically shown.
[0025] Figure 3 The test results of the transparent antistatic polyurethane elastomer prepared according to Example 2 are schematically shown. DETAILED DESCRIPTION
[0026] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as being limited to the examples set forth herein; on the contrary, these embodiments are provided so that the present disclosure will be more comprehensive and complete, and the concepts of the example embodiments are fully conveyed to those skilled in the art. The described features, structures, or characteristics may be combined in one or more embodiments in any suitable manner. In the following description, many specific details are provided to provide a full understanding of the embodiments of the present disclosure. However, those skilled in the art will appreciate that the technical solutions of the present disclosure may be practiced while omitting one or more of the specific details, or other methods, components, devices, steps, etc. may be adopted. In other cases, known technical solutions are not shown or described in detail to avoid obscuring various aspects of the present disclosure.
[0027] The terms "a", "an", "the" and "said" used in this specification are used to indicate the presence of one or more elements / components, etc.; the terms "including" and "having" are used to express an open-ended inclusion and mean that there may be additional elements / components, etc. in addition to the listed elements / components, etc.; the terms "first" and "second" etc. are used only as labels and are not intended to limit the quantity of their objects.
[0028] Polyurethane, also known as polyurethane, or PU for short, is a promising organic polymer material. Its polymer backbone contains a unique structure of carbamate group (-NHCOO). Polyurethane can be used to make elastic foams for seat cushions and mattresses. In addition, polyurethane can also be used as building insulation materials. With the development of technology, the application scope of polyurethane materials is constantly expanding, including automotive manufacturing, medical equipment, electronic products, construction, sporting goods, aerospace and other fields.
[0029] Polyurethane has good elasticity and can quickly recover to its original state after deformation, which is derived from the special structure of its molecular chain, including carbamate group (-NHCOO-), which can stretch and bend under external force, and quickly recover to its original state. In addition, the controllable hardness, high wear resistance, temperature stability and cross-linking ability of polyurethane also provide it with excellent elastic properties. However, the existence of the structure of carbamate group enables polyurethane to effectively isolate electric charge under electric field, prevent current flow, and show good electrical insulation performance as a whole. Based on this, its surface is easy to generate static electricity after friction with foreign objects, causing the accumulation of static charge, and long-term static charge accumulation can cause product processing or easy adsorption of dust in the air during use or cause electric shock, and even produce sparks to ignite flammable items and cause fire and explosion accidents. Therefore, the antistatic modification of PU is of great significance, and it is necessary to design a transparent antistatic PU elastomer and its preparation method to solve the above problems.
[0030] In order to solve the above technical problems, a transparent antistatic polyurethane elastomer is provided in an embodiment of the present disclosure. The components of the transparent antistatic polyurethane elastomer may include: isocyanate, polyol / amine, chain extender and antistatic additive.
[0031] In the embodiments of the present disclosure, since the components of the transparent antistatic polyurethane elastomer include antistatic additives, the introduction of antistatic additives can effectively reduce the generation and accumulation of static electricity on the surface of the transparent antistatic polyurethane elastomer, thereby avoiding safety problems caused by static electricity accumulation, improving the antistatic stability of the transparent antistatic polyurethane elastomer, and improving the safety of the elastomer.
[0032] Next, the transparent antistatic polyurethane elastomer will be described in detail.
[0033] The components of the transparent antistatic polyurethane elastomer may include isocyanate, polyol / amine, chain extender and antistatic additive.
[0034] The components of the antistatic additive may include: a quaternary ammonium salt cationic surfactant with a hydroxyl functional group at the end, tri-n-butylmethylammonium bis(trifluoromethanesulfonyl)imide salt, and polyethylene glycol with a molecular weight of 600.
[0035] Specifically, the component of the quaternary ammonium salt cationic surfactant having a hydroxyl functional group at the end is 60%, the component of tri-n-butylmethylammonium bis(trifluoromethanesulfonyl)imide salt is 20% and the component of polyethylene glycol with a molecular weight of 600 is 20%.
[0036] For the isocyanate in the transparent antistatic polyurethane elastomer, the isocyanate may be a six-membered ring diisocyanate, which refers to a diisocyanate containing a six-membered ring. Of course, other types of isocyanates may also be used, which are determined according to actual needs.
[0037] The polyol / amine in the transparent antistatic polyurethane elastomer can be hydroxy-terminated polytetramethylene glycol (PTMEG) with different molecular weights or other types.
[0038] The chain extender in the transparent antistatic polyurethane elastomer is a substance used to extend the molecular chain and increase the molecular weight. The chain extender in the transparent antistatic polyurethane elastomer of the embodiment of the present disclosure may be adipic acid dihydrazide.
[0039] The transparent antistatic polyurethane elastomer in the disclosed embodiment can effectively reduce the generation and accumulation of static electricity on the surface of the transparent antistatic polyurethane elastomer by introducing an internally mixed antistatic additive, thereby ensuring the antistatic stability of the elastomer. Since the hard segment structure of the transparent antistatic polyurethane elastomer contains multiple acyl semicarbazide and carbamate groups, which are connected by alicyclic hexaatoms with higher flexibility, this structural design is conducive to the formation of a higher density hydrogen bond array and has a better energy dissipation mechanism, so that the transparent antistatic polyurethane elastomer has better robustness.
[0040] In the embodiments of the present disclosure, a method for preparing a transparent antistatic polyurethane elastomer is also provided, which is used to prepare the transparent antistatic polyurethane elastomer. Figure 1 A schematic diagram of the process for preparing a transparent antistatic polyurethane elastomer is shown schematically in Figure 1 As shown in, the preparation method of the transparent antistatic polyurethane elastomer mainly comprises the following steps:
[0041] In step S110, polyol / amine is added to a flask, and heated and stirred in a vacuum environment to remove water in the solvent;
[0042] In step S120, after the reaction system is cooled, a mixture of isocyanate and dibutyltin dilaurate is dissolved in an N,N-dimethylacetamide solution and added to the flask through a syringe, and the reaction system is heated and stirred under a nitrogen environment, and then cooled after heating and stirring;
[0043] In step S130, a chain extender is dissolved in an N,N-dimethylacetamide solution and added to a reaction system, and reacted and stirred under a nitrogen environment to obtain a viscous transparent solution;
[0044] In step S140, an antistatic additive is added to the viscous transparent solution, and mechanical stirring is performed at room temperature to obtain a polymer solution;
[0045] In step S150, the polymer solution is poured into a plexiglass mold, vacuumed to remove bubbles, and heated and cured to obtain a transparent antistatic polyurethane elastomer.
[0046] The preparation method in the embodiment of the present disclosure only needs to dissolve a mixture of isocyanate and dibutyltin dilaurate in an N,N-dimethylacetamide solution, dissolve a chain extender in an N,N-dimethylacetamide solution and add the solution to a reaction system, react and stir under a nitrogen environment, add an antistatic additive to the viscous transparent solution and stir, and pour the polymer solution into a plexiglass mold to evacuate and remove bubbles and heat to cure. Only stirring, evacuating and heating to cure are required to obtain a transparent antistatic polyurethane elastomer. The operation steps are simple, the process flow is short, and the obtained transparent antistatic polyurethane elastomer has high stability and is suitable for industrial production.
[0047] In some embodiments, a transparent antistatic polyurethane elastomer can be prepared by the following method, specifically including the following steps: 100 equivalents of polytetrahydrofuran, pre-dehydrated at 120°C and 3×133.32Pa for 1h, adding 48 equivalents of diphenylmethane diisocyanate, stirring and reacting for 10min, adding 10.76 equivalents of benzyl alcohol (chain extender), stirring for another 15min, forming a high-viscosity paste polymer, pouring it into a container coated with release agent silicone oil, and baking it at 180°C for 8h to become a thermoplastic rubber. And hot pressing at 160°C and a pressure of 10MPa to form a product, so as to obtain a transparent antistatic polyurethane elastomer.
[0048] Next, the preparation method of the transparent antistatic polyurethane elastomer in the embodiment of the present disclosure is specifically described with reference to the accompanying drawings.
[0049] In step S110 , polyol / amine is added into a flask, and heated and stirred in a vacuum environment to remove water vapor.
[0050] In the embodiment of the present disclosure, the flask can be a three-necked round-bottom flask, and the flask can be connected to a mechanical stirring device. When the polyol / amine is polytetrahydrofuran (PTMEG), the polytetrahydrofuran can be a hydroxy-terminated polytetrahydrofuran of different molecular weights. The weight of the polytetrahydrofuran (PTMEG) can be 10 g, or it can be determined according to actual needs. The molecular weight of the polytetrahydrofuran (PTMEG) is Mn=2000 g mol -1 Furthermore, the polyol / amine may be added into a flask, and the polyol / amine may be heated and stirred in a vacuum environment to remove water in the polyol / amine.
[0051] When the polyol / amine is heated and stirred in a vacuum environment, the heating temperature is 90-110° C. and the stirring time is 20-30 minutes to remove water vapor in the polyol / amine. For example, the water vapor can be removed by stirring at 110° C. for 30 minutes in a vacuum environment.
[0052] In step S120, after the reaction system is cooled to the first temperature, a mixture of isocyanate and dibutyltin dilaurate is dissolved in N,N-dimethylacetamide solution and added to the flask through a syringe, the reaction system is heated and stirred under a nitrogen environment, and then cooled to the second temperature after heating and stirring.
[0053] In the disclosed embodiment, the reaction system refers to that after the reaction system is cooled to the first temperature, a mixture of isocyanate and dibutyltin dilaurate (DBTDL) can be dissolved in an N, N-dimethylacetamide solution. Dibutyltin dilaurate (DBTDL) and N, N-dimethylacetamide solution can be the basic materials for preparing polyurethane elastomers. Among them, the first temperature is used to indicate the temperature at which the reaction begins, which can be 80°C. After the reaction system is cooled to the first temperature, isocyanate and dibutyltin dilaurate (DBTDL) can be mixed to obtain a mixture, and the mixture can be dissolved in an N, N-dimethylacetamide solution. Among them, the isocyanate can be diisocyanate (IPDI) or toluene-2,4-diisocyanate (TDI), which is determined according to actual needs. In addition, different types of isocyanates have different corresponding weights, and the weight of diisocyanate (IPDI) can be greater than that of toluene-2,4-diisocyanate (TDI). For example, the weight of IPDI may be 2.22 g, and the weight of toluene-2,4-diisocyanate (TDI) may be 1.74 g.
[0054] After the reaction system is cooled to the first temperature, a mixture of isocyanate and dibutyltin dilaurate (DBTDL) can be dissolved in N, N-dimethylacetamide solution. After the mixture is dissolved in N, N-dimethylacetamide solution, it can be added to the flask by a syringe. The reaction system is heated and stirred under a nitrogen environment, and then cooled to a second temperature. Wherein, the second temperature is lower than the second temperature. Specifically, the first temperature can be 75°C-85°C, for example, 75°C, 80°C, 85°C; the second temperature is 35°C-45°C, for example, 35°C, 40°C, 45°C. The stirring time for heating and stirring the reaction system under a nitrogen environment is 2-3 hours.
[0055] For example, the reaction system can be cooled to a first temperature of 80°C, and a mixture of isocyanate and dibutyltin dilaurate (DBTDL) can be dissolved in an N,N-dimethylacetamide solution. After the mixture is dissolved in the N,N-dimethylacetamide solution, it can be added to the flask through a syringe. The mixture is heated and stirred for 2-3 hours under a nitrogen environment, and then cooled to a second temperature of 40°C after heating and stirring.
[0056] For example, after the reaction system is cooled to a first temperature of 80°C, a mixture of IPDI and DBTDL is dissolved in an N,N-dimethylacetamide solution (DMAc) and added to the flask via a syringe. The reaction system is heated and stirred at 80°C for 3 hours under a nitrogen atmosphere, and then cooled to 40°C. Alternatively, after the reaction system is cooled to 80°C, a mixture of toluene-2,4-diisocyanate (TDI) and DBTDL is dissolved in an N,N-dimethylacetamide solution (DMAc) and added to the flask via a syringe. The reaction system is heated and stirred at 80°C for 3 hours under a nitrogen atmosphere, and then cooled to a second temperature of 40°C.
[0057] In step S130, the chain extender is dissolved in N,N-dimethylacetamide solution and added into the reaction system, and reacted and stirred under a nitrogen environment to obtain a viscous transparent solution.
[0058] In the disclosed embodiment, a chain extender can be added to an N,N-dimethylacetamide solution, and the solution is added to the reaction system, and mechanical stirring is performed in a nitrogen environment to obtain a viscous transparent solution. The mechanical stirring time is 12-15 hours. The viscous transparent solution is an IPDI-SPU2000 solution or a TDI-SPU2000 solution. When the isocyanate is a diisocyanate (IPDI), the viscous transparent solution is an IPDI-SPU2000 solution; when the isocyanate is toluene-2,4-diisocyanate (TDI), the viscous transparent solution is a TDI-SPU2000 solution.
[0059] In step S140, an antistatic additive is added to the viscous transparent solution, and mechanical stirring is performed at room temperature to obtain a polymer solution.
[0060] In the disclosed embodiment, the antistatic additive can be added to the viscous transparent solution and mechanically stirred at room temperature to obtain a polymer solution. The mechanical stirring time can be 5 minutes to obtain a polymer solution with good dispersion of the antistatic additive. In some embodiments, an antistatic additive including 60% of a quaternary ammonium salt cationic surfactant with a hydroxyl functional group at the end, 20% of tri-n-butylmethylammonium bis(trifluoromethanesulfonyl)imide salt and 20% of a polyethylene glycol with a molecular weight of 600 can be added to an IPDI-SPU2000 solution or a TDI-SPU2000 solution.
[0061] In step S150, the polymer solution is poured into a plexiglass mold, vacuumed to remove bubbles, and heated and cured to obtain a transparent antistatic polyurethane elastomer.
[0062] In the embodiments of the present disclosure, the types of isocyanates are different, and the corresponding preparation processes may also be different. For example, after vacuuming and removing bubbles, the transparent antistatic polyurethane elastomer may be directly heated and cured. Alternatively, after vacuuming and removing bubbles, the transparent antistatic polyurethane elastomer may be prepolymerized at a preset temperature and heated and cured.
[0063] The temperature for vacuuming and evacuating bubbles may be 30°C-40°C, the time for vacuuming and evacuating bubbles may be 5-10 minutes, the heating temperature during the heat curing process may be 70°C-80°C, and the curing time may be 2-3 hours. For example, the heating temperature during the heat curing process may be 75°C. The preset temperature for prepolymerization may be lower than the heating temperature for heat curing, and the preset temperature may be 50°C-60°C, for example, the preset temperature may be 60°C. The time for prepolymerization at the preset temperature may be 1 hour, or other suitable values, which are not specifically limited here.
[0064] It should be noted that when the isocyanate is IPDI, it can be prepolymerized at a preset temperature after vacuuming to remove bubbles, and then heated to cure, that is, prepolymerized at a preset temperature and then heated to cure. When the isocyanate is toluene-2,4-diisocyanate (TDI), it is not necessary to prepolymerize at a preset temperature, and can be directly heated to cure. Of course, it is also possible to prepolymerize at a preset temperature after vacuuming to remove bubbles, and then heat to cure after prepolymerization.
[0065] In the embodiment of the present disclosure, prepolymerization can be performed at a preset temperature for 1 hour. By prepolymerizing at the preset temperature, the structure of the molecular chain can be freely adjusted, thereby avoiding the problem of poor molecular chain structure caused by a one-time temperature increase and improving performance.
[0066] For example, when the isocyanate is diisocyanate (IPDI), the obtained polymer solution is finally poured into a pre-prepared plexiglass mold, placed in a vacuum drying oven, and evacuated at 30°C to remove bubbles for 5 minutes, then prepolymerized at 60°C for 1 hour, then heated to 75°C and cured for 2 hours to obtain a transparent antistatic polyurethane elastomer.
[0067] When the isocyanate is toluene-2,4-diisocyanate (TDI), the obtained polymer solution can be poured into a pre-prepared plexiglass mold, placed in a vacuum drying oven, evacuated at 30°C to remove bubbles for 5 minutes, then directly heated to 75°C and cured for 2 hours to obtain a transparent antistatic polyurethane elastomer.
[0068] On this basis, the preparation method of the transparent antistatic polyurethane elastomer in the embodiments of the present disclosure is specifically described in combination with the following embodiments.
[0069] In the process of preparing the transparent antistatic polyurethane elastomer, different types of isocyanates can be selected, such as diisocyanate (IPDI) or toluene-2,4-diisocyanate (TDI) as the isocyanate. Different types of isocyanates may have different processes for preparing the transparent antistatic polyurethane elastomer.
[0070] Example 1
[0071] The preparation method of transparent antistatic polyurethane elastomer using diisocyanate (IPDI) mainly comprises the following steps:
[0072] Step 1: Add 10 g of polyol / amine PTMEG (Mn=2000 g mol-1) into a three-necked round-bottom flask connected to a mechanical stirring device, and stir for 30 minutes under heating conditions at 110° C. in a vacuum environment to remove water vapor.
[0073] Step 2: After the reaction system is cooled to 80°C, 2.22 g of IPDI and 0.02 g of DBTDL are mixed and dissolved in 5 mL of N,N-dimethylacetamide solution DMAc and added to the flask via a syringe. The reaction system is heated and stirred at 80°C for 3 hours under a nitrogen environment and then cooled to 40°C.
[0074] Step 3: Dissolve 0.87 g of adipic acid dihydrazide AD as a chain extender in 60 mL of N,N-dimethylacetamide solution DMAc, add it to the reaction system, and stir it at 40°C for 15 hours under a nitrogen environment. Finally, a viscous and transparent solution, namely IPDI-SPU2000 solution, is obtained. The IPDI-SPU2000 solution is a viscous and transparent solution.
[0075] Step 4: Add 0.5 g of antistatic additive to the IPDI-SPU2000 solution and mechanically stir at room temperature for 5 minutes to obtain a polymer solution in which the antistatic agent is well dispersed.
[0076] Step 5: Pour the obtained polymer solution into a pre-prepared plexiglass mold, put it into a vacuum drying oven, evacuate the air bubbles at 30°C for 5 minutes, then prepolymerize it at 60°C for 1 hour, then heat it to 75°C and cure it for 2 hours to finally obtain a transparent antistatic polyurethane elastomer as a sample.
[0077] Example 2
[0078] The preparation method of a transparent antistatic polyurethane elastomer using toluene-2,4-diisocyanate (TDI) as isocyanate mainly comprises the following steps:
[0079] Step 1: Add 10 g of PTMEG (Mn = 2000 gmol-1) into a three-necked round-bottom flask connected to a mechanical stirring device, and stir at 110° C. in a vacuum environment for 30 minutes to remove water vapor.
[0080] Step 2: After the reaction system is cooled to 80°C, 1.74 g of toluene-2,4-diisocyanate (TDI) and 0.02 g of DBTDL are mixed and dissolved in 30 mL of N,N-dimethylacetamide solution DMAc, and added to the flask via a syringe. The reaction system is heated and stirred at 80°C under a nitrogen environment for 3 hours, and then cooled to 40°C.
[0081] Step 3: 0.87 g of adipic acid dihydrazide AD as a chain extender was dissolved in 250 mL of N,N-dimethylacetamide solution (DMAc) solvent, added to the reaction system, and stirred at 40 ° C for 15 hours under a nitrogen environment to finally obtain a TDI-SPU2000 solution, which was a viscous and transparent solution.
[0082] Step 4: Add 0.3 g of antistatic additive to the TDI-SPU2000 solution and mechanically stir at room temperature for 5 minutes to obtain a polymer solution in which the antistatic agent is well dispersed.
[0083] Step 5: Pour the obtained polymer solution into a pre-prepared plexiglass mold, put it into a vacuum drying oven, evacuate the air bubbles at 30°C for 5 minutes, then directly heat it to 75°C and cure it for 2 hours to finally obtain a transparent antistatic polyurethane elastomer as a sample.
[0084] In the disclosed embodiment, a transparent antistatic polyurethane elastomer can be obtained by simply stirring the solution, evacuating the bubbles and heating to cure it. The operation steps are simple and the process flow is short. The obtained transparent antistatic polyurethane elastomer has high stability and is suitable for industrial production.
[0085] In the embodiments of the present disclosure, the electrostatic dissipation performance of the transparent antistatic polyurethane elastomer prepared in Embodiment 1 and Embodiment 2 can be tested.
[0086] Figure 2 The test results of the transparent antistatic polyurethane elastomer prepared according to Example 1 are schematically shown in FIG. Figure 2 As shown in , the transparent antistatic polyurethane elastomer prepared by using diisocyanate (IPDI) has a surface resistance of the order of magnitude of 8, that is, the electrostatic dissipation performance is of the order of magnitude of 8.
[0087] Figure 3 The test results of the transparent antistatic polyurethane elastomer prepared according to Example 2 are schematically shown in FIG. Figure 3 As shown in , the transparent antistatic polyurethane elastomer prepared based on toluene-2,4-diisocyanate (TDI) has a surface resistance of the order of 10, that is, the electrostatic dissipation performance is of the order of 10.
[0088] The above test results show that the electrostatic dissipation properties of the prepared transparent antistatic polyurethane elastomer meet the preparation requirements.
[0089] In summary, the technical solution in the embodiments of the present disclosure, by introducing an internally mixed antistatic additive, can effectively reduce the generation and accumulation of static electricity on the surface of the polyurethane elastomer, thereby ensuring the antistatic stability of the transparent antistatic polyurethane elastomer.
[0090] The transparent antistatic polyurethane elastomer in the disclosed embodiment contains multiple acyl semicarbazide and carbamate groups in its hard segment structure, which are connected by alicyclic six atoms with higher flexibility. This structural design is conducive to forming a higher density hydrogen bond array, has a better energy dissipation mechanism, and the prepared transparent antistatic polyurethane elastomer has higher robustness. A crystalline polytetrahydrofuran flexible chain segment is introduced into the soft segment of the transparent antistatic polyurethane elastomer, and an acyl semicarbazide group is introduced into the hard segment. The spacing between the acyl semicarbazide groups in the hard segment is regulated by six-membered ring diisocyanate, so as to achieve the dense and orderly aggregation of the hard segment in the elastomer and the high crystallization of the soft segment. The adverse effect of the addition of antistatic agent on the physical and mechanical properties of the product is overcome, so that its surface resistance is reduced to an ideal value. Moreover, the hardness, tensile strength, elongation at break, and resilience of the transparent antistatic polyurethane elastomer prepared in the disclosed embodiment are better than those of ordinary polyurethane elastomers.
[0091] The method for preparing the transparent antistatic polyurethane elastomer in the disclosed embodiment has simple operating steps, a short overall process flow, and a high batch stability of the prepared transparent antistatic polyurethane elastomer. It is suitable for industrial production, has low cost and excellent formula.
[0092] In this exemplary embodiment, a target material is also provided. The target material can be used in the fields of automobile manufacturing, medical equipment, electronic products, construction, sporting goods, and aerospace, and the target material can be used as long as it includes a transparent antistatic polyurethane elastomer, and this exemplary embodiment does not make any special restrictions on this.
[0093] In addition, the above-mentioned figures are only schematic illustrations of the processes included in the method according to the exemplary embodiments of the present disclosure, and are not intended to be limiting. It is easy to understand that the processes shown in the above-mentioned figures do not indicate or limit the time sequence of these processes. In addition, it is also easy to understand that these processes can be performed synchronously or asynchronously, for example, in multiple modules.
[0094] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing the invention disclosed herein. This application is intended to cover any modification, use or adaptation of the present disclosure, which follows the general principles of the present disclosure and includes common knowledge or customary techniques in the art that are not disclosed in the present disclosure. The specification and examples are intended to be exemplary only, and the true scope and spirit of the present disclosure are indicated by the appended claims.
[0095] It should be understood that the present disclosure is not limited to the exact structures that have been described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof. The scope of the present disclosure is limited only by the appended claims.
Claims
1. A transparent antistatic polyurethane elastomer, characterized in that: The components of the transparent antistatic polyurethane elastomer include isocyanate, polyol / amine, chain extender and antistatic additive.
2. The transparent antistatic polyurethane elastomer according to claim 1, characterized in that: The component ratio of the antistatic additive includes: 60% of a quaternary ammonium salt cationic surfactant with a hydroxyl functional group at the end, 20% of tri-n-butylmethylammonium bis(trifluoromethanesulfonyl)imide salt and 20% of polyethylene glycol with a molecular weight of 600.
3. The transparent antistatic polyurethane elastomer according to claim 1, characterized in that: The isocyanate is a six-membered ring diisocyanate.
4. The transparent antistatic polyurethane elastomer according to claim 1, characterized in that: The polyol / amine is hydroxy-terminated polytetrahydrofuran with different molecular weights.
5. The transparent antistatic polyurethane elastomer according to claim 1, characterized in that: The chain extender is adipic acid dihydrazide.
6. A method for preparing a transparent antistatic polyurethane elastomer, characterized in that: include: Add polyol / amine into the flask, heat and stir in a vacuum environment to remove water vapor in the solvent; After the reaction system is cooled to the first temperature, a mixture of isocyanate and dibutyltin dilaurate is dissolved in N,N-dimethylacetamide solution and added to the flask through a syringe, the reaction system is heated and stirred under a nitrogen environment, and then cooled to a second temperature after heating and stirring; Dissolve the chain extender in N,N-dimethylacetamide solution, add it into the reaction system, react and stir under nitrogen environment to obtain a viscous transparent solution; adding an antistatic additive to the viscous transparent solution and mechanically stirring the solution at room temperature to obtain a polymer solution; The polymer solution is poured into an organic glass mold, vacuumed to remove bubbles, and heated and cured to obtain a transparent antistatic polyurethane elastomer.
7. The method for preparing a transparent antistatic polyurethane elastomer according to claim 6, characterized in that: The heating temperature of the polyol / amine is 90° C.-110° C., and the stirring time is 20-30 minutes.
8. The method for preparing a transparent antistatic polyurethane elastomer according to claim 6, characterized in that: The first temperature is 75°C-85°C, and the second temperature is 35°C-45°C.
9. The method for preparing a transparent antistatic polyurethane elastomer according to claim 6, characterized in that: The mechanical stirring time is 12-15 hours.
10. The method for preparing a transparent antistatic polyurethane elastomer according to claim 6, characterized in that: The time for vacuuming and removing bubbles is 5-10 minutes, the heating temperature during the heating and curing process is 70° C.-80° C., and the curing time is 2-3 hours.
Citation Information
Cited By
Anti-static high-temperature-resistant polyurethane microporous elastomer and preparation method thereof
CN119331213A
Antistatic and high-temperature resistant polyurethane microporous elastomer and its preparation method
CN119331213B