Inorganic resin heat insulation coating as well as preparation method and application thereof

By combining modified inorganic resin and cesium tungsten nanopowder, combined with modified silicon acrylic emulsion and polyvinylpyrrolidone, the infrared barrier rate and storage stability of inorganic resin insulation coatings are solved, and high-efficiency insulation effect is achieved and cost-optimized, suitable for electrostatic filming.

CN118978819AActive Publication Date: 2024-11-19SHANGHAI YISAI NEW MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411457278.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-11-19
Estimated Expiration
2044-10-18

AI Technical Summary

Technical Problem

The existing inorganic resin thermal insulation coatings have limitations in thermal insulation performance, flexibility and storage stability, especially the low infrared barrier rate, which makes it difficult to meet the efficient thermal insulation needs of electrostatic films.

Method used

By combining modified inorganic resin and cesium oxide tungsten nanopowder, combined with modified silicon acrylic emulsion and polyvinylpyrrolidone, the dispersion and film formation properties of the material are regulated, the infrared barrier rate and storage stability of the coating are improved, and the coating is stored through Specific process steps and raw material proportions are optimized to form high-efficiency thermal insulation coatings.

Benefits of technology

It achieves low transmittance, excellent heat insulation effect and good storage stability, improves the hardness, wear resistance and weather resistance of the coating, and reduces the cost of raw materials, and is suitable for the field of electrostatic filming.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention belongs to the technical field of coating compositions, and provides an inorganic resin heat insulation coating and a preparation method and application thereof, the heat insulation coating comprises the following raw materials by weight: 40-60 parts of modified inorganic resin, 15-25 parts of modified cesium tungsten oxide slurry, 4-8 parts of a coalescing agent, 2-6 parts of an ultraviolet light absorber, 0.5-1 part of a bactericide, and 0.1-0.4 part of an antifoaming agent. The heat insulation coating is low in transmittance, good in toughness and storage stability, excellent in heat insulation effect and capable of being used in the field of electrostatic film pasting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coating compositions, and in particular relates to an inorganic resin heat-insulating coating and a preparation method and application thereof. Background Art

[0002] As global energy consumption continues to increase, the demand for lightweight and efficient thermal insulation materials is also rising. Electrostatic film is a thin film that uses the principle of electrostatic adsorption to fix on the surface of an object. As a material widely used in many fields such as construction and agriculture, the optimization of its thermal insulation performance becomes particularly important. Although traditional electrostatic films have good lightness and flexibility, they are insufficient in thermal insulation performance, which limits their effectiveness in specific application scenarios. Thermal insulation coating is a new type of coating that absorbs and shields near-infrared light and ultraviolet light. It can increase the thermal insulation effect of electrostatic film and achieve the purpose of energy saving and consumption reduction, which is of great significance. The electrostatic film coated with thermal insulation coating of the present invention has excellent thermal insulation effect, is widely used in transparent scene sun protection, heat insulation and heat preservation, and can be used in construction, automobiles, greenhouses, cultural tourism and other fields.

[0003] With the advancement of technology, thermal insulation coatings are developing in a more efficient and environmentally friendly direction. Among them, inorganic resins, as a new type of polymer material, have excellent heat resistance, chemical corrosion resistance, high mechanical strength and good electrical insulation properties. In recent years, with the development of materials science, the application of inorganic resins in the field of coatings has gradually increased, especially in the preparation of thermal insulation coatings, showing great potential. However, existing inorganic resin thermal insulation coatings still have certain limitations in terms of thermal insulation performance, flexibility and storage stability.

[0004] Chinese patent CN 110511670 A discloses a coating composition with heat insulation and anti-fouling functions prepared from a non-easy-to-clean resin. The coating uses an easy-to-clean modified additive to solve the cleaning problem and reduce the production cost of the coating composition. In addition, since the polysilazane material is abandoned, the problems of the coating being brittle due to polysilazane, insufficient heat insulation due to too thin a coating, and slight whitening during coating are also solved. However, the infrared blocking rate of this coating composition is still low.

[0005] Therefore, there is an urgent need to develop an inorganic resin thermal insulation coating with a high infrared blocking rate so that it can have excellent thermal insulation effect when coated on an electrostatic film. Summary of the invention

[0006] In view of the existing technical problems, the purpose of the present invention is to provide an inorganic resin thermal insulation coating and a preparation method thereof. The thermal insulation coating of the present invention has low transmittance, good toughness and storage stability, and excellent thermal insulation effect, and is used in the field of electrostatic film.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows: The present invention first provides an inorganic resin thermal insulation coating, which comprises the following raw materials in parts by weight: 40-60 parts of modified inorganic resin, 15-25 parts of modified cesium tungsten oxide slurry, 4-8 parts of film-forming aid, 2-6 parts of ultraviolet absorber, 0.5-1 parts of bactericide, and 0.1-0.4 parts of defoaming agent.

[0008] The reaction mechanism and effects of the present invention are as follows:

[0009] 1. Silicon-based inorganic resins generally have excellent thermal stability and can maintain their physical and chemical properties at high temperatures, making them suitable for applications that require high temperature resistance. However, inorganic resins have poor storage stability and are prone to problems such as precipitation, stratification, and gelation.

[0010] The present invention mixes organic alkoxysilane, silica sol and organic solvent and adjusts the ratio of the three, so that the inorganic resin formed has the function of enhancing mechanical properties; further, the inorganic resin is modified to introduce side chains with polar functional groups, which can produce a charge effect, inhibit the self-polymerization process of the silica sol through electrostatic repulsion, and improve the storage stability of the silica sol; at the same time, the side chains grafted to the surface of the silica sol and not participating in the reaction can hinder the contact between particles due to steric hindrance before the silica sol is solidified, thereby improving the stability of the silica sol and further improving the storage stability of the inorganic resin coating.

[0011] More importantly, the surface energy of silica sol is relatively high, and during the dehydration condensation curing film formation process, a large internal stress will be generated, which can easily cause the coating to crack. The addition of modified silicone-acrylic emulsion can make up for its shortcomings and improve the film-forming performance. In addition, the modified silicone-acrylic emulsion prepared in this application not only has the characteristics of pure acrylic emulsion, but also improves the hardness, wear resistance, tensile strength, water resistance, acid and alkali resistance, and weather resistance of the thermal insulation coating.

[0012] 2. Cesium tungsten oxide nanopowder has a high specific surface area and surface energy, which makes it difficult to disperse evenly in inorganic resins. If the dispersion is uneven, gaps may appear on the interface of the resin material, which will increase the chance of water entering the gaps. The penetration of water will cause the resin material to gradually decompose and become brittle, and its performance will decrease.

[0013] The present invention selects a specific amount of sorbitol to modify the cesium tungsten oxide nanopowder, which can improve the dispersibility and stability of the cesium tungsten oxide nanopowder and improve the thermal insulation performance of the resin. Furthermore, polyvinyl pyrrolidone is introduced to prevent further agglomeration of nanoparticles, thereby obtaining a more uniform thermal insulation coating; at the same time, polyvinyl pyrrolidone can improve the rheological properties of the thermal insulation coating, so that the coating has better coating performance during construction, and is easy to form a uniform coating film, thereby improving the overall adhesion, hardness, water resistance and thermal insulation of the coating.

[0014] In addition, cesium tungsten oxide nanopowder has a strong infrared blocking effect, but its price is relatively high; antimony tin oxide nanopowder has a narrow infrared shielding range, but its price is low. This application studies and regulates the mass ratio of modified cesium tungsten oxide nanopowder and antimony tin oxide nanopowder to meet the requirements of infrared blocking rate and visible light transmittance without affecting the raw material usage cost.

[0015] In some embodiments, the method for preparing the modified inorganic resin comprises the following steps: (1) Mixing organic alkoxysilane, organic solvent and silica sol, heating to 40-50°C, stirring for 30-60 minutes, and evacuating to obtain an inorganic resin; (2) Add silica sol and organic acid to a reaction kettle, heat to 65-80°C, keep warm for reaction for 1-1.5 hours, add the mixture of inorganic resin and deionized water obtained in step (1), and continue to keep warm for reaction for 1-2 hours; wait for the reaction kettle to cool to 50-60°C, add silane coupling agent dropwise while stirring, keep warm for reaction for another 1.5-2.5 hours, cool, add modified silicone-acrylic emulsion, stir for 1-2 hours, and obtain modified inorganic resin.

[0016] In some embodiments, the mass ratio of the organic alkoxysilane to the silica sol in step (1) is 1:(0.5-0.7).

[0017] In some embodiments, in step (2), the mass ratio of silica sol, inorganic resin and modified silicone acrylic emulsion is (1.8-2.6):1:(0.5-0.65).

[0018] In some embodiments, the method for preparing the modified silicone acrylic emulsion comprises the following steps: A1. Methyl methacrylate, butyl acrylate and acrylic acid were mixed to obtain a mixture 1; methyl methacrylate, butyl acrylate, acrylic acid and vinyl silicone oil were mixed to obtain a mixture 2; A2. Sodium dodecyl sulfate, nonylphenol polyoxyethylene ether OP-10, deionized water and ammonia water are mixed, heated to 75-85°C while stirring, potassium persulfate is added, mixture 1 obtained in step A1 is added dropwise, the addition time is controlled to be 1.5-2.5h, the reaction is kept warm for 0.5-1h, and mixture 2 obtained in step A1 is added dropwise, the addition time is controlled to be 2-2.5h, the reaction is kept warm for 2-3h, cooled, filtered and discharged to obtain a modified silicone acrylic emulsion.

[0019] Preferably, in the mixture 1 in step A1, the mass ratio of methyl methacrylate, butyl acrylate and acrylic acid is 1:1:(0.4-0.6); in the mixture 2, the mass ratio of methyl methacrylate, butyl acrylate, acrylic acid and vinyl silicone oil is 1:1:(0.4-0.6):(0.4-0.6).

[0020] Preferably, the mass ratio of sodium dodecyl sulfate, nonylphenol polyoxyethylene ether OP-10, deionized water and 20wt%-28wt% ammonia water in step A2 is 1:(1-2):(15-20):(0.05-0.15).

[0021] Preferably, the amount of potassium persulfate added in step A2 is 1.2-2.5% of the total mass of sodium dodecyl sulfate, nonylphenol polyoxyethylene ether OP-10, deionized water and ammonia water.

[0022] In some embodiments, the method for preparing the modified cesium tungsten oxide nano-slurry comprises the following steps: S1. Add cesium tungsten oxide nanopowder, deionized water, sorbitol and sodium hydroxide into a reactor, stir, disperse by ball milling and dry to obtain modified cesium tungsten oxide nanopowder; S2. The modified cesium tungsten oxide nanopowder, antimony tin oxide nanopowder and deionized water obtained in step S1 are mixed and ball-milled, polyvinyl pyrrolidone is added, stirred for 1-2 hours, and ultrasonicated for 20-30 minutes to obtain modified cesium tungsten oxide nanoslurry.

[0023] In some embodiments, the mass ratio of the cesium tungsten oxide nanopowder to sorbitol in step S1 is 1:(0.05-0.1).

[0024] In some embodiments, the mass ratio of the modified cesium tungsten oxide nanopowder, antimony tin oxide nanopowder and polyvinyl pyrrolidone in step S2 is 1: (0.4-0.6): (0.05-0.15).

[0025] In some embodiments, the film-forming aid is any one or more of trimethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, 3-aminopropyltrimethoxysilane and 3-aminopropyltriethoxysilane.

[0026] Preferably, the film-forming aid is 3-aminopropyltrimethoxysilane and / or 3-aminopropyltriethoxysilane.

[0027] Preferably, the particle size of the cesium tungsten oxide powder is 35-55 nm.

[0028] In some embodiments, the defoaming agent is a silicone defoaming agent.

[0029] The present invention also provides a method for preparing an inorganic resin thermal insulation coating, comprising the following steps: The modified inorganic resin, the modified cesium tungsten oxide slurry, the film-forming aid, the ultraviolet absorber, the bactericide and the defoamer are mechanically blended to obtain the heat-insulating coating.

[0030] The third aspect of the present invention provides an application of an inorganic resin heat-insulating coating in the field of electrostatic film, and the preparation method of the electrostatic film comprises the following steps: 1. Apply the thermal insulation coating to the upper surface of the substrate layer using a coating machine, adjust the thickness, and dry to obtain a thermal insulation coating layer; 2. Apply corona to the substrate layer with the thermal insulation coating layer obtained in step 1 to obtain an electrostatic film.

[0031] Preferably, the substrate layer of the electrostatic film is a PET substrate layer or a PP substrate layer.

[0032] Further preferably, the PP substrate layer comprises at least two layers: one layer is an insulating layer for preventing static electricity leakage; and one layer is a base layer for carrying static electricity.

[0033] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0034] 1. The thermal insulation coating of the present invention has low transmittance, good toughness and storage stability, excellent thermal insulation effect, and can be used in the field of electrostatic film.

[0035] 2. The modified inorganic resin of the present invention has good storage stability and excellent film-forming performance. The introduced modified silicone acrylic emulsion not only makes up for the coating cracking problem that may be caused by internal stress of silica sol, but also improves the hardness, wear resistance, tensile strength, water resistance, acid and alkali resistance and weather resistance of the thermal insulation coating.

[0036] 3. The present invention uses specific sorbitol and polyvinyl pyrrolidone to modify the cesium tungsten oxide nanopowder, so that it is stably and evenly dispersed in the inorganic resin, thereby improving the overall performance of the thermal insulation coating. At the same time, the present application has regulated the mass ratio of the modified cesium tungsten oxide nanopowder and the antimony tin oxide nanopowder through research, so that the infrared blocking rate and visible light transmittance are not affected, and the cost of raw materials is low. DETAILED DESCRIPTION

[0037] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, rather than to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0038] The thermal insulation coatings were prepared according to the proportions of the raw materials and the preparation methods specified in the following examples and comparative examples.

[0039] In order to facilitate those skilled in the art to implement the present invention, some raw material manufacturers of the embodiments and comparative examples are described as follows: Cesium tungsten oxide nanopowder: purchased from Hangzhou Jikang New Materials Co., Ltd., particle size 40 nm; Silicone defoamer: purchased from Hunan Jiaxinzhi New Material Technology Co., Ltd., model BYK-141; Polydiallyldimethylammonium chloride: purchased from Jinan Zhendong Chemical Co., Ltd. Other raw materials are not specially specified and can be purchased from the market.

[0040] Preparation Example 1 The preparation method of modified silicone acrylic emulsion A comprises the following steps: A1. 20 g of methyl methacrylate, 20 g of butyl acrylate and 10 g of acrylic acid were mixed to obtain a mixture 1; 20 g of methyl methacrylate, 20 g of butyl acrylate, 10 g of acrylic acid and 10 g of vinyl triethoxysilane were mixed to obtain a mixture 2; A2. Mix 1.4g of sodium dodecyl sulfate, 2.1g of nonylphenol polyoxyethylene ether OP-10, 25.2g of deionized water, and 0.14g of 25wt% ammonia water, heat to 80°C while stirring, add 0.6g of potassium persulfate, add dropwise the mixture 1 obtained in step A1, control the dropping time to 2h, keep the temperature for reaction for 45min, then add dropwise the mixture 2 obtained in step A1, control the dropping time to 2.5h, keep the temperature for reaction for another 2.5h, cool to room temperature, filter the material, and obtain modified silicone acrylic emulsion A.

[0041] Preparation Example 2 The preparation method of modified silicone acrylic emulsion B is the same as that of Preparation Example 1, except that the amount of vinyltriethoxysilane added in step A1 is 6 g.

[0042] Preparation Example 3 The preparation method of modified inorganic resin A comprises the following steps: (1) 10 g of methyltriethoxysilane, 4 g of ethanol, 2 g of isopropanol, and 6 g of silica sol were mixed, heated to 50°C, stirred for reaction for 45 min, and vacuumed for 5 min to obtain an inorganic resin; (2) Add 11 g of silica sol and 2 g of tartaric acid to a reaction kettle, heat to 75°C, keep warm for 1 h, add a mixture of 5 g of inorganic resin obtained in step (1) and 4 g of deionized water, and continue to keep warm for 2 h; after the reaction kettle is cooled to 55°C, add 1 g of silane coupling agent KH-560 dropwise while stirring, keep warm for another 2 h, cool to room temperature, add 3 g of modified silicone-acrylic emulsion A, and stir for 1.5 h to obtain modified inorganic resin A.

[0043] Preparation Example 4 The preparation method of modified inorganic resin B is the same as that of Preparation Example 3, except that the amount of silica sol added in step (1) is 4 g.

[0044] Preparation Example 5 The preparation method of modified inorganic resin C is the same as that of Preparation Example 3, except that the amount of modified silicone acrylic emulsion A added in step (1) is 2 g.

[0045] Preparation Example 6 The preparation method of modified inorganic resin D is the same as that of Preparation Example 3, except that modified silicone acrylic emulsion B is used instead of modified silicone acrylic emulsion A in step (2).

[0046] Preparation Example 7 The preparation method of the modified inorganic resin E comprises the following steps: (1) 10 g of methyltriethoxysilane, 4 g of ethanol, 2 g of isopropanol, and 6 g of silica sol were mixed, heated to 50°C, stirred for reaction for 45 min, and vacuumed for 5 min to obtain an inorganic resin; (2) Add 11 g of silica sol and 2 g of tartaric acid to a reaction kettle, heat to 75°C, and keep the temperature for reaction for 1 h. Add a mixture of 5 g of inorganic resin obtained in step (1) and 4 g of deionized water, and continue to keep the temperature for reaction for 2 h. After the temperature of the reaction kettle drops to 55°C, add 1 g of silane coupling agent KH-560 dropwise while stirring, keep the temperature for reaction for another 2 h, and cool to room temperature to obtain modified inorganic resin E.

[0047] Preparation Example 8 The preparation method of modified cesium tungsten oxide nano-slurry A comprises the following steps: S1. 10 g of cesium tungsten oxide nanopowder, 20 g of deionized water, 0.8 g of sorbitol, and 0.2 g of a 20 wt% aqueous sodium hydroxide solution were added to a reactor, stirred for 30 min, ball-milled for 1 h, and dried at 60 ° C for 4 h to obtain modified cesium tungsten oxide nanopowder; S2. 6 g of modified cesium tungsten oxide nanopowder, 3 g of antimony tin oxide nanopowder and 20 g of deionized water obtained in step S1 were mixed and ball-milled for 3 h, 0.72 g of polyvinyl pyrrolidone was added, stirred for 1.5 h, and ultrasonicated for 30 min to obtain modified cesium tungsten oxide nano-slurry A.

[0048] Preparation Example 9 The preparation method of modified cesium oxide tungsten nano-slurry B is the same as that of Preparation Example 1, except that the amount of sorbitol added is 1.2 g.

[0049] Preparation Example 10 The preparation method of modified cesium tungsten oxide nano-slurry C comprises the following steps: S1. 10 g of cesium tungsten oxide nanopowder, 20 g of deionized water, 0.8 g of sorbitol, and 0.2 g of a 20 wt% aqueous sodium hydroxide solution were added to a reactor, stirred for 30 min, ball-milled for 1 h, and dried at 60 ° C for 4 h to obtain modified cesium tungsten oxide nanopowder; S2. 6 g of the modified cesium tungsten oxide nanopowder obtained in step S1 and 20 g of deionized water were mixed and ball-milled for 3 h, 0.72 g of polyvinyl pyrrolidone was added, stirred for 1.5 h, and ultrasonicated for 30 min to obtain modified cesium tungsten oxide nano-slurry C.

[0050] Example 1

[0051] A thermal insulation coating of an inorganic resin comprises the following raw materials, measured in parts by weight: 50 parts of a modified inorganic resin A, 20 parts of a modified cesium tungsten oxide slurry A, 6 parts of 3-aminopropyltrimethoxysilane, 4 parts of 2,4-dihydroxybenzophenone, 0.75 parts of polydiallyldimethylammonium chloride, and 0.25 parts of an organosilicon defoamer BYK-141.

[0052] The preparation method of the thermal insulation coating of this embodiment comprises the following steps: The modified inorganic resin A, the modified cesium tungsten oxide slurry A, 3-aminopropyltrimethoxysilane, 2,4-dihydroxybenzophenone, polydiallyldimethylammonium chloride and the silicone defoamer BYK-141 are mechanically blended to obtain a thermal insulation coating.

[0053] Example 2

[0054] A thermal insulation coating of an inorganic resin comprises the following raw materials, measured in parts by weight: 40 parts of a modified inorganic resin A, 15 parts of a modified cesium tungsten oxide slurry A, 4 parts of 3-aminopropyltrimethoxysilane, 2 parts of 2,4-dihydroxybenzophenone, 0.5 parts of polydiallyldimethylammonium chloride, and 0.1 parts of an organosilicon defoamer BYK-141.

[0055] The preparation method of the thermal insulation coating of this embodiment is the same as that of Example 1.

[0056] Example 3

[0057] A thermal insulation coating of an inorganic resin comprises the following raw materials, measured by weight: 60 parts of a modified inorganic resin A, 25 parts of a modified cesium tungsten oxide slurry A, 8 parts of 3-aminopropyltriethoxysilane, 6 parts of 2,4-dihydroxybenzophenone, 1 part of polydiallyldimethylammonium chloride, and 0.4 parts of an organosilicon defoamer BYK-141.

[0058] The preparation method of the thermal insulation coating of this embodiment is the same as that of Example 1.

[0059] Example 4

[0060] An inorganic resin heat-insulating coating and a preparation method thereof, wherein the specific implementation manner is the same as that of Example 1, except that an equal amount of modified inorganic resin B is used to replace modified inorganic resin A.

[0061] Example 5

[0062] An inorganic resin heat-insulating coating and a preparation method thereof, wherein the specific implementation manner is the same as that of Example 1, except that an equal amount of modified inorganic resin C is used to replace modified inorganic resin A.

[0063] Example 6

[0064] An inorganic resin heat-insulating coating and a preparation method thereof, wherein the specific implementation manner is the same as that of Example 1, except that an equal amount of modified inorganic resin D is used to replace modified inorganic resin A.

[0065] Example 7

[0066] An inorganic resin heat-insulating coating and a preparation method thereof, wherein the specific implementation manner is the same as that of Example 1, except that an equal amount of modified inorganic resin E is used to replace modified inorganic resin A.

[0067] Example 8

[0068] An inorganic resin heat-insulating coating and a preparation method thereof, wherein the specific implementation manner is the same as that of Example 1, except that an equal amount of modified cesium tungsten oxide slurry B is used to replace modified cesium tungsten oxide slurry A.

[0069] Example 9

[0070] An inorganic resin heat-insulating coating and a preparation method thereof, wherein the specific implementation manner is the same as that of Example 1, except that an equal amount of modified cesium tungsten oxide slurry C is used to replace modified cesium tungsten oxide slurry A.

[0071] Comparative Example 1 An inorganic resin heat-insulating coating and a preparation method thereof, wherein the specific implementation manner is the same as that of Example 1, except that an equal amount of commercially available potassium silicate is used to replace the modified inorganic resin A.

[0072] Comparative Example 2 An inorganic resin heat-insulating coating and a preparation method thereof, wherein the specific implementation manner is the same as that of Example 1, except that an equal amount of commercially available cesium tungsten oxide nanopowder is used to replace the modified cesium tungsten oxide slurry A.

[0073] Effect evaluation: The thermal insulation coatings prepared in the above-mentioned Examples 1-9 and Comparative Examples 1-2 were tested and analyzed, and the specific results are shown in Table 1.

[0074] Performance Testing: (1) The sample was applied on an electrostatic film and cured at 60°C for 2 hours to make the dry film coating thickness 6 μm. The infrared blocking rate and visible light transmittance of the electrostatic film coating were tested using an LS182 optical transmittance measuring instrument; (2) The coating is qualified if there is no caking, coagulation or mildew when tested for 30 days of thermal storage stability according to standard JG / T26-2002.

[0075] Table 1

[0076] From the results in Table 1, it can be seen that the thermal insulation coatings prepared in Examples 1-3 have good infrared blocking rate, visible light transmittance and thermal storage stability, thus making them have better thermal insulation effect.

[0077] Compared with Example 1, when preparing the modified inorganic resin, Example 4 changes the mass ratio of organic alkoxysilane, organic solvent and silica sol, and Example 5 changes the mass ratio of silica sol, inorganic resin and modified silicone-acrylic emulsion, which affects the uniformity of the final coating; Example 6 changes the type of modified silicone-acrylic emulsion, and Example 7 does not add modified silicone-acrylic emulsion to modify the inorganic resin, which may cause cracking of the coating and poor toughness. Comparative Example 1 uses an equal amount of commercially available potassium silicate to replace the modified inorganic resin A, which has poor dispersion stability, thereby affecting the infrared blocking rate, visible light transmittance and thermal storage stability.

[0078] Compared with Example 1, when preparing the modified cesium tungsten oxide nano-slurry, Examples 8-9 and Comparative Example 2 changed the mass ratio of cesium oxide tungsten nano-powder and sorbitol in Example 8, which affected the compatibility of cesium oxide tungsten nano-powder with the resin, and Example 9 changed the mass ratio of modified cesium oxide tungsten nano-powder, antimony tin oxide nano-powder and polyvinyl pyrrolidone, which affected the infrared blocking rate and visible light transmittance. Comparative Example 2 used an equal amount of cesium oxide tungsten nano-powder to replace the modified cesium oxide tungsten nano-powder A, and the dispersion compatibility became worse, thereby affecting the infrared blocking rate, visible light transmittance and thermal storage stability.

[0079] (3) Application testing

[0080] The thermal insulation coating prepared in Examples 1-3 was applied to the electrostatic film for testing. The thermal insulation coating prepared in Examples 1-3 was applied to the upper surface of the PP substrate layer using a coating machine, the thickness was adjusted to 40 µm, and baked at 70°C for 5 minutes to obtain a thermal insulation coating layer. The PP substrate layer with the thermal insulation coating layer was subjected to corona treatment to obtain an electrostatic film.

[0081] Adhesion test: In an environment with a temperature of 23±2℃ and a relative humidity of 50±5%, use a grid knife to cut a 2cm×2cm incision on the coating surface. The incision penetrates the entire thermal insulation coating layer. Use a soft brush to gently brush along the incision direction to ensure that there are no residual fragments under the coating. Stick 3M610 tape on the cut grid pattern to ensure that the tape is in full contact with the coating surface. After 2 minutes, quickly tear off the tape at an angle of about 60°, observe and evaluate the shedding of the coating, and rate the results according to ASTM standards.

[0082] The test shows that the thermal insulation coating layer prepared in Examples 1-3 has only very small flakes at the intersection of the cuts, the actual damage in the grid area does not exceed 5%, and the ASTM grade is not less than 4B. It can be seen that the thermal insulation coating has good adhesion and can be well used in electrostatic film.

[0083] The above is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present application. Although the present application is disclosed as above in the preferred embodiment, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases. However, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution.

Claims

1. A thermal insulation coating of an inorganic resin, characterized in that: The thermal insulation coating comprises the following raw materials by weight: 40-60 parts of modified inorganic resin, 15-25 parts of modified cesium tungsten oxide slurry, 4-8 parts of film-forming aid, 2-6 parts of ultraviolet absorber, 0.5-1 parts of bactericide, and 0.1-0.4 parts of defoamer; The preparation method of the modified inorganic resin comprises the following steps: (1) Mixing organic alkoxysilane, organic solvent and silica sol, heating to 40-50°C, stirring for 30-60 minutes, and evacuating to obtain an inorganic resin; (2) Add silica sol and organic acid to a reaction kettle, heat to 65-80°C, keep warm for 1-1.5 hours, add the mixture of inorganic resin and deionized water obtained in step (1), and continue to keep warm for 1-2 hours; wait for the reaction kettle to cool to 50-60°C, add silane coupling agent dropwise while stirring, keep warm for another 1.5-2.5 hours, cool, add modified silicone-acrylic emulsion, stir for 1-2 hours, and obtain modified inorganic resin; The preparation method of the modified cesium tungsten oxide nano-slurry comprises the following steps: S1. Add cesium tungsten oxide nanopowder, deionized water, sorbitol and sodium hydroxide into a reactor, stir, disperse by ball milling and dry to obtain modified cesium tungsten oxide nanopowder; S2. The modified cesium tungsten oxide nanopowder, antimony tin oxide nanopowder and deionized water obtained in step S1 are mixed and ball-milled, polyvinyl pyrrolidone is added, stirred for 1-2 hours, and ultrasonicated for 20-30 minutes to obtain a modified cesium tungsten oxide nanoslurry; wherein the mass ratio of the modified cesium tungsten oxide nanopowder, antimony tin oxide nanopowder and polyvinyl pyrrolidone is 1: (0.4-0.6): (0.05-0.15).

2. The inorganic resin thermal insulation coating according to claim 1, characterized in that: The mass ratio of the organic alkoxysilane to the silica sol in step (1) is 1:(0.5-0.7).

3. The inorganic resin thermal insulation coating according to claim 1, characterized in that: In step (2), the mass ratio of silica sol, inorganic resin and modified silicone acrylic emulsion is (1.8-2.6):1:(0.5-0.65).

4. The inorganic resin thermal insulation coating according to claim 1, characterized in that: The mass ratio of the cesium tungsten oxide nanopowder to sorbitol in step S1 is 1:(0.05-0.1).

5. The inorganic resin thermal insulation coating according to claim 1, characterized in that: In parts by weight, the film-forming aid is any one or more of trimethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, 3-aminopropyltrimethoxysilane and 3-aminopropyltriethoxysilane.

6. A method for preparing the inorganic resin thermal insulation coating according to any one of claims 1 to 5, characterized in that: The following steps are included: The modified inorganic resin, the modified cesium tungsten oxide slurry, the film-forming aid, the ultraviolet absorber, the bactericide and the defoamer are mechanically blended to obtain the heat-insulating coating.

7. An application of the inorganic resin thermal insulation coating according to any one of claims 1 to 5 in the field of electrostatic film application, characterized in that: The preparation method of the electrostatic film comprises the following steps:

1. Apply the thermal insulation coating to the upper surface of the substrate layer using a coating machine, adjust the thickness, and dry to obtain a thermal insulation coating layer; 2. Apply corona to the substrate layer with the thermal insulation coating layer obtained in step 1 to obtain an electrostatic film.

Citation Information

Patent Citations

  • Organic-inorganic compound modified water-based acrylic resin and preparation method thereof

    CN104558450A

  • Lithium silicate interior and exterior wall coating and preparation method thereof

    CN114716852A

  • Energy-saving heat-insulating coating and preparation method thereof

    CN118126616A

  • Heat insulation coating based on cesium tungsten oxide and preparation method and application thereof

    CN118667417A

  • Insulation coating agent for blocking solar heat

    KR101447280B1