ABS (Acrylonitrile Butadiene Styrene) highlight paint coating for automobile parts and preparation method of ABS highlight paint coating

By adding modified silicone polyester leveling agent, closed isocyanate and high-performance polyester modified silicone to the high-gloss paint of automobile accessories, the pits, burrs and gloss reductions during the baking of water-based high-gloss paints is solved. The problem is that the flatness and scratch resistance of the paint surface are improved, and the pass rate of the finished product is improved.

CN118978849APending Publication Date: 2024-11-19SICHUAN AOBEILONG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410966242.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The water-based ABS high-gloss paint of existing automotive accessories is prone to pits, burrs and gloss reduction during baking, resulting in scratches on the paint surface, reducing the pass rate of the finished product and increasing production costs.

Method used

Improve paint surface tension and mechanical properties to avoid pits and burrs by adding specific mass percentages of modified silicone polyester leveling agents, modified enclosed isocyanates and high-performance polyester modified silicones to high-gloss paint coatings. and improve scratch resistance.

Benefits of technology

It effectively avoids the occurrence of pits and burrs during baking, improves the gloss and scratch resistance of the paint surface, and improves the pass rate and production efficiency of the finished product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses an ABS (Acrylonitrile Butadiene Styrene) high-gloss paint coating for automobile parts and a preparation method thereof, the ABS high-gloss paint coating comprises a modified component and a basic component, and the mass percentage of the modified component is 1.9-2.2% of the mass percentage of the basic component. The modified component is prepared from the following components in percentage by mass: 0 to 0.35 percent of modified organic silicon polyester flatting agent, 0 to 0.3 percent of high-performance polyester modified organic silicon and 1.4 to 1.6 percent of modified blocked isocyanate. According to the invention, through specific modified components, pits and burrs are prevented from being generated on the paint surface in the baking process of the ABS high-gloss paint coating, the glossiness of the final paint surface is improved, and the scratch resistance is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of coatings, and in particular to an ABS high-gloss paint coating for automobile accessories and a preparation method thereof. Background Art

[0002] High gloss paint has a wide range of uses and is suitable for various high-end electrical appliances, handicrafts, and wood products, such as laptops, VCDs, hair dryers, audio-visual equipment, cameras, mobile phones, telephones, cars, etc. It has excellent gloss and leveling, performance, etc. It has the characteristics of good fullness, natural three-dimensional effect, high gloss, good hardness, and good leveling. It also has excellent adhesion and resistance to yellowing and chemicals.

[0003] After the existing ABS high-gloss paint for auto parts is baked, the paint surface of the auto parts must be flat and smooth, and the uniformity must be consistent to avoid scratches on the paint surface. At present, most auto parts in my country use water-based automotive paint, and water-based automotive paint is prone to pits, burrs, gloss reduction and other problems during the baking process of auto parts, and the paint surface is easily scratched. This leads to a lower qualified rate of the final product, an increase in the scrap rate, and an increase in production costs. Summary of the invention

[0004] The purpose of the present invention is to provide an ABS high-gloss paint coating for automobile accessories and a preparation method thereof. After uniformly mixing modified components with different mass percentages with basic components, a high-gloss paint coating is prepared and used for baking automobile accessories, which avoids pits and burrs, improves scratch resistance, and solves the technical problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention adopts the following solutions:

[0006] An ABS high-gloss paint for automobile accessories comprises a modified component and a basic component, wherein the mass percentage of the modified component is 1.9% to 2.2% of the mass percentage of the basic component.

[0007] The technical concept of the present application is to solve the problems of pits, burrs, gloss reduction and easy scratches on the paint surface during the baking process of ABS high-gloss paint by adding a specific mass percentage of modified silicone polyester leveling agent, modified blocked isocyanate and high-performance polyester modified silicone.

[0008] Furthermore, the modified component includes the following components by mass percentage: 0-0.35% modified silicone polyester leveling agent, 0-0.3% high-performance polyester modified silicone and 1.4%-1.6% modified blocked isocyanate.

[0009] Furthermore, the basic component includes the following components in mass percentage: 40% to 45% polyurethane resin, 4% to 5% film-forming aid, 0.5% to 0.6% dispersant, 5% to 15% pigment, 0.2% to 0.3% wetting agent, 0.4% to 0.6% anti-settling agent, 5% to 15% filler, 5% to 8% water, 7% to 8% curing agent I, and 3.24% to 6.1% dilution curing agent solvent.

[0010] It should be noted that the basic components in this application are prior art and will not be described in detail here.

[0011] Furthermore, the mass percentage of the modified blocked isocyanate is 20% of the mass percentage of the curing agent I.

[0012] Furthermore, the preparation method of the modified organic silicone polyester leveling agent is: silicone oil with a hydrogen content of 0.3% and a molecular weight of 800, terminal allyl polyether and a catalyst with a weight ratio of 15 μg / g are stirred and reacted under nitrogen protection conditions to obtain the modified organic silicone polyester leveling agent.

[0013] Specifically, the movement of wet film paint is divided into three stages: spreading, pre-leveling and post-leveling. The surface tension, shear force, solvent evaporation rate, etc. of wet film paint have intricate relationships in each stage and influence each other. The pits on the paint surface of wet film paint mainly appear in the late leveling stage. With the uneven evaporation of the solvent and the film-forming resin itself, the paint surface will have a very small range of Bénard vortices, making the low surface tension like the eddy current in the vertical direction of the high surface tension.

[0014] By modifying the existing silicone polyester leveling agent, its compatibility with polyurethane resin is increased, and under the action of a catalyst, an ester chain is introduced into the polysiloxane chain through a catalytic addition reaction. The modified silicone polyester leveling agent forms a monomolecular layer on the outer surface of the paint surface, slowing down the solvent evaporation rate, reducing the gradient of the outer surface tension, providing a uniform outer surface tension, and allowing the vertical vortex to flow in the horizontal direction. This avoids pits during the baking process.

[0015] Furthermore, the mass percentage of the silicone oil to the terminal allyl polyether is 1:1.00-1.25.

[0016] Furthermore, the stirring speed is 200-250 r / min; and the reaction temperature is 120-125°C.

[0017] Furthermore, the preparation method of the modified blocked isocyanate is: dropwise adding isophorone diisocyanate under nitrogen conditions, and heating to 65° C. after the dropwise addition is completed to obtain the modified blocked isocyanate.

[0018] Specifically, before the prepolymer containing terminal isocyanate (isophorone diisocyanate) is dispersed and chain extended, methyl ethyl ketone oxime blocks the terminal isocyanate in the prepolymer, delaying the reaction in the early stage of the reaction. When the temperature rises to 70 degrees, the terminal isocyanate is unblocked. During the rapid rise in baking temperature, when the paint surface is fixed, the temperature rises and the paint surface reaction speed is accelerated, making the internal structure more precisely combined.

[0019] Since the modified blocked isocyanate protects the -NCO group, it will not react before the temperature reaches the unblocking temperature. In the first stage, the low-boiling water and solvent evaporate in advance before unblocking. When the temperature rises, the solvent evaporation rate reaches equilibrium. In the second stage, the unblocked isocyanate participates in the reaction. In the third stage, the modified blocked isocyanate is unblocked and participates in the reaction, which solves the problem of flat appearance and improves the mechanical properties of the coating. The prepolymer containing terminal isocyanate, that is, isophorone diisocyanate, is modified by the hydrophilic reagent dihydroxymethyl propionic acid (DMPA), and then methyl ethyl ketone oxime is used as a blocking agent to synthesize the modified blocked isocyanate as a curing agent.

[0020] Furthermore, the reaction temperature of the dropwise addition of methyl ethyl ketone oxime is 60° C., and the dropwise addition time is 1 hour.

[0021] The above-mentioned method for preparing an ABS high-gloss paint coating for automobile accessories is adopted, and 0-0.35% by mass of a modified silicone polyester leveling agent, 0-0.3% by mass of a high-performance polyester modified silicone and 1.4%-1.6% by mass of a modified blocked isocyanate and 70.34%-106.86% by mass of a basic component are uniformly mixed to obtain an ABS high-gloss paint coating.

[0022] The beneficial effects of the present invention are:

[0023] 1. The present invention changes the flow state of polyester during baking by adding a modified organic silicon polyester leveling agent, thereby avoiding uneven surface tension and the occurrence of pits during baking.

[0024] 2. By using a prepolymer containing terminal isocyanate (isophorone diisocyanate), after modification with a hydrophilic reagent dihydroxymethylpropionic acid, methyl ethyl ketone oxime is used as a blocking agent, a modified blocked isocyanate is synthesized as a curing agent, and a closed chain is connected to change the initial reaction conditions of the polyester to avoid burrs during the baking process.

[0025] 3. By adding high-performance polyester modified silicone and polyester polymer back melting, the gloss of the paint surface can be improved, and the scratch resistance of the paint surface can be improved. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] The present invention is an ABS high-gloss paint for automobile parts, comprising the following components in percentage by mass:

[0028] Modified components: 0-0.35% modified silicone polyester leveling agent, 0-0.3% high-performance polyester modified silicone and 1.4%-1.6% modified blocked isocyanate.

[0029] Basic components: 40% to 45% polyurethane resin, 4% to 5% film-forming aid, 0.5% to 0.6% dispersant, 5% to 15% pigment, 0.2% to 0.3% wetting agent, 0.4% to 0.6% anti-settling agent, 5% to 15% filler, 5% to 8% water, 7% to 8% curing agent I, 3.24% to 6.1% dilution curing agent solvent.

[0030] The modified component and the basic component are uniformly mixed and stirred to obtain an ABS high-gloss paint.

[0031] Example 1

[0032] Example 1 of the present invention, preparation of modified silicone polyester leveling agent:

[0033] Add 0.3% hydrogen-containing silicone oil with a molecular weight of 800, terminal allyl polyether and catalyst into a flask with a stirrer and a thermometer, and stir at a speed of 200-250r / min under nitrogen protection. The reaction temperature is 120-125°C, and the catalyst addition amount is 15ug / g. After 7.5 hours of reaction, the polyether-modified silicone oil product is synthesized. By adjusting the ratio of different hydrogen-containing silicone oils and terminal allyl polyethers (the mass percentage of silicone oil to terminal allyl polyether is 1:1.00-1.25), the hydrogen content of the product is detected by chemical titration, and the conversion rate of Si-H in hydrogen-containing silicone oil is calculated. Determine the best reactant ratio for the conversion rate of silicon-hydrogen bonds.

[0034] Table 1 Conversion rate of Si-H in hydrogen-containing silicone oil obtained by different ratios of hydrogen-containing silicone oil and terminal allyl polyether

[0035] Reactant ratio 1:1.00 1:1.05 1:1.10 1:1.15 1:1.20 1:1.25 Si-H bond conversion rate 87.22 88.35 89.28 93.30 92.15 92.05

[0036] According to Table 1, when the mass percentage ratio of hydrogen-containing silicone oil to terminal allyl polyether is 1:1.15, the Si-H conversion rate in hydrogen-containing silicone oil is the highest. According to the above ratio, hydrogen-containing silicone oil with different side chains and terminal allyl polyether are selected to react to obtain modified silicone polyester leveling agents with different hydrogen-silicon-hydrogen conversion rates. The same amount of silicone polyester leveling agents prepared by adding to varnish are used for comparative experiments to test surface tension.

[0037] Surface tension performance data obtained by reacting different side chain hydrogenated silicone oils on surface 2

[0038]

[0039] According to Table 2, the modified silicone polyester leveling agent made of No. 3 silicone oil with a hydrogen content of 0.3% has the lowest surface tension when the same amount is added to the varnish. Therefore, the modified silicone polyester leveling agent is prepared by reacting the hydrogen-containing silicone oil with a hydrogen content of 0.3% with the terminal allyl polyether.

[0040] Example 2

[0041] This embodiment 2 is the preparation of the modified blocked isocyanate of the present invention:

[0042] Methyl ethyl ketone oxime (MEKO) was added dropwise to isophorone diisocyanate (IPDI) under nitrogen conditions. The reaction temperature for the addition of methyl ethyl ketone oxime was 60° C. and the addition time was 1 h. After the addition was completed, the temperature was raised to 65° C. to obtain a modified blocked isocyanate.

[0043] A certain amount of isophorone diisocyanate is added to a flask equipped with a stirrer and a thermometer, and a measured amount of methyl ethyl ketone oxime is added dropwise under nitrogen protection to react until -NCO is completely blocked. During the reaction, samples are taken at regular intervals to determine the -NCO content, and the di-n-butylamine method is used for titration.

[0044] Table 3 -NCO blocking rate at different H / NCO ratios

[0045]

[0046] According to Table 3, as the H / NCO ratio increases, the NCO blocking rate does not increase much. Finally, the H / NCO ratio of 1.1 was selected as the final reaction condition.

[0047] Thermogravimetric analysis (TGA) of modified blocked isocyanate: The initial deblocking temperature of the modified blocked isocyanate is determined by TGA. The mass change of the modified blocked isocyanate during heating is measured. The heating rate is usually controlled within the range of 5°C / min. The sample is placed in the TGA instrument. No catalyst is added during the deblocking reaction. Heating is started and the mass change data is recorded.

[0048] Table 4 Initial deblocking temperature of modified blocked isocyanate

[0049] Sample mass percentage % 100 100 100 95 85 82 Heating temperature(℃) 35 45 55 65 75 85

[0050] According to Table 4, the initial unblocking temperature of the modified blocked isocyanate is 65°C, which meets the requirements. At the same time, the modified blocked isocyanate is sealed and stored at room temperature, and no precipitation is observed for 6 months. It has good stability and no unblocking reaction occurs when stored at room temperature.

[0051] Example 3

[0052] 0-0.35% of modified silicone polyester leveling agent, 0-0.3% of high-performance polyester modified silicone and 1.4%-1.6% of modified blocked isocyanate, 40%-45% of polyurethane resin, 4%-5% of film-forming aid, 0.5%-0.6% of dispersant, 5%-15% of pigment, 0.2%-0.3% of wetting agent, 0.4%-0.6% of anti-settling agent, 5%-15% of filler, 5%-8% of water, 7%-8% of curing agent I, and 3.24%-6.1% of dilute curing agent solvent are mixed uniformly to obtain ABS high-gloss paint coatings with different addition amounts of modified silicone polyester leveling agent, and the ABS high-gloss paint coatings are used for spraying automobile accessories and baked at a certain temperature.

[0053] The addition amounts of the modified silicone polyester leveling agent in Example 3 were 0%, 0.1%, 0.15%, 0.20%, 0.25%, 0.3% and 0.35%, respectively. After baking, the surface tension of the high gloss paint was measured at a temperature of 30°C and a pressure of 100KPa.

[0054] Table 5 Surface tension of paint with different addition amounts of modified silicone polyester leveling agent

[0055]

[0056] According to Table 5, as the amount of modified silicone polyester leveling agent added increases, the surface tension of the wet film paint is reduced. When the addition amount is 0.3% and 0.35%, the surface tension of the paint does not change much. At the same time, the surface leveling effect of 0.3% addition can meet the paint appearance effect, so 0.3% is taken as the final addition amount.

[0057] Example 4

[0058] 0.3% modified silicone polyester leveling agent, 0-0.3% high-performance polyester modified silicone, modified blocked isocyanate (accounting for 0%-30% of the whole curing agent I), 40%-45% polyurethane resin, 4%-5% film-forming aid, 0.5%-0.6% dispersant, 5%-15% pigment, 0.2%-0.3% wetting agent, 0.4%-0.6% anti-settling agent, 5%-15% filler, 5%-8% water, 7%-8% curing agent I, 3.24%-6.1% dilution curing agent solvent are mixed uniformly to obtain ABS high-gloss paint coatings with different modified blocked isocyanate addition amounts, and the ABS high-gloss paint coatings are used for spraying automobile accessories and baked at a certain temperature.

[0059] The modified blocked isocyanate was added in different proportions to the overall curing agent I, specifically 0%, 5%, 15%, 20%, 25% and 30%, and the baking temperature was 70°C to 85°C for 2 hours, and the appearance of the paint surface was tested.

[0060] Table 6 Appearance and hardness data of paint surface with different proportions of modified blocked isocyanate in the overall curing agent I

[0061]

[0062] According to Table 6, when the proportion of the modified blocked isocyanate in the whole curing agent I is between 0% and 20%, the smoothness and hardness of the paint surface are significantly improved, and there is no significant improvement when it is higher than 20%. Therefore, 20% is taken as the final addition amount of the modified blocked isocyanate.

[0063] Example 5

[0064] 0.3% modified silicone polyester leveling agent, 0-0.3% high-performance polyester modified silicone and 1.4%-1.6% modified blocked isocyanate, 40%-45% polyurethane resin, 4%-5% film-forming aid, 0.5%-0.6% dispersant, 5%-15% pigment, 0.2%-0.3% wetting agent, 0.4%-0.6% anti-settling agent, 5%-15% filler, 5%-8% water, 7%-8% curing agent I, 3.24%-6.1% dilution curing agent solvent are mixed uniformly to obtain ABS high-gloss paint containing different amounts of high-performance polyester modified silicone, and the ABS high-gloss paint is used for spraying automobile accessories and baked at a certain temperature.

[0065] The mass percentage addition of high-performance polyester modified silicone is: 0%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, the baking temperature is 70℃~85℃, the baking time is 2h, and the paint surface related data is tested.

[0066] Table 7 Performance data of ABS high gloss paint with different addition amounts of high performance polyester modified silicone

[0067]

[0068] According to Table 7, when the mass percentage of high-performance polyester modified silicone is between 0% and 25%, the gloss, recoatability and anti-hanging performance of the paint surface are significantly improved. When the addition amount is 0.2%, each performance reaches the best, so the proportion of 0.2% is taken as the final addition amount of high-performance polyester modified silicone.

[0069] Adding 0.2% by mass of high-performance polyester-modified silicone can perfectly dissolve in the polyester polymer, solve the problem of reduced gloss of the product caused by the precipitation of ordinary silicone, and improve the scratch resistance of the material.

[0070] The above description is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been disclosed as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. An ABS high gloss paint for automotive parts, characterized in that: It comprises a modified component and a basic component, wherein the mass percentage of the modified component is 1.9% to 2.2% of the mass percentage of the basic component.

2. The ABS high gloss paint for automobile accessories according to claim 1, characterized in that: The modified component comprises the following components in percentage by mass: 0-0.35% of modified organic silicon polyester leveling agent, 0-0.3% of high-performance polyester modified organic silicon and 1.4%-1.6% of modified blocked isocyanate.

3. The ABS high gloss paint for automobile accessories according to claim 2, characterized in that: The basic component comprises the following components by mass percentage: 40% to 45% polyurethane resin, 4% to 5% film-forming aid, 0.5% to 0.6% dispersant, 5% to 15% pigment, 0.2% to 0.3% wetting agent, 0.4% to 0.6% anti-settling agent, 5% to 15% filler, 5% to 8% water, 7% to 8% curing agent I, and 3.24% to 6.1% dilution curing agent solvent.

4. The ABS high gloss paint for automobile accessories according to claim 3, characterized in that: The mass percentage of the modified blocked isocyanate is 20% of the mass percentage of the curing agent I.

5. The ABS high gloss paint for automobile accessories according to claim 3, characterized in that: The preparation method of the modified organic silicon polyester leveling agent is as follows: silicone oil with a hydrogen content of 0.3% and a molecular weight of 800, terminal allyl polyether and a catalyst with a weight ratio of 15 μg / g are stirred and reacted under nitrogen protection conditions to obtain the modified organic silicon polyester leveling agent.

6. The ABS high gloss paint for automobile accessories according to claim 5, characterized in that: The mass percentage of the silicone oil to the terminal allyl polyether is 1:1.00-1.

25.

7. The ABS high gloss paint for automobile accessories according to claim 5, characterized in that: The stirring speed is 200-250 r / min; the reaction temperature is 120-125°C.

8. The ABS high gloss paint for automobile accessories according to claim 3, characterized in that: The preparation method of the modified blocked isocyanate comprises the following steps: adding methyl ethyl ketone oxime dropwise to isophorone diisocyanate under nitrogen conditions, and heating the mixture to 65° C. after the addition is completed to obtain the modified blocked isocyanate.

9. The ABS high gloss paint for automobile accessories according to claim 8, characterized in that: The reaction temperature for the dropwise addition of methyl ethyl ketone oxime was 60°C and the dropwise addition time was 1 hour.

10. A method for preparing an ABS high-gloss paint for automobile accessories according to any one of claims 1 to 9, characterized in that: 0-0.35% by mass of a modified silicone polyester leveling agent, 0-0.3% by mass of a high-performance polyester modified silicone, 1.4%-1.6% by mass of a modified blocked isocyanate, and 70.34%-106.86% by mass of a basic component are uniformly mixed to obtain an ABS high-gloss paint coating.