Piezoelectric super-hydrophobic double-layer antifouling coating as well as preparation method and application thereof
By designing a piezoelectric superhydrophobic double-layer antifouling coating, the piezoelectric bottom layer kills microorganisms, while the superhydrophobic surface layer reduces attachment sites, thus solving the problems of toxicity and insufficient antifouling effect of traditional marine antifouling coatings and achieving an environmentally friendly and long-lasting antifouling effect.
Patent Information
- Application Number
- CN202411062542.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-05
AI Technical Summary
Existing marine antifouling coatings have toxicity issues, and superhydrophobic coatings are difficult to meet antifouling requirements in marine environments and cannot effectively prevent marine organisms from attaching.
A piezoelectric superhydrophobic dual-layer antifouling coating is adopted, including a piezoelectric bottom layer and a superhydrophobic surface layer. The piezoelectric bottom layer kills attached microorganisms, while the superhydrophobic surface layer reduces attachment sites. Through a layer-by-layer spraying process combined with piezoelectric catalysis and micro-nano structure layers, sterilization and antifouling are achieved.
Without adding toxic substances, it effectively prevents marine organisms from adhering, extends the service life of the coating, and has environmentally friendly and excellent antifouling properties.
Smart Images

Figure CN118978845A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of marine antifouling coatings, and in particular to a piezoelectric super-hydrophobic double-layer antifouling coating and a preparation method and application thereof. Background Art
[0002] Ships, offshore platforms and other facilities are important components of marine transportation and marine exploration. When these offshore facilities are in contact with seawater for a long time, a large number of marine organisms often attach to their surfaces, causing marine biofouling. This attachment can have a serious impact on the equipment. Harmful attachments can increase the surface roughness of the hull and fuel consumption, accelerate the corrosion of underwater facilities, and shorten their service life. Polluting organisms attached to the surface of ships may also cause the invasion of alien species and destroy the ecological balance. Therefore, preventing marine pollution is of great significance to the exploration and utilization of marine resources.
[0003] Traditional marine antifouling coatings contain toxic materials. Traditional marine antifouling coatings release toxic materials at a certain speed to form a toxic environment to prevent marine organisms from attaching. Obviously, with the continuous release of antifouling agents, the antifouling effect will gradually decrease. Although traditional marine antifouling coatings play a certain role in antifouling, they also cause certain harm to the marine environment and marine organisms.
[0004] In addition, some researchers have proposed green and safe super-hydrophobic coatings. For example, the Chinese invention patent application with application number 201710504936.1 discloses "a method for preparing a nano zinc oxide epoxy resin composite super-hydrophobic coating". The super-hydrophobic coating is prepared by nano zinc oxide, epoxy resin and other materials. The super-hydrophobic coating has excellent super-hydrophobic properties. However, in the marine environment, offshore industrial facilities are immersed in seawater for a long time. Therefore, the requirements for anti-fouling coatings for offshore industrial facilities are more stringent. It is difficult to meet the anti-fouling requirements by only using super-hydrophobic coatings to control the hydrophobicity of the substrate of offshore industrial facilities. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a piezoelectric super-hydrophobic double-layer antifouling coating and a preparation method and application thereof. The present invention provides a piezoelectric super-hydrophobic double-layer antifouling coating and a preparation method and application thereof. The obtained piezoelectric super-hydrophobic double-layer antifouling coating can not only reduce the attachment sites of organisms on the coating through the super-hydrophobic surface layer, but also can generate charges through the piezoelectric bottom layer to react with water to generate active oxygen, thereby achieving sterilization and antifouling properties.
[0006] To achieve the above purpose, the technical solution designed by the present invention is as follows:
[0007] The invention provides a piezoelectric super-hydrophobic double-layer antifouling coating. The piezoelectric super-hydrophobic double-layer antifouling coating comprises, by weight, a piezoelectric bottom layer coated on a substrate surface and a super-hydrophobic surface layer coated on the piezoelectric bottom layer; the piezoelectric bottom layer is prepared from 114 to 130 parts of a film-forming resin, 60 to 90 parts of an inorganic piezoelectric material, 1 to 30 parts of an inorganic conductive material, 25 to 33 parts of an auxiliary agent and 42 to 53 parts of a solvent; the super-hydrophobic surface layer consists of a micro-nano structure layer and a hydrophobic layer coated on the micro-nano structure layer, the micro-nano structure layer is prepared from 22 to 39 parts of a film-forming resin, 41 to 163 parts of nano zinc oxide, 7 to 13 parts of an auxiliary agent and 52 to 162 parts of a solvent, and the hydrophobic layer is prepared from 11 to 51 parts of a low surface energy resin, 5 to 13 parts of an auxiliary agent and 52 to 162 parts of a solvent.
[0008] Compared with other technologies, the present invention adopts a layer-by-layer spray coating technology. The bottom layer kills bacteria and other microorganisms attached to the coating based on piezoelectric catalysis, and the surface layer reduces the attachment sites of large organisms on the coating based on the constructed micro-nano structure. It plays a role in preventing fouling in the two important processes of marine fouling formation. The present invention combines two anti-fouling strategies with a simple spraying process to extend the service life of the coating.
[0009] Furthermore, the piezoelectric base layer is prepared from 114 to 120 parts of a film-forming resin, 82 to 88 parts of an inorganic piezoelectric material, 3 to 17.8 parts of an inorganic conductive material, 26.8 to 28 parts of an additive and 45 to 53 parts of a solvent; the micro-nanostructure layer is prepared from 39 parts of a film-forming resin, 148 parts of nano zinc oxide, 10 to 11 parts of an additive and 137 to 162 parts of a solvent; and the hydrophobic layer is prepared from 41 parts of a low surface energy resin, 5 parts of an additive and 162 parts of a solvent.
[0010] The invention does not add toxic substances and will not release toxic materials into the ocean during use, thus having the advantage of being environmentally friendly.
[0011] Furthermore, the film-forming resin is at least one of epoxy resin, fluorocarbon resin and polyurethane resin; the auxiliary agent is at least one of dispersant, defoamer, anti-settling agent and curing agent; and the solvent is at least one of xylene, trifluorotoluene, n-hexane and toluene.
[0012] The present invention uses a resin with anti-corrosion performance as a film-forming material, and is often used in marine facilities such as ships because of its physical and chemical stability, mechanical properties and adhesion to the substrate.
[0013] Furthermore, in the piezoelectric base layer, the inorganic piezoelectric material is at least one of zinc oxide, barium titanate and tourmaline; and the inorganic conductive material is at least one of multi-walled carbon nanotubes, single-walled carbon nanotubes, silver powder, copper powder and graphene.
[0014] The present invention does not add toxic substances but adds inorganic piezoelectric materials, and uses the wave energy in the ocean to create external mechanical vibration conditions, thereby achieving the purpose of sterilization and antifouling; the present invention adds inorganic conductive materials to provide more conductive paths in the coating system to collect and transfer the charges generated by the inorganic piezoelectric materials under external mechanical vibration to the surface of the coating, thereby reacting with the water around the coating to generate more active oxygen, thereby enhancing the sterilization and antifouling properties of the coating.
[0015] Furthermore, in the piezoelectric bottom layer, the inorganic piezoelectric material is zinc oxide, and the zinc oxide is one of flower-shaped zinc oxide, four-needle zinc oxide whiskers, and zinc oxide nanowires.
[0016] The invention uses zinc oxides of different morphologies as fillers, and the coating prepared by using four-needle zinc oxide whiskers has strong piezoelectricity.
[0017] Furthermore, in the piezoelectric bottom layer, the inorganic piezoelectric material is four-needle zinc oxide whiskers.
[0018] Furthermore, the nano zinc oxide of the micro-nano structure layer is at least one of 150nm spherical zinc oxide, 100nm spherical zinc oxide, 50nm spherical zinc oxide, and 10nm spherical zinc oxide.
[0019] The present invention uses nano zinc oxide of different particle sizes to construct a micro-nano structure layer, the water contact angle of the coating is large, and the constructed super-hydrophobic surface layer can exert a better anti-fouling effect.
[0020] Furthermore, the low surface energy resin of the hydrophobic layer is at least one of silicone resin, fluorocarbon resin and fluorosilicone resin.
[0021] The present invention adopts low surface energy resin as the outermost layer of the coating, further improving the super hydrophobicity of the coating to achieve the purpose of reducing the attachment sites of large fouling organisms.
[0022] The present invention also provides a method for preparing the piezoelectric super-hydrophobic double-layer antifouling coating, comprising the following steps:
[0023] (1) Preparation of piezoelectric primer: weigh a film-forming resin, an inorganic piezoelectric material, an inorganic conductive material, an additive and a solvent by weight, and mix the components uniformly to obtain a piezoelectric primer;
[0024] (2) Preparation of super-hydrophobic surface coating: weighing film-forming resin, nano zinc oxide, additives and solvent by weight, and mixing the components to obtain a micro-nano structure layer coating; then weighing low surface energy resin, additives and solvent by weight, and mixing the components to obtain a hydrophobic layer coating;
[0025] (3) Coating of piezoelectric base layer: coating the piezoelectric base layer coating on the surface of the substrate and drying it until the surface is dry to form the piezoelectric base layer;
[0026] (4) Coating of super-hydrophobic surface layer: The micro-nano structure layer coating is evenly sprayed on the semi-dry surface of the piezoelectric bottom layer. After drying until completely dry, the hydrophobic layer coating is evenly sprayed on the micro-nano structure layer. After drying, the micro-nano structure layer and the hydrophobic layer together form a super-hydrophobic surface layer.
[0027] The present invention combines a super-hydrophobic surface layer with a piezoelectric bottom layer and utilizes the synergistic effect of the two anti-fouling strategies to achieve better anti-fouling effect and longer service life.
[0028] Furthermore, in the step 3), the drying condition is 90° C. for 25 min; in the step 4), the first drying condition is 60° C. for 50 min; and the second drying condition is 30° C. for 30 min.
[0029] The double-layer structure of the present invention uses the same film-forming resin and prepares the composite coating with a semi-dry spraying process. The slurry mixed with zinc oxide, film-forming resin and other materials used to construct the micro-nano structure is "seeded" on the semi-dry piezoelectric base layer to solve the interface problem between the double-layer coatings.
[0030] The present invention provides an antifouling application of the piezoelectric super-hydrophobic double-layer antifouling coating in the bottom topcoat of ships, offshore platforms and offshore industrial facilities.
[0031] The invention has excellent antifouling properties, is environmentally friendly, has a simple preparation process, is low-cost, is suitable for substrates of most offshore facilities, and has broad application prospects.
[0032] Principle of the present invention:
[0033] (1) A layer-by-layer spray coating technology is used. The bottom layer kills bacteria and other microorganisms attached to the coating based on piezoelectric catalysis, and the surface layer reduces the attachment sites of large organisms on the coating based on the constructed micro-nano structure. It plays a role in preventing fouling in the two important processes of marine fouling formation. The present invention combines two anti-fouling strategies with a simple spraying process to extend the service life of the coating.
[0034] (2) Based on the two anti-fouling strategies of piezoelectric catalysis and construction of micro-nanostructures, and considering that nano zinc oxide is both a piezoelectric crystal material and has the potential to construct surface micro-nanostructures, this study uses piezoelectric fillers and film-forming resins as the main body, adds conductive fillers to enhance the charge transfer capacity of the piezoelectric bottom layer so that the coating can achieve the purpose of wave response to kill microorganisms; then uses zinc oxide to construct a super-hydrophobic layer; finally, a low surface energy resin is used as the outermost layer of the coating, which further improves the super-hydrophobic properties of the coating to achieve the purpose of reducing the attachment sites of large fouling organisms.
[0035] (3) The nano zinc oxide on the surface smoothly transfers the charge generated by the piezoelectric bottom layer under the force of the waves to the surface of the coating, acting as a "bridge for charge transfer". At the same time, since zinc oxide itself has the ability of piezoelectric catalysis, the zinc oxide on the surface not only transfers the charge generated by the piezoelectric bottom layer, but also generates its own charge to the surface of the coating to react with the surrounding water and dissolved oxygen to generate superoxide free radicals, hydroxyl free radicals and other active oxygen species, thereby enhancing the piezoelectric catalytic bactericidal effect of the coating.
[0036] (4) Since the prepared coating is a double-layer structure, it is particularly important to solve the interface problem between the two layers of coating. Therefore, the double-layer structure of this study uses the same film-forming resin and uses a semi-dry spraying process to prepare the composite coating. The slurry mixed with zinc oxide, film-forming resin and other substances used to construct the micro-nano structure is "seeded" on the semi-dry piezoelectric bottom layer to solve the interface problem between the double-layer coating.
[0037] (5) The super-hydrophobic surface layer of the present invention is constructed by a micro-nano structure layer and a hydrophobic layer. Achieving a super-hydrophobic surface requires high surface roughness and low surface tension. The micro-nano structure is constructed to increase the surface roughness, and the hydrophobic layer reduces the surface tension to increase the water contact angle of the coating. Combining these two methods can effectively construct a super-hydrophobic surface. The present invention adds nano zinc oxide to the micro-nano structure layer and adds a low surface energy resin to the hydrophobic layer to achieve a super-hydrophobic effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 The piezoelectric output diagram of the piezoelectric bottom layer of samples 1 to 8 and sample 1 under 200W power ultrasound;
[0039] Figure 2 It is a summary diagram of the water contact angles of samples 1 to 8 and the piezoelectric bottom layer of sample 1;
[0040] Figure 3 It is a summary diagram of the hydroxyl radical content released by the coatings of the control group and samples 1 to 8 under ultrasound conditions over a period of time;
[0041] Figure 4 It is a summary diagram of the superoxide free radical content released by the control group and the coatings of samples 1 to 8 under ultrasound conditions over a period of time;
[0042] Figure 5 The graphs are the antibacterial test results of the control group and samples 1 to 8;
[0043] Figure 6 The anti-algae test results of the control group and sample 1 coating are shown in FIG. DETAILED DESCRIPTION
[0044] The present invention is further described in detail below in conjunction with specific embodiments so that those skilled in the art can understand.
[0045] Example 1
[0046] A method for preparing a piezoelectric super-hydrophobic double-layer antifouling coating, comprising the following steps:
[0047] (1) Preparation of piezoelectric primer: 50 parts by weight of xylene was added to a disperser, and 1.2 parts of defoamer, 1.8 parts of anti-settling agent, and 1 part of dispersant were added at a line speed of 6 m / s, and stirred for 10 min. 120 parts of epoxy resin were added at a line speed of 10 m / s, and stirred for 60 min to form a slurry. 82 parts of tetrapod-shaped zinc oxide whiskers and 3 parts of multi-walled carbon nanotubes were added and dispersed at a high power of 300 W for 30 min. After uniform dispersion, the mixture was added to a disperser, and the speed was adjusted to 6 m / s. 24 parts of curing agent were added and stirred for 5 min to obtain slurry a, i.e., piezoelectric primer.
[0048] (2) Preparation of super hydrophobic surface coating: 146 parts by weight of xylene are added to a disperser, 1 part of defoamer and 1.4 parts of anti-settling agent are added at a linear speed of 6m / s, and stirred for 10min. 39 parts of epoxy resin are added at a linear speed of 10m / s, and stirred for 20min to form a slurry. 74 parts of 100nm spherical zinc oxide and 74 parts of 10nm spherical zinc oxide are added, and dispersed for 40min with a high-power ultrasonic dispersion of 300W. After uniform dispersion, a disperser is added, the speed is adjusted to 6m / s, and 8 parts of curing agent are added and stirred for 5min to obtain slurry b, i.e., micro-nano structure layer coating.
[0049] 41 parts of silicone resin, 162 parts of n-hexane and 5 parts of curing agent were added into a disperser and stirred for 15 minutes at a linear speed of 6 m / s to obtain slurry c, i.e., a hydrophobic layer coating.
[0050] (3) Coating of piezoelectric base layer: spray the piezoelectric base layer coating evenly on the tinplate sheet and dry it at 90°C for 25 minutes until it is semi-dry to form the piezoelectric base layer.
[0051] (4) Coating of super-hydrophobic surface layer: The micro-nano structure layer coating is evenly sprayed on the semi-dry surface of the piezoelectric bottom layer. After drying at 60°C for 50 min, the hydrophobic layer coating is evenly sprayed on the micro-nano structure layer. After drying at 30°C for 30 min, the micro-nano structure layer and the hydrophobic layer together form a super-hydrophobic surface layer.
[0052] Example 2
[0053] A method for preparing a piezoelectric super-hydrophobic double-layer antifouling coating, comprising the following steps:
[0054] (1) Preparation of piezoelectric primer: 45 parts by weight of xylene was added to a disperser, and 1.5 parts of defoamer and 2.5 parts of anti-settling agent were added at a line speed of 6 m / s, and stirred for 5 min. 118 parts of epoxy resin were added at a line speed of 10 m / s, and stirred for 60 min to form a slurry. 88 parts of flower-shaped zinc oxide and 13.3 parts of copper powder were added and dispersed at a high power of 300 W for 30 min. After uniform dispersion, the mixture was added to a disperser, and the speed was adjusted to 6 m / s. 23.6 parts of curing agent were added and stirred for 5 min to obtain slurry a, i.e., piezoelectric primer.
[0055] (2) Preparation of super hydrophobic surface coating: 137 parts by weight of xylene are added to a disperser, 1 part of defoamer and 1 part of anti-settling agent are added at a linear speed of 6m / s, and stirred for 10min. 39 parts of epoxy resin are added at a linear speed of 10m / s, and stirred for 20min to form a slurry. 100 parts of 100nm spherical zinc oxide and 48 parts of 10nm spherical zinc oxide are added, and dispersed for 40min with a high-power ultrasonic dispersion of 300W. After uniform dispersion, a disperser is added, the speed is adjusted to 6m / s, and 8 parts of curing agent are added and stirred for 5min to obtain slurry b, i.e., micro-nano structure layer coating.
[0056] 41 parts of silicone resin, 162 parts of n-hexane and 5 parts of curing agent were added into a disperser and stirred for 15 minutes at a linear speed of 6 m / s to obtain slurry c, i.e., a hydrophobic layer coating.
[0057] (3) Coating of piezoelectric base layer: spray the piezoelectric base layer coating evenly on the tinplate sheet and dry it at 90°C for 25 minutes until it is semi-dry to form the piezoelectric base layer.
[0058] (4) Coating of super-hydrophobic surface layer: The micro-nano structure layer coating is evenly sprayed on the semi-dry surface of the piezoelectric bottom layer. After drying at 60°C for 50 min, the hydrophobic layer coating is evenly sprayed on the micro-nano structure layer. After drying at 30°C for 30 min, the micro-nano structure layer and the hydrophobic layer together form a super-hydrophobic surface layer.
[0059] Example 3
[0060] A method for preparing a piezoelectric super-hydrophobic double-layer antifouling coating, comprising the following steps:
[0061] (1) Preparation of piezoelectric primer: 53 parts by weight of xylene was added to a disperser, and 1.5 parts of defoamer and 2.5 parts of anti-settling agent were added at a line speed of 6 m / s, and stirred for 5 min. 114 parts of epoxy resin were added at a line speed of 10 m / s, and stirred for 60 min to form a slurry. 86 parts of zinc oxide nanowires and 17.8 parts of graphene were added and dispersed at a high power ultrasonic dispersion of 300 W for 30 min. After uniform dispersion, the mixture was added to a disperser, and the speed was adjusted to 6 m / s. 22.8 parts of curing agent were added and stirred for 5 min to obtain slurry a, i.e., piezoelectric primer.
[0062] (2) Preparation of super hydrophobic surface coating: 162 parts by weight of xylene are added to a disperser, 1 part of defoamer and 2 parts of anti-settling agent are added at a linear speed of 6 m / s, and stirred for 10 min. 39 parts of epoxy resin are added at a linear speed of 10 m / s, and stirred for 20 min to form a slurry. 74 parts of 100 nm spherical zinc oxide and 74 parts of 50 nm spherical zinc oxide are added, and dispersed for 40 min with a high-power ultrasonic dispersion of 300 W. After uniform dispersion, a disperser is added, the speed is adjusted to 6 m / s, and 8 parts of curing agent are added and stirred for 5 min to obtain slurry b, i.e., micro-nano structure layer coating.
[0063] 41 parts of silicone resin, 162 parts of n-hexane and 5 parts of curing agent were added into a disperser and stirred for 15 minutes at a linear speed of 6 m / s to obtain slurry c, i.e., a hydrophobic layer coating.
[0064] (3) Coating of piezoelectric base layer: spray the piezoelectric base layer coating evenly on the tinplate sheet and dry it at 90°C for 25 minutes until it is semi-dry to form the piezoelectric base layer.
[0065] (4) Coating of super-hydrophobic surface layer: The micro-nano structure layer coating is evenly sprayed on the semi-dry surface of the piezoelectric bottom layer. After drying at 60°C for 50 min, the hydrophobic layer coating is evenly sprayed on the micro-nano structure layer. After drying at 30°C for 30 min, the micro-nano structure layer and the hydrophobic layer together form a super-hydrophobic surface layer.
[0066] Example 4
[0067] A method for preparing a piezoelectric super-hydrophobic double-layer antifouling coating, comprising the following steps:
[0068] (1) Preparation of piezoelectric primer: 42 parts by weight of trifluorotoluene was added to a disperser, and 1.2 parts of defoamer, 1.8 parts of anti-settling agent, and 2 parts of dispersant were added at a line speed of 6 m / s, and stirred for 10 min. 114 parts of fluorocarbon resin were added at a line speed of 10 m / s, and stirred for 60 min to form a slurry. 60 parts of barium titanate and 1 part of single-walled carbon nanotubes were added and dispersed at a high power of 300 W for 30 min. After uniform dispersion, the mixture was added to a disperser, and the speed was adjusted to 6 m / s. 20 parts of curing agent were added and stirred for 5 min to obtain slurry a, i.e., piezoelectric primer.
[0069] (2) Preparation of super hydrophobic surface coating: 52 parts by weight of trifluorotoluene were added to a disperser, 1 part of defoamer and 2 parts of anti-settling agent were added at a linear speed of 6 m / s, and stirred for 10 min. 22 parts of fluorocarbon resin were added at a linear speed of 10 m / s, and stirred for 20 min to form a slurry. 41 parts of 50 nm spherical zinc oxide were added and dispersed for 40 min with a high-power ultrasonic dispersion of 300 W. After uniform dispersion, a disperser was added, the speed was adjusted to 6 m / s, and 4 parts of curing agent were added and stirred for 5 min to obtain slurry b, i.e., micro-nano structure layer coating.
[0070] 15 parts of fluorocarbon resin, 52 parts of trifluorotoluene and 5 parts of curing agent were added into a disperser and stirred for 15 minutes at a linear speed of 6 m / s to obtain slurry c, i.e., a hydrophobic layer coating.
[0071] (3) Coating of piezoelectric base layer: spray the piezoelectric base layer coating evenly on the tinplate sheet and dry it at 90°C for 25 minutes until it is semi-dry to form the piezoelectric base layer.
[0072] (4) Coating of super-hydrophobic surface layer: The micro-nano structure layer coating is evenly sprayed on the semi-dry surface of the piezoelectric bottom layer. After drying at 60°C for 50 min, the hydrophobic layer coating is evenly sprayed on the micro-nano structure layer. After drying at 30°C for 30 min, the micro-nano structure layer and the hydrophobic layer together form a super-hydrophobic surface layer.
[0073] Example 5
[0074] A method for preparing a piezoelectric super-hydrophobic double-layer antifouling coating, comprising the following steps:
[0075] (1) Preparation of piezoelectric primer: 53 parts by weight of xylene was added to a disperser, and 1.2 parts of defoamer, 1.8 parts of anti-settling agent, and 2 parts of dispersant were added at a line speed of 6 m / s, and stirred for 10 min. 130 parts of polyurethane resin were added at a line speed of 10 m / s, and stirred for 60 min to form a slurry. 90 parts of tourmaline and 30 parts of silver powder were added and dispersed at a high power ultrasonic dispersion of 300 W for 30 min. After uniform dispersion, the mixture was added to a disperser, and the speed was adjusted to 6 m / s. 28 parts of curing agent were added and stirred for 5 min to obtain slurry a, i.e., piezoelectric primer.
[0076] (2) Preparation of super hydrophobic surface coating: 162 parts by weight of xylene were added to a disperser, 2.5 parts of defoamer and 1.5 parts of anti-settling agent were added at a linear speed of 6 m / s, and stirred for 10 min. 39 parts of polyurethane resin were added at a linear speed of 10 m / s, and stirred for 20 min to form a slurry. 163 parts of 50 nm spherical zinc oxide were added and dispersed for 40 min with a high-power ultrasonic dispersion of 300 W. After uniform dispersion, a disperser was added, the speed was adjusted to 6 m / s, and 9 parts of curing agent were added and stirred for 5 min to obtain slurry b, i.e., micro-nano structure layer coating.
[0077] 51 parts of fluorosilicone resin, 162 parts of toluene and 13 parts of curing agent were added into a disperser, and stirred for 15 minutes at a linear speed of 6 m / s to obtain slurry c, i.e., a hydrophobic layer coating.
[0078] (3) Coating of piezoelectric base layer: spray the piezoelectric base layer coating evenly on the tinplate sheet and dry it at 90°C for 25 minutes until it is semi-dry to form the piezoelectric base layer.
[0079] (4) Coating of super-hydrophobic surface layer: The micro-nano structure layer coating is evenly sprayed on the semi-dry surface of the piezoelectric bottom layer. After drying at 60°C for 50 min, the hydrophobic layer coating is evenly sprayed on the micro-nano structure layer. After drying at 30°C for 30 min, the micro-nano structure layer and the hydrophobic layer together form a super-hydrophobic surface layer.
[0080] Example 6
[0081] The method for preparing a piezoelectric super-hydrophobic double-layer antifouling coating in this embodiment is the same as that in Embodiment 1, except that the inorganic piezoelectric material in this embodiment uses 82 parts of flaky zinc oxide.
[0082] Example 7
[0083] The preparation method of a piezoelectric super-hydrophobic double-layer antifouling coating in this embodiment is the same as that in Embodiment 1, except that the inorganic piezoelectric material in this embodiment uses 60 parts of four-needle zinc oxide whiskers.
[0084] Example 8
[0085] The preparation method of a piezoelectric super-hydrophobic double-layer antifouling coating in this embodiment is the same as that in Embodiment 1, except that the inorganic conductive material in this embodiment is 30 parts of multi-walled carbon nanotubes.
[0086] Comparative Example 1
[0087] A method for preparing a piezoelectric bactericidal coating, the steps are as follows:
[0088] (1) Preparation of piezoelectric coating: Add 50 parts by weight of xylene into a disperser, add 1.2 parts of defoamer, 1.8 parts of anti-settling agent, and 1 part of dispersant at a line speed of 6 m / s, and stir for 10 minutes. Add 120 parts of epoxy resin at a line speed of 10 m / s, and stir for 60 minutes to form a slurry. Add 82 parts of tetrapod-shaped zinc oxide whiskers and 3 parts of multi-walled carbon nanotubes and disperse them at a high power of 300 W for 30 minutes. After uniform dispersion, add to the disperser, adjust the speed to 6 m / s, add 24 parts of curing agent and stir for 5 minutes to obtain a piezoelectric coating.
[0089] (2) Application of piezoelectric coating: The piezoelectric coating paint is evenly sprayed on the tinplate sheet and dried at 90°C to form a piezoelectric sterilization coating.
[0090] Example 9
[0091] Performance test of piezoelectric superhydrophobic double-layer antifouling coating
[0092] Antifouling coatings were prepared according to Examples 1 to 8 and Comparative Example 1 to obtain piezoelectric bottom layers of Sample 1, Sample 2, Sample 3, Sample 4, Sample 5, Sample 6, Sample 7, Sample 8 and Sample 1, respectively.
[0093] (1) Piezoelectric performance test: To test the open circuit voltage of the coating, the sample encapsulated in PET is connected to the electrochemical workstation using a wire, an ultrasonic force of 200 W is applied at a frequency of 0.5 Hz, and the output voltage of the piezoelectric film is detected using a CHI 760E electrochemical workstation. The test results are shown in Figure 1 .
[0094] Depend on Figure 1 It can be seen that the piezoelectric bottom layers of samples 1, 2, 3 and sample 1 are all piezoelectric. The output voltage of the piezoelectric bottom layer of sample 1 is relatively high. After the super-hydrophobic surface layer is applied, the output voltage of the composite coating is further improved. Under the external mechanical vibration of ultrasonic waves simulating ocean waves, the asymmetric structure of the piezoelectric crystal causes the internal positive and negative charge centers to shift, forming an electric dipole moment and a built-in electric field, and electrons and holes move to the surface of the material in opposite directions. A certain amount of conductive material helps to enhance the ability of the piezoelectric coating to release electrical signals. On the one hand, conductive materials can promote the uniform dispersion of piezoelectric materials to a certain extent; on the other hand, compounding an appropriate amount of conductive materials in a polymer matrix can improve the polymer's ability to transmit electrical signals to obtain a better piezoelectric response effect.
[0095] In summary, samples 1 to 2 exhibit good piezoelectric properties, especially the composite piezoelectric marine antifouling coating of sample 1 exhibits the best piezoelectric properties. Comparing sample 1 and sample 6, it can be seen that the piezoelectricity of the obtained coatings is quite different when zinc oxide with different morphologies is used as filler. The piezoelectricity of the antifouling coating obtained in Example 1 using four-needle zinc oxide whiskers as inorganic piezoelectric fillers is better. Comparing sample 1 and sample 7, it can be seen that high and low concentrations of four-needle zinc oxide whiskers are used as inorganic piezoelectric materials, respectively, which shows that a high piezoelectric filler concentration (82 parts by weight of four-needle zinc oxide whiskers) can significantly enhance the piezoelectric properties of the coating. This is because the more piezoelectric fillers, the easier it is to form a charge transfer path in the resin. Samples 1 and 8, respectively, use low and high concentrations of multi-walled carbon nanotubes as inorganic conductive materials, which shows that a high conductive filler concentration (15 parts by weight of multi-walled carbon nanotubes) will weaken the piezoelectric properties of the coating. This is because the excessive carbon nanotubes wrap the zinc oxide, causing it to lose its semiconductor properties.
[0096] (2) Water contact angle test: The so-called super-hydrophobic surface refers to a surface with a static water contact angle (WCA) greater than 150°. The super-hydrophobic surface can form an air layer in the space of the microstructure / nanostructure, thereby significantly reducing the contact between seawater and the substrate surface, thereby reducing the attachment sites of organisms to achieve the purpose of anti-fouling.
[0097] The specific process steps are as follows: Use the JC2000C3 contact angle measuring instrument to test samples 1 to 8 and the piezoelectric bottom layer of sample 1. The samples are placed on the instrument platform, deionized water is used, and the measurement is performed according to the standard of the angle measurement method with a measurement accuracy of 0.5. The test results are shown in Figure 2 .
[0098] Depend on Figure 2 It can be seen that among all the samples, the water contact angle of sample 1 is the largest at 152.12°, indicating that the water contact angle of the super-hydrophobic surface layer is closely related to the particle size of zinc oxide. The smaller the particle size, the larger the surface water contact angle and the better the hydrophobic effect. The super-hydrophobic coating constructed by sample 1 can exert a better anti-fouling effect.
[0099] Example 10
[0100] Antifouling coatings were prepared according to Examples 1 to 8, and Sample 1, Sample 2, Sample 3, Sample 4, Sample 5, Sample 6, Sample 7 and Sample 8 were obtained respectively. A blank coating was set as a control group. The thickness of the coatings was 300 μm.
[0101] (1) Test of hydroxyl radical production: Hydroxyl radical (·OH) is generally considered to be an active group that exerts a bactericidal effect. The 2-hydroxyterephthalic acid generated by the reaction of hydroxyl radical with terephthalic acid has an obvious fluorescence effect and has a fluorescence characteristic intensity peak at a wavelength of about 425 nm. The application of fluorescence technology to the detection of intermediate free radicals in the degradation process can prove that hydroxyl radicals with strong oxidizing properties are generated during the catalytic degradation process.
[0102] The specific process steps are as follows:
[0103] (i) Add 50 mL of 5×10 -4 mol·L -1 In the aqueous solution of terephthalic acid, an ultrasonic cleaning machine with a power of 200W is used to provide piezoelectric effect.
[0104] (ii) Hydroxyl free radical detection experiment was carried out under the external mechanical vibration simulated by ultrasound. 3 mL of liquid was drawn every 5 minutes and then centrifuged at 9000 r / min. -1 After centrifugation at a speed of 5 min, the supernatant was taken.
[0105] (iii) The supernatant was analyzed and measured by F-7000 fluorescence spectrophotometer to determine the concentration of 2-hydroxyterephthalic acid produced, and the amount of hydroxyl radicals generated by the sample during this period was calculated.
[0106] (2) Test of superoxide free radical production: Superoxide free radical (·O2 - ) can react with nitro blue tetrazolium solution to reduce the ultraviolet absorption peak of nitro blue tetrazolium solution at 259nm. Therefore, the ultraviolet-visible absorption intensity of nitro blue tetrazolium solution can be used to detect O2 - presence and concentration.
[0107] The specific process steps are as follows:
[0108] (i) Add 50 mL of 2.5×10 -5 mol·L -1 In the nitro blue tetrazolium solution, an ultrasonic cleaning machine with a power of 200W provides piezoelectric effect.
[0109] (ii) Superoxide free radical detection experiment was carried out under the external mechanical vibration simulated by ultrasound. 3 mL of liquid was drawn every 5 minutes and then centrifuged at 9000 r / min. -1 After centrifugation at a speed of 5 min, the supernatant was taken.
[0110] (iii) The supernatant was analyzed and measured by UV-2600 ultraviolet-visible spectrophotometer to determine the concentration of nitro blue tetrazolium solution, and the amount of hydroxyl radicals generated by the sample during this period of time was calculated.
[0111] Depend on Figures 3-4 It can be seen that: at the same time and under the same conditions, the content of hydroxyl radicals and superoxide radicals produced by sample 1 is higher than that of other samples, and the trend of the results is consistent with the trend of the results of the piezoelectric performance test. The coating can use the wave energy in the ocean to create external mechanical vibration conditions, so that electrons and holes move to the surface of the material in opposite directions, react with dissolved oxygen and surrounding water to generate superoxide radicals, hydroxyl radicals and other active oxygen that can kill bacteria and other microorganisms. This shows that the environmentally friendly composite marine antifouling coating based on piezoelectric catalysis prepared by the present invention can produce more active oxygen that can kill bacteria.
[0112] (3) Antibacterial and antifouling performance test: Gram-negative Escherichia coli and Gram-positive Staphylococcus aureus were used as the dominant microorganisms for antibacterial experiments. The blank control group samples and samples 1 to 8 were cut into the same size and sterilized for 30 minutes. 1.5 mL of bacterial suspension (1.0×10 5CFU / mL) was inoculated into an EP tube containing a sample, and a pure tinplate sheet was placed in the EP tube as a control group for bacterial proliferation; then the bacterial tube was cultured for 4 hours without ultrasound, and then continued to be cultured for 8 hours under 50kHz, 200W ultrasound. At the end of the co-culture, the bacterial solution was diluted to a certain multiple, and an appropriate amount of the bacterial solution was spread on the solid culture medium and cultured in a 37°C incubator for 12 hours. At the end of the experiment, the plate count method was used to determine the number of viable planktonic bacteria in the culture medium. Sterilization rate (%) = (number of original bacteria - number of viable bacteria) / number of original bacteria × 100%.
[0113] Depend on Figure 5 As shown in Table 2, the piezoelectric super-hydrophobic double-layer antifouling coating prepared by the present invention has a sterilization rate of more than 90% against Escherichia coli (Gram-negative bacteria) and a sterilization rate of more than 91.5% against Staphylococcus aureus (Gram-positive bacteria). The antibacterial rate of sample 1 against Escherichia coli and Staphylococcus aureus is 100%, indicating that the coating has strong sterilization and antifouling properties against both Gram-negative and Gram-positive bacteria.
[0114] Table 2 Summary of antibacterial rates of the control group and samples 1 to 8 coatings
[0115]
[0116]
[0117] (4) Test of anti-algae and anti-fouling performance: Anti-algae experiments were conducted with triangular brown finger algae and small crescent-shaped algae as the dominant marine algae. Samples 1 to 8 were cut into the same size as the slide and sterilized for 30 minutes with the blank control group samples. 30 μL of algae solution of a certain concentration, 30 mL of artificial seawater and the sample were placed in a culture dish and cultured under ultrasonic conditions of 50 kHz and 200 W for 3 hours, and then placed in a 20°C incubator for 7 days. After the co-culture was completed, 200 μL of algae solution was taken and the absorbance was measured using an enzyme marker. Anti-algae rate (%) = (absorbance of control group algae solution - absorbance of sample algae solution) / absorbance of control group algae solution × 100%.
[0118] Depend on Figure 6 As shown in Table 3, the anti-algae rate of sample 1 of the present invention against brown finger algae is 98.6%, and the anti-algae rate against small crescent algae is 95.7%, indicating that the coating has strong anti-algae and anti-fouling properties against brown finger algae and small crescent algae.
[0119] Table 3 Summary of anti-algae rates of the control group and samples 1 to 8 coatings
[0120]
[0121]
[0122] Although the above embodiments have been described in detail, they are only a part of the embodiments of the present invention, not all of them. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all belong to the protection scope of the present invention.
Claims
1. A piezoelectric super-hydrophobic double-layer antifouling coating, characterized in that: By weight, the piezoelectric super-hydrophobic double-layer antifouling coating comprises a piezoelectric base layer coated on the surface of a substrate and a super-hydrophobic surface layer coated on the piezoelectric base layer; the piezoelectric base layer is prepared from 114 to 130 parts of a film-forming resin, 60 to 90 parts of an inorganic piezoelectric material, 1 to 30 parts of an inorganic conductive material, 25 to 33 parts of an auxiliary agent and 42 to 53 parts of a solvent; the super-hydrophobic surface layer is composed of a micro-nano structure layer and a hydrophobic layer coated on the micro-nano structure layer, the micro-nano structure layer is prepared from 22 to 39 parts of a film-forming resin, 41 to 163 parts of nano zinc oxide, 7 to 13 parts of an auxiliary agent and 52 to 162 parts of a solvent, and the hydrophobic layer is prepared from 15 to 51 parts of a low surface energy resin, 5 to 13 parts of an auxiliary agent and 52 to 162 parts of a solvent.
2. The piezoelectric super-hydrophobic double-layer antifouling coating according to claim 1, characterized in that: The piezoelectric base layer is prepared from 114 to 120 parts of a film-forming resin, 82 to 88 parts of an inorganic piezoelectric material, 3 to 17.8 parts of an inorganic conductive material, 26.8 to 28 parts of an auxiliary agent and 45 to 53 parts of a solvent; the micro-nanostructure layer is prepared from 39 parts of a film-forming resin, 148 parts of nano zinc oxide, 10 to 11 parts of an auxiliary agent and 137 to 162 parts of a solvent; and the hydrophobic layer is prepared from 41 parts of a low surface energy resin, 5 parts of an auxiliary agent and 162 parts of a solvent.
3. The piezoelectric super-hydrophobic double-layer antifouling coating according to claim 1, characterized in that: The film-forming resin is at least one of epoxy resin, fluorocarbon resin and polyurethane resin; the auxiliary agent is at least one of dispersant, defoamer, anti-settling agent and curing agent; the solvent is at least one of xylene, trifluorotoluene, n-hexane and toluene.
4. The piezoelectric super-hydrophobic double-layer antifouling coating according to claim 1, characterized in that: In the piezoelectric bottom layer, the inorganic piezoelectric material is at least one of zinc oxide, barium titanate and tourmaline; the inorganic conductive material is at least one of multi-walled carbon nanotubes, single-walled carbon nanotubes, silver powder, copper powder and graphene.
5. The piezoelectric super-hydrophobic double-layer antifouling coating according to claim 4, characterized in that: In the piezoelectric bottom layer, the inorganic piezoelectric material is zinc oxide, and the zinc oxide is one of flower-shaped zinc oxide, four-needle zinc oxide whisker, and zinc oxide nanowire.
6. The piezoelectric super-hydrophobic double-layer antifouling coating according to claim 1, characterized in that: The nano zinc oxide of the micro-nano structure layer is at least one of 150nm spherical zinc oxide, 100nm spherical zinc oxide, 50nm spherical zinc oxide, and 10nm spherical zinc oxide.
7. The piezoelectric super-hydrophobic double-layer antifouling coating according to claim 1, characterized in that: The low surface energy resin of the hydrophobic layer is at least one of an organic silicone resin, a fluorocarbon resin and a fluorosilicone resin.
8. A method for preparing a piezoelectric super-hydrophobic double-layer antifouling coating according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) Preparation of piezoelectric primer: weigh a film-forming resin, an inorganic piezoelectric material, an inorganic conductive material, an additive and a solvent by weight, and mix the components uniformly to obtain a piezoelectric primer; (2) Preparation of super-hydrophobic surface coating: weighing film-forming resin, nano zinc oxide, additives and solvent by weight, and mixing the components to obtain a micro-nano structure layer coating; then weighing low surface energy resin, additives and solvent by weight, and mixing the components to obtain a hydrophobic layer coating; (3) Coating of piezoelectric base layer: coating the piezoelectric base layer coating on the surface of the substrate and drying it until the surface is dry to form the piezoelectric base layer; (4) Coating of super-hydrophobic surface layer: The micro-nano structure layer coating is evenly sprayed on the semi-dry surface of the piezoelectric bottom layer. After drying until completely dry, the hydrophobic layer coating is evenly sprayed on the micro-nano structure layer. After drying, the micro-nano structure layer and the hydrophobic layer together form a super-hydrophobic surface layer.
9. The method for preparing a piezoelectric super-hydrophobic double-layer antifouling coating according to claim 8, wherein in step 3), the drying condition is 90° C., 25 min; in step 4), the first drying condition is 60° C., 50 min; and the second drying condition is 30° C., 30 min.
10. An application of the piezoelectric superhydrophobic double-layer antifouling coating as claimed in any one of claims 1 to 7 in antifouling topcoat on the bottom of ships, offshore platforms and offshore industrial facilities.
Citation Information
Patent Citations
Super-hydrophobic conductive composite coating for preventing lunar dust adhesion and preparation method thereof
CN117363061A
Piezoelectric antifouling coating as well as preparation method and application thereof
CN118291007A
Marine antifouling paint with piezoelectric conductivity and preparation and application thereof
CN118308007A
Process for treating a glass or porcelain component having a superhydrophobic protective coating
WO2018220294A1
Electric antifouling
WO2019180326A1
Cited By
Antifouling coating material based on piezoelectric super-hydrophobic effect as well as preparation method and application of antifouling coating material
CN121319717A