Interface bonding and damage repairing method for soft material
By using specific bonding liquid and initiator to form the bonding layer on the flexible soft robot interface, the problem of the bonding layer not matching the body gel after deletion damage of the flexible soft robot is solved, and a strong interface bonding is achieved and damage repair, maintain or improve mechanical properties, and do not affect water molecules and ion transport.
Patent Information
- Application Number
- CN202411121261.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-19
AI Technical Summary
The prior art is difficult to effectively solve the problem of mismatch between the adhesive layer and the body gel after deficient mechanical damage of flexible soft robots, resulting in distortion after material repair, affecting its mechanical properties and ion transport function.
By using specific bonding liquids, including monomers and initiators at the interface of the soft material, applying pressure to self-grow it to form an adhesive layer, the strong bonding and damage repair between the two gels are achieved, and the formation of a strong bonding and damage repair. The adhesive layer has the characteristics of self-growth thickness, which can closely fit the damaged interface and maintain or enhance mechanical properties.
It realizes interface bonding and deletion damage repair to a variety of soft material materials, high peel strength, and improved Young's modulus. After repair, it does not affect the transmission of water molecules and ions, extends the service life of soft material and improves its mechanics. performance.
Smart Images

Figure CN118978868A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of soft material bonding, and in particular to an interface bonding and damage repair method for soft material. Background Art
[0002] With the development of robot applications, hard and non-deformable materials such as metals can no longer meet the needs of new robots for complex scenarios such as flexible bending and micro-stress sensing; low modulus and high toughness soft materials have great potential in the development of flexible soft robots. However, flexible soft robots are susceptible to mechanical damage when interacting with the outside world; when soft materials are cut and punctured, the robot's sensing, movement and reliability are reduced, seriously affecting its operation and work. In order to solve the problem of repairing mechanical damage to flexible soft robots, researchers have proposed a self-healing material strategy, which can be divided into external aid type and intrinsic self-healing type according to the repair type.
[0003] The external aid type mainly repairs the damage by applying a gel adhesive to the damaged part to bond the gel material. Suo et al. placed a chitosan solution between two polyacrylamide (pAAm) hydrogels under acidic conditions. The polymer chains in the chitosan solution diffused into the pAAm gel to form a new network that interlocked with the pAAm gel network and completed the bonding (Yang J, Bai R, Suo Z. Advanced Materials, 2018, 30 (25): 1800671). However, the adhesive layer generated by most hydrogel adhesives after repairing the gel material will hinder the transmission of water molecules and ions, and the mismatch of deformation will cause damage under high strain, which will seriously affect the mechanical, electrical and other application functions of the gel material, limiting the application of gel materials in soft robots or flexible sensors. Intrinsic repair achieves simple interfacial bonding and repair of hydrogels through interfacial reversible covalent or reversible non-covalent interactions. Li et al. synthesized a hyaluronic acid hydrogel by reacting sodium periodate with sodium hyaluronate and cystamine hydrochloride, which has the ability to self-repair after damage (Li S, Pei M, Wan T, et al. Carbohydr Polym, 2020, 250: 116922). However, the intrinsic bonding repair method requires a special chemical structure design, and the mechanical properties of the material are relatively low. At the same time, neither the external aid type nor the intrinsic self-repair type methods can effectively solve the problem of bonding repair with missing damage; when the flexible soft material faces missing mechanical damage, the mismatch between the adhesive layer and the missing damage of the bulk gel will cause the material to be deformed after repair, which seriously affects the mechanical properties and ion transmission properties of the soft material.
[0004] Therefore, there is an urgent need to develop a method for interfacial bonding and damage repair of soft materials to achieve functions such as defect repair and not affecting the transmission of substances such as water molecules and ions after the damage is repaired. This method has extremely high application value in fields such as robotics. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for interfacial bonding and damage repair of soft materials. The method provided by the present invention can achieve bonding and missing damage repair for different soft materials, has good mechanical properties, and does not affect the transmission of substances such as water molecules and ions after the damage is repaired.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] In a first aspect, the present invention provides a method for interfacial bonding and damage repair of soft matter materials, selected from one of (a) and (b):
[0008] (a) soaking the soft material in adhesive liquid a respectively until swelling equilibrium is reached, taking out and bonding them, applying pressure, and forming an adhesive layer by self-growth at the interface; the adhesive liquid a comprises a monomer and an initiator; the adhesive liquid a is divided into an oxidized adhesive liquid and a reduced adhesive liquid;
[0009] (b) soaking the soft material in adhesive solution b until swelling equilibrium is reached, taking it out and coating it with initiator solution respectively, attaching it to the coating part, applying pressure, and forming an adhesive layer by self-growth at the interface; the adhesive solution b comprises a monomer;
[0010] The initiator is an oxidative initiator or a reducing initiator;
[0011] The thickness of the adhesive layer is 5 μm-1.1 mm;
[0012] The monomer is at least one of the following general formula (I) and general formula (II):
[0013] The general formula (I) is
[0014] The R1 is hydrogen or methyl;
[0015] R2 is hydrogen, and R3 is one of hydrogen, C1-C18 alkyl and its isomers, phenyl, chlorophenyl, phenol, butoxymethyl, benzyl, hydroxyethyl, hydroxyphenyl, dimethylaminopropyl, methylpropanesulfonic acid, and benzenesulfonic acid; or R2 and R3 are each independently one of C1-C4 alkyl and acetonyl; or R2 is methyl, and R3 is ethyl;
[0016] The general formula (II) is
[0017] The R4 is hydrogen or methyl;
[0018] The R5 is one of hydrogen, C1-C20 alkyl and isomers thereof, hydroxyethyl, ethyltrimethylammonium chloride, C1-C20 perfluoroalkyl, benzyl, phenyl, bornyl, and tetrahydrofuranyl.
[0019] The present invention proposes a method for promoting the bonding and damage repair of soft materials based on interface self-diffusion growth, which drives the monomer and initiator to diffuse to the bonding interface through osmotic pressure, induces the monomer to polymerize and grow at the interface to form a bonding layer of a certain thickness, and realizes the bonding and damage repair between two gels. The generated bonding layer has the characteristics of self-growth of thickness, and the mechanical properties are maintained or even enhanced at the bonding layer, which can realize the effective bonding of the interface and the healing of damage.
[0020] The above method (a) is an immersion method, and the method (b) is a coating method; the oxidative initiator and the reduced initiator are immersed or coated on the interface of the two soft materials to be bonded by the above methods (a) and (b), and the two initiators alone will not induce polymerization of specific monomers; when the two soft materials are bonded together under a certain pressure, the oxidative initiator and the reduced initiator react at the interface, thereby inducing polymerization of the monomers. The monomers conforming to the above structure polymerize at the interface and cross-link to form a third layer network, forming an interlocking entanglement structure with the polymer network of the soft materials on both sides, achieving strong bonding, so that the bonding layer can fit tightly with the soft materials on both sides of the bonding interface and the damaged interface.
[0021] The bonding and repairing methods of the present invention are applicable to a variety of soft materials, including: hydrogels (such as polyacrylamide, sodium polyacrylate, polyethylene glycol, poly(ethylene glycol acrylate), poly-N-isopropylacrylamide, poly(hydroxyethyl methacrylate), rubbers (such as polyisoprene, styrene-butadiene rubber, butadiene rubber, isoprene rubber, chloroprene rubber, butyl rubber, nitrile rubber, ethylene-propylene rubber, epoxidized natural rubber), elastomers (such as polyolefin elastomers TPO, thermoplastic elastomers TPE, dynamically vulcanized polyolefin elastomers TPV, polystyrene elastomers TPS, polyether-ester elastomers TPEE, polyamide elastomers TPA, silicone elastomers, and foamed materials of the above materials), and combinations thereof.
[0022] For different soft matter materials, the above-mentioned bonding and damage repair methods can spontaneously form an adhesive layer with a thickness of 5μm-1.1mm at the interface. The formed adhesive layer can fit tightly with the soft matter materials on both sides of the bonding interface or the damage defect. After bonding, the peel strength can reach more than 5N / m and can reach a maximum of more than 180N / m; the Young's modulus can reach up to 180kPa; and the generated adhesive layer can repair missing damage within 4mm, and has good repair effects on damage of different shapes; at the same time, after repairing the damage, it does not affect the transmission functions of substances such as water molecules and ions, and the mechanical properties of the repaired soft matter material are maintained or improved to a certain extent, which has extremely high application value in the fields of flexible soft robot damage repair.
[0023] Preferably, the adhesive liquid a and the adhesive liquid b further include a cross-linking agent.
[0024] Preferably, the oxidative initiator is at least one of ammonium persulfate, sodium persulfate, formic acid peroxide, calcium peroxyphosphate, potassium persulfate, and potassium peroxymonosulfate, and the reducing initiator is at least one of ferrous chloride, ferrous sulfate, cuprous chloride, NaHSO3, Na2SO3, Na2S2O3, tartaric acid, and glucose;
[0025] Or the oxidative initiator is at least one of dialkyl peroxide, cyclohexanone peroxide, isopropylbenzene hydroperoxide, tert-butyl hydroperoxide, acetone peroxide, tert-butyl ketone peroxide, benzophenone peroxide, di(2,4-dichlorobenzoyl) peroxide, and diisopropylbenzene peroxide, and the reducing initiator is at least one of formic acid, sulfonic acid, trialkyl boron, diisobutylonitrile hydrazine, tertiary amine, cyclopentane salt, thiol, and organic metal compound.
[0026] The present invention mainly utilizes olefin free radical polymerization reaction, and its initiator is a redox initiator. Redox initiators are divided into water-soluble oxidation and reduction initiators and oil-soluble oxidation and reduction initiators; according to different soft material types and implementation scenarios, a combination of the above water-soluble or oil-soluble initiators is used.
[0027] Preferably, the applied pressure is 0.04-1000 kPa.
[0028] Preferably, the bonding time is 1 min-12 h.
[0029] The peel strength of the adhesive layer and the thickness of the adhesive layer increase with the increase of bonding time, and stop increasing with the end of the monomer polymerization reaction. When equilibrium is reached and the thickness no longer changes, the peel strength reaches the highest.
[0030] Preferably, the oxidized bonding liquid comprises the following components in concentrations: 0.5-7M monomer, 0.0005-0.14M oxidized initiator; the reduced bonding liquid comprises the following components in concentrations: 0.5-7M monomer, 0.0005-0.14M reduced initiator;
[0031] The concentration of the monomer in the bonding solution b is 0.5-7M; the concentration of the oxidative initiator or the reduced initiator in the initiator solution is 0.1-0.7M.
[0032] More preferably, the concentration of the cross-linking agent is 0.0005-0.7M.
[0033] Further preferably, in the method (b), after applying the initiator solution, waiting for 0.1 min-12 h before bonding, can make the initiator diffuse better at the interface of the soft material, so that the cross-linking network is more solid.
[0034] As a preferred embodiment, the monomer is acrylamide; or the monomer is methacrylamide and methacrylic acid. In this case, the adhesive layer formed has high peel strength and good mechanical properties.
[0035] Preferably, in the oxidized adhesive solution or the reduced adhesive solution, the molar concentration ratio of the crosslinking agent to the monomer is (0.01-0.02): 1. Under this molar ratio condition, the peel strength of the formed adhesive layer is relatively high.
[0036] Preferably, in the oxidized adhesive solution or the reduced adhesive solution, the molar concentration ratio of the initiator to the monomer is (0.002-0.005): 1. Under this molar ratio condition, the monomer fully reacts to a threshold value, and the thickness of the formed adhesive layer is substantially the highest.
[0037] In a second aspect, the present invention provides the application of the interface bonding and damage repair method of the above-mentioned soft matter material in repairing missing damage of gel material, repairing damage of ion conductive gel and preparing interface coating composite material.
[0038] Preferably, the gel material loss damage includes fracture damage and local loss damage.
[0039] Compared with the prior art, the present invention has the following beneficial effects:
[0040] The soft material interface bonding and damage repair method provided by the present invention effectively realizes the self-diffusion growth interface bonding or damage repair of various soft material materials by limiting two specific different bonding methods, as well as the monomer, initiator, and cross-linking agent in the bonding liquid, and regulating the component ratio thereof. The bonding layer has high peel strength and good mechanical properties, and the functions such as the transmission of water molecules and ions are not affected after the damage is repaired. It can be applied to the fields of flexible soft robots, for repairing gel material missing damage, ion conductive gel damage (including fracture damage and local missing damage), and for preparing interface coating composite materials, extending the service life of soft material and improving its mechanical properties, and has high application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 Schematic diagram of the chemical composition and reaction mechanism of the bonding liquid in Example 1;
[0042] Figure 2 This is a schematic diagram of the interface bonding step in Example 1;
[0043] Figure 3 is a top view of the PVA / AAm hydrogel after interface bonding in Example 1;
[0044] Figure 4 The bonding cross section of the PVA / AAm hydrogel in Example 1 and the cross section of the PVA / AAm gel after bonding and peeling;
[0045] Figure 5 The scanning electron microscope images of the cross section of the PVA / AAm hydrogel and the bonding cross section of the PVA / AAm hydrogel prepared in Example 1;
[0046] Figure 6 This is a scanning electron microscope image of the cross section of the PVA / AAm hydrogel after bonding and peeling of Example 1;
[0047] Figure 7 The process diagram and effect diagram of repairing the PVA / AAm hydrogel of the missing damage in Example 2;
[0048] Figure 8 The peel strength results of the PVA / AAm hydrogel prepared in the example under different redox initiator combinations;
[0049] Fig. 9 This is a picture showing the effect of bonding the AAc / AAm hydrogel prepared in the example with a bonding liquid without adding a cross-linking agent;
[0050] Fig.10 This is a comparison result of the peeling strength of the hydrogel bonded by the interface bonding method of Example 1 and other initiation methods in Comparative Example 1;
[0051] Fig.11 This is a graph showing the thickness of the adhesive layer formed by using different adhesive solutions in Comparative Example 2;
[0052] Fig.12 The peel strength results of Example 1 and Comparative Example 2 after bonding using different adhesive solutions;
[0053] Fig.13 The results of the peel strength (a), bonding layer thickness (b), Young's modulus (c), and bonding layer toughness (d) of PVA / AAm hydrogel bonded with adhesive solutions of different AAm monomer concentrations;
[0054] Fig.14 The results of the peel strength (a) and bonding layer thickness (b) of PVA / AAm hydrogel at different bonding times;
[0055] Fig.15 The relationship between the Young's modulus and the cross-linking agent concentration of the bonding layer formed by bonding PVA / AAm hydrogel with adhesive solutions of different cross-linking agent concentrations (a); the relationship between the peel strength and the Young's modulus (b) result diagram;
[0056] Fig.16 The results of the peel strength (a) and the thickness of the bonding layer (b) of the PVA / AAm hydrogel bonded by the bonding solution with different initiator concentrations;
[0057] Fig.17 The peel strength of PVA / AAm hydrogel bonded with adhesive solutions of different initiator concentrations varies with bonding time, (a) 0.1%; (b) 0.5%; (c) 1%; (d) 2%;
[0058] Fig.18 (a) Load normalized curve of blank sample under different constant strains; (b) Load normalized curve of PVA / AAm bonding under different constant strains; (c) Peel strength of hydrogel under different constant strains; (d) Adhesive layer thickness of hydrogel under different constant strains;
[0059] Fig.19 The peeling curve (a) and peeling strength (b) results of the bonding between the prepared PVA / AAm hydrogel and seven kinds of gel materials;
[0060] Fig. 20 The peel strength results of PVA / AAm hydrogel bonded with adhesive solutions of different monomer systems are shown in the figure;
[0061] Fig.21 The peel strength results of bonding PVA / AAm gel and five soft materials using HEA monomer system adhesive liquid;
[0062] Fig. 22The schematic diagram of the experiment on the molecular diffusion and transport regulation at the interface of PVA / AAm hydrogel using different films and the peel strength result diagram;
[0063] Fig.23 The bonding and repair effects of PVA / AAm hydrogels under different damage shapes; (a) heart-shaped; (b) circle; (c) pentagon; (d) star-shaped; (e) rectangle;
[0064] Fig.24 The effect diagrams of PVA / AAm hydrogel repair of defect injuries of different widths before and after.
[0065] Fig.25 The tensile curves (a) and conductivity (b) of different widths of missing damage before and after repair;
[0066] Fig.26 Nernst diagrams of PVA / AAm hydrogels before and after repair of injuries of different widths. DETAILED DESCRIPTION
[0067] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention will be further described below in conjunction with specific examples. The test methods used in the following examples are conventional methods unless otherwise specified; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.
[0068] Example 1
[0069] An embodiment of the interface bonding method of soft matter materials of the present invention.
[0070] The soft material for interface repair in this embodiment is polyvinyl alcohol / acrylamide hydrogel (PVA / AAm), and the specific preparation steps are as follows:
[0071] S1. The hydrogel was prepared by photoinitiated free radical polymerization, the concentration of the polyvinyl alcohol solution was 13.5wt%, the mass ratio of acrylamide to polyvinyl alcohol was 1:1; the crosslinker was MBA, the concentration was 1% of the molar concentration of the monomer; the initiator was α-keto, the concentration was 0.1% of the molar concentration of the monomer;
[0072] S2. The pre-configured transparent reaction solution was irradiated with ultraviolet light at a wavelength of 365 nm (about 70 mW / cm) for 8 hours in an argon environment of a glove box for polymerization;
[0073] S3. The polymerized gel was placed in an oven at 60°C for 4 hours to reduce its swelling degree, and then immersed in deionized water to achieve swelling equilibrium to obtain PVA / AAm hydrogel with a swelling degree of about 150%. The color of the PVA / AAm hydrogel before and after swelling changed from transparent to white, and the transmittance decreased.
[0074] The PVA / AAm interface bonding method described in this embodiment comprises the following steps:
[0075] (1) Preparation of bonding liquid:
[0076] Oxidative bonding liquid: an aqueous solution containing 3M acrylamide (AAm), 0.03M polyethylene glycol diacrylate (PEGDA) and 0.006M potassium persulfate (KPS);
[0077] Reduction type adhesive solution: an aqueous solution containing 3M AAm, 0.03M PEGDA and 0.006M N,N,N',N'-tetramethylethylenediamine (TEMED);
[0078] The pre-prepared adhesive solution was stored in a refrigerator at 4°C to prevent the self-polymerization of the adhesive solution containing KPS at room temperature (25°C).
[0079] (2) The PVA / AAm hydrogel was cut into 15 mm × 50 mm blocks. Two pieces of PVA / AAm hydrogel were immersed in the oxidized and reduced adhesive solutions for 1-2 minutes respectively until swelling equilibrium was reached.
[0080] (3) The two pieces of PVA / AAm hydrogel after soaking were taken out and placed in a special mold. A heavy object (weight) was applied on top to make the two pieces of gel fit tightly. A pressure of 6.53 kPa was applied and the two pieces of gel were left under the pressure for 8 hours.
[0081] The chemical composition and reaction mechanism of the bonding liquid in this embodiment are as follows: Figure 1 ; Schematic diagram of interface bonding Figure 2 , which includes a bonding mold and a pressure-applying method; the PVA / AAm hydrogel obtained by the present invention after bonding is as follows Figure 3 .
[0082] The bonding cross section of the PVA / AAm hydrogel in this embodiment and the cross section of the PVA / AAm hydrogel after peeling are shown in FIG. Figure 4 , where the bonding cross section and its magnified image are shown in (ab), the peeled cross section and its magnified image are shown in (cd); the scanning electron microscope images of the cross section of the prepared soft material PVA / AAm hydrogel (left) and the cross section of the PVA / AAm hydrogel bonding interface (right) are compared as shown Figure 5 ; Scanning electron microscopy of the cross section of the interfacially bonded PVA / AAm hydrogel after peeling Figure 6 . Figure 4-6 This proves that the bonding layer generated by the bonding repair method in this embodiment has the characteristic of self-growth in thickness, and can achieve firm bonding of the interface of soft matter and repair damage to restore it to its original state.
[0083] Example 2
[0084] An embodiment of the damage repair method for soft matter of the present invention.
[0085] The soft material hydrogel for damage repair in this embodiment is PVA / Aam, and its preparation method is the same as that in Example 1.
[0086] The PVA / AAm interface bonding method described in this embodiment comprises the following steps:
[0087] (1) Soak the PVA / AAm hydrogel with a gap to be repaired in an adhesive solution for 1-2 minutes. The adhesive solution is an aqueous solution containing 3M AAm and 0.03M PEGDA;
[0088] (2) The PVA / AAm hydrogel after immersion was taken out, and an aqueous solution containing 0.006M KPS and an aqueous solution containing 0.006M TEMED were applied to the two ends of the gel to be repaired, respectively, and a pressure of 6.53 kPa was applied, and the gel was placed under pressure for 8 hours.
[0089] The schematic diagram of the present embodiment for repairing the missing damage and the damage filling effect of the hydrogel forming the adhesive layer are shown in the figure below. Figure 7 .
[0090] It can be seen that when the above-mentioned coating method is used for damage repair, the adhesive layer self-grows and fills the 0.5mm gap at the missing damage, thereby achieving the effect of repairing the missing damage.
[0091] Example 3
[0092] The only difference between Example 3 and Example 1 is that the oxidative initiator KPS in the oxidative adhesive solution is replaced with 0.006 M ammonium persulfate (APS).
[0093] Example 4
[0094] The only difference between Example 4 and Example 1 is that the reduced initiator TEMED in the reduced adhesive solution is replaced with 0.006 M dimethylacetamide (DMA).
[0095] Example 5
[0096] The only difference between Example 5 and Example 1 is that the oxidative initiator KPS in the oxidative and reduced bonding solutions is replaced with 0.006 M ammonium persulfate (APS), and the reduced initiator TEMED is replaced with 0.006 M dimethylacetamide (DMA).
[0097] Example 6
[0098] The only difference between Example 6 and Example 1 is that the oxidative initiator KPS in the oxidative and reduced bonding solutions is replaced with 0.006 M ammonium persulfate (APS), and the reduced initiator TEMED is replaced with 0.006 M tartaric acid (TA).
[0099] Example 7
[0100] The difference between Example 7 and Example 1 is that AAc / Aam hydrogel is prepared, and the cross-linking agent in the oxidized and reduced adhesive solutions is removed for bonding.
[0101] Comparative Example 1
[0102] The difference between Comparative Example 1 and Example 1 is that the polymerization bonding is completed by using redox primary initiation, ultraviolet initiation and thermal initiation respectively.
[0103] The redox primary initiation method is: mix equal volumes of oxidative adhesive and reducing adhesive, quickly put the hydrogel into the mixed solution and soak it for 3 minutes, take it out and put it into a special mold for bonding;
[0104] The UV initiation method is: using UV photoinitiator α-keto instead of KPS and TEMED, other parameters remain unchanged, and after the hydrogel has reached absorption equilibrium, it is placed in a mold and irradiated with a 365nm UV lamp in an argon environment of a glove box for bonding;
[0105] Thermal initiation is as follows: the hydrogel is placed in an oxidative adhesive solution, and after absorption equilibrium, it is placed in a special mold and bonded in an oven at 70°C.
[0106] Comparative Example 2
[0107] The difference between Comparative Example 2 and Example 1 is that the monomers and the crosslinking agent in the oxidized adhesive liquid and the reduced adhesive liquid are removed separately, that is, one adhesive liquid only contains the oxidized initiator or the reduced initiator.
[0108] Effect Example 1
[0109] In order to explore the firmness of the soft material interface bonding method and damage repair method provided by the present invention after bonding, the peel strength of the soft material obtained in Examples 1, 3-6 and Comparative Examples 1 and 2 after bonding was tested.
[0110] The peel strength results of the same PVA / AAm hydrogels in Examples 1 and 3-6 under different redox initiator combinations are as follows: Figure 8 .
[0111] Depend on Figure 8It can be seen that different redox initiators have different bonding effects on the AAm monomer system. Under the KPS / TEMED combination of Example 1, the peel strength of the PVA / AAm hydrogel after bonding is as high as 110N / m, which is the best and significantly higher than the combinations of other embodiments; under the APS / TEMED combination of Example 3, the peel strength of the PVA / AAm hydrogel after bonding is 57N / m, which is relatively high; and in Examples 4-6, the redox initiators are KPS / DMA, APS / DMA and APS / TA combinations, and the peel strengths of the PVA / AAm hydrogel after bonding are 5N / m, 8N / m and 13N / m, respectively.
[0112] The effect of bonding AAc / AAm hydrogel using bonding liquid without adding crosslinking agent in Example 7 is as follows: Fig. 9 .Depend on Fig. 9 It can be seen that removing the cross-linking agent can also achieve interfacial bonding of soft matter materials.
[0113] The peel strength results of hydrogels bonded by different initiation methods in Example 1 and Comparative Example 1 are as follows: Fig.10 .
[0114] Depend on Fig.10 It can be seen that the peel strength after bonding using the interface bonding method of Example 1 is as high as 110 N / m. Although its peel strength is lower than that of thermal initiation, it is still significantly better than UV initiation and redox one-time initiation. Compared with thermal initiation, the bonding method of the present invention is simpler to operate and can be carried out at room temperature in the air. At the same time, the peel strength is higher. Therefore, the initiation method of the present invention has certain advantages.
[0115] In Comparative Example 2, the thickness of the adhesive layer formed by using adhesive liquids with different components after peeling is as follows: Fig.11 The peel strength results after bonding with different adhesives in Example 1 and Comparative Example 2 are as follows Fig.12 .
[0116] Depend on Fig.11 , 12 It can be seen that: when immersed in the adhesive solution of different components in Comparative Example 2, the spontaneously grown adhesive layer mainly grows from the interface of the solution containing the monomer and the cross-linking agent, while the thickness of the interface growth containing a single oxidizing / reducing initiator after treatment is significantly lower; and compared with Example 1, the peel strength of Comparative Example 2 after bonding is significantly reduced.
[0117] Effect Example 2
[0118] In order to explore the influence of component concentration and reaction conditions on the bonding effect of soft material in the interface bonding and damage repair method of soft material provided by the present invention, the following effect exploration experiments were carried out respectively. The difference from the bonding method of Example 1 is only the change of a single variable:
[0119] ① Monomer concentration C in the adhesive solution M They are 1M, 1.5M, 2M, 2.5M, 3M, 3.5M and 7M respectively.
[0120] ②The bonding time is 1min, 5min, 10min, 30min, 1h, 2h, 4h and 12h respectively.
[0121] ③Concentration of crosslinking agent in adhesive solution C cro They are 0.003M, 0.006M, 0.015M, 0.03M, 0.06M, 0.09M, 0.12M, 0.15M, 0.3M (C cro C M The percentages are 0.1%, 0.2%, 0.5%, 1%, 2%, 3%, 4%, 5%, and 10% respectively).
[0122] ④The concentration of initiator in the adhesive liquid C ini They are 0.003M, 0.006M, 0.015M, 0.03M, 0.06M (C ini C M The percentages are 0.1%, 0.2%, 0.5%, 1% and 2% respectively).
[0123] ⑤ During the bonding process, five different moving distances of the mold were selected, and the strains of pressure applied to the hydrogel were 5%, 10%, 15%, 20%, and 25%, respectively.
[0124] The changes of the peel strength (a), bonding layer thickness (b), Young's modulus (c), and bonding layer toughness (d) of PVA / AAm hydrogel after bonding with the change of monomer concentration are shown in Figure 2. Fig.13 .Depend on Fig.13 It can be seen that the peel strength, adhesive layer thickness, Young's modulus and adhesive layer toughness all increase with the increase of monomer concentration, and the maximum Young's modulus can reach 130 kPa.
[0125] The peel strength (a) and bonding layer thickness (b) of PVA / AAm hydrogel after bonding at different bonding times. Fig.14 .Depend on Fig.14 It can be seen that the peel strength and the thickness of the adhesive layer should increase with the increase of the bonding time t, and stop increasing with the end of the monomer polymerization reaction, reaching equilibrium within 2 hours, at which time the peel strength reaches 110N / m and the thickness of the adhesive layer reaches 900μm.
[0126] The relationship between the Young's modulus and crosslinker concentration of the bonding layer formed after bonding PVA / AAm hydrogel at different crosslinker concentrations (a), and the relationship between the peel strength and Young's modulus (b) Fig.15 .Depend on Fig.15 It can be seen that the peel strength after bonding shows a trend of first increasing and then decreasing with the increase of crosslinking agent concentration. cro / C M The peel strength is strongest when the cross-linking agent concentration is about 1% (concentration 0.03M); Young's modulus increases with the increase of cross-linking agent concentration, reaching a maximum of 180kPa; the cross-linking agent concentration has little effect on the thickness of the adhesive layer.
[0127] The peel strength (a) and bonding layer thickness (b) of PVA / AAm hydrogel bonded with adhesive solutions of different initiator concentrations are shown in Figure 2. Fig.16 Different C ini / C M % Peel strength changes with bonding time Fig.17 , (a) 0.1%; (b) 0.5%; (c) 1%; (d) 2%. Fig.16 , 17 It can be seen that the relationship between peel strength and initiator concentration shows a trend of first increasing and then balancing. ini / C M When the initiator concentration is about 0.2% (concentration 0.006M), the equilibrium is reached; when the initiator concentration is too low, some monomers do not react, so the thickness of the formed bonding layer is low. When the initiator concentration reaches the threshold for sufficient monomer reaction, the thickness of the bonding layer can no longer grow and tends to be stable.
[0128] The self-grown adhesive peel strength and adhesive layer thickness of PVA / AAm hydrogel after normalization treatment under different strains are shown in Figure 2. Fig.18 .Depend on Fig.18 It can be seen that: as the strain changes are controlled differently, the peel strength and the thickness of the adhesive layer remain basically unchanged.
[0129] In summary, under the component concentrations and reaction conditions specified in the present invention, better soft material interface bonding and damage repair effects can be achieved.
[0130] Effect Example 3
[0131] In order to explore the bonding effects of different monomer systems of the interface bonding and damage repair method of soft material provided by the present invention on different soft material materials, the following effect exploration experiments were carried out respectively, wherein the interface bonding method only controlled the corresponding variables to change, and the rest was the same as Example 1:
[0132] ① The PVA / AAm hydrogel prepared in Example 1 was bonded with the following seven different gel materials: polyacrylamide (pAAm), poly N-isopropylacrylamide (pNIPAM), polyhydroxyethyl methyl acrylate (pHEMA), polyacrylamide / sodium alginate [p(AAm / SA)], polyacrylamide / poly 2-acrylamido-2-methylpropane sulfonic acid (pAAm / pAMPS), polyacrylamide-co-acrylic acid p (AAm-co-AAc) and poly N,N-dimethylacrylamide (pDMA).
[0133] ② The following four different monomers and monomer combinations were used to prepare the adhesive liquid: methacrylamide (MAAm), hydroxyethyl methyl acrylate (HEMA), acrylamide-acrylic acid (AAm-AAc) and methacrylamide-methacrylic acid (MAAm-MAAc).
[0134] ③ Using a bonding liquid with a hydroxyethyl acrylate (HEA) monomer system, PVA / AAm gel was bonded to the following five different soft materials: polyurethane (PU), acrylonitrile-butadiene-styrene copolymer resin (ABS), polycarbonate (PC), polyvinyl chloride (PVC) and nitrile rubber (NBR).
[0135] The peeling curves (a) and peeling strengths (b) of PVA / AAm hydrogel after bonding with seven gel materials are shown in Figure 2. Fig.19 .Depend on Fig.19 It can be seen that: using the bonding method of the present invention, PVA / AAm hydrogel can be effectively bonded to 7 kinds of gel materials, and the highest peel strength can reach more than 150N / m.
[0136] The peel strength results after bonding PVA / AAm hydrogel using adhesive solutions with different monomer systems are as follows: Fig. 20 .Depend on Fig. 20 It can be seen that different monomer systems can achieve effective bonding of PVA / AAm hydrogel, and the peel strength of the MAAm-MAAc system can reach up to 180N / m or more.
[0137] The peel strength results of PVA / AAm gel and five soft materials bonded by HEA monomer system adhesive are shown in the figure. Fig.21 .Depend on Fig.21 It can be seen that the peel strength of the five soft materials after bonding with PVA / AAm gel is between 45 and 68 N / m, among which the peel strength between PU and gel is the lowest at 45 N / m, and the peel strength between NBR and gel is the highest at 68 N / m.
[0138] In summary, the self-diffusion growth bonding method can achieve effective bonding between different soft materials under the different monomer systems defined in the present invention, and has excellent universality.
[0139] Effect Example 4
[0140] In order to explore the influence of the interface bonding and damage repair method of the soft material provided by the present invention on the self-growing bonding performance under the external "transmission channel", the following tests were conducted:
[0141] The interface bonding method of the soft material in Example 1 was used, except that the porous material film was fully wetted in deionized water, and the wetted film was placed between the two PVA / AAm hydrogels to be bonded during bonding to serve as a "transmission channel". Experiments were conducted using different porous material films as shown in Table 1 to observe the formation of the bonding layer and measure the peel strength after bonding. The experimental steps and results are shown in FIG. Fig. 22 .
[0142] Depend on Fig. 22 It can be seen that: when the film at the hydrogel interface is a PE film or a UM film, the diffusion channel at the interface is too small, and the adhesive liquid on both sides cannot diffuse to the other side in a short time to react; when it is a PE film, the PVA / AAm hydrogel does not observe the formation of an adhesive layer after 24 hours; when it is a UM film, after 24 hours, the adhesive liquid only generates an adhesive layer on the film, and the adhesive layer grows alone and is not connected to the hydrogel body, and the peel strength is only 10N / m. When the pore size of the film at the hydrogel interface is greater than a certain value, that is, when the transmission membrane is MF, Nylon, or FP membrane, the peel strength is higher, which is almost the same as the blank sample without any film. Therefore, based on the above results, it is inferred that when the membrane pore size is large enough and does not affect the diffusion rate of the adhesive liquid molecules, the interface film will not seriously affect the formation of the adhesive layer and the peel strength of the gel. Therefore, the interface bonding method of the present invention can also be further used to prepare composite materials.
[0143] Table 1 Parameters of different porous materials used in the present invention
[0144] film Abbreviation Aperture Polyethylene film PE <0.1nm Molecular Retention Membrane UM 7nm Water filtration membrane MF 0.45μm Nylon mesh (800 mesh) Nylon 18μm Qualitative filter paper FP 100μm
[0145] Effect Example 5
[0146] In order to explore the repair effect of the interface bonding and damage repair method of the soft material provided by the present invention on defect-type damage of different damage shapes and different thicknesses, the following tests were performed respectively:
[0147] ① The method in Example 1 was used to bond and repair the PVA / AAm hydrogel cut using molds of different shapes, and the gel was stained with a 1% concentration of rhodamine stain to further observe the repair effect.
[0148] ② The method in Example 2 was used to repair missing damage of multiple thicknesses, namely 0.1 mm, 1 mm, and 2 mm.
[0149] The results of PVA / AAm hydrogel repair under different damage shapes are shown in Figure 2. Fig.23 . Among them, (a) heart-shaped; (b) circular; (c) pentagonal; (d) star-shaped; (e) rectangular. Fig.23 It can be seen that the soft material interface bonding and damage repair method provided by the present invention can achieve effective bonding and repair of missing damage of various shapes. It can be observed that a transparent polymer layer appears between the two gels being bonded, and this layer is the bonding layer grown by the bonding liquid on the interface of the two gels. And the repaired PVA / AAm hydrogel is moderately stretched, and the bonding between the two gels is firm, and under moderate strain, there will be no separation phenomenon.
[0150] The effects of PVA / AAm hydrogel before and after repair of defect injuries of different widths Fig.24 ; The tensile curves (a) and conductivity (b) of different width defect damage before and after repair are shown in Figure 2. Fig.25 ; Nernst plots of PVA / AAm hydrogel before and after repair of different width injuries Fig.26 .
[0151] Depend on Figure 24-26 It can be seen that the self-diffusion growth bonding method can achieve ideal repair effects for the repair of missing damage with a width of 0.1-2mm. After the damage is repaired, a transparent bonding layer is generated to fill the damage. Moreover, after the repair of missing damage of each width, the tensile properties of the PVA / AAm hydrogel are significantly better than the tensile properties before the repair, and the performance has been significantly improved. In addition, the Young's modulus of the PVA / AAm hydrogel with missing damage of different widths after repair is similar, and the difference is large compared with the Young's modulus of the gel before repair, indicating that the polymerization of AAm monomers during the repair process will increase the Young's modulus of the gel. And the conductivity of the PVA / AAm hydrogel with missing damage of different widths after repair is also improved. The increase in Young's modulus and conductivity further illustrates that the self-diffusion growth bonding method can achieve good repair of missing damage of different widths.
[0152] In summary, the two interface bonding and damage repair methods provided by the present invention can both achieve effective self-diffusion growth bonding, have good repair effects on damage of different shapes and missing damage of larger thickness, and even improve the performance of soft materials, with good adaptability and strong practicality.
[0153] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for interfacial bonding and damage repair of soft materials, characterized in that: One of (a) and (b): (a) soaking the soft material in adhesive liquid a respectively until swelling equilibrium is reached, taking out and bonding them, applying pressure, and forming an adhesive layer by self-growth at the interface; the adhesive liquid a comprises a monomer and an initiator; the adhesive liquid a is divided into an oxidized adhesive liquid and a reduced adhesive liquid; (b) soaking the soft material in adhesive solution b until swelling equilibrium is reached, taking it out and coating it with initiator solution respectively, attaching it to the coating part, applying pressure, and forming an adhesive layer by self-growth at the interface; the adhesive solution b comprises a monomer; The initiator is an oxidative initiator or a reducing initiator; The thickness of the adhesive layer is 5 μm-1.1 mm; The monomer is at least one of the following general formula (I) and general formula (II): The general formula (I) is The R1 is hydrogen or methyl; R2 is hydrogen, and R3 is one of hydrogen, C1-C18 alkyl and its isomers, phenyl, chlorophenyl, phenol, butoxymethyl, benzyl, hydroxyethyl, hydroxyphenyl, dimethylaminopropyl, methylpropanesulfonic acid, and benzenesulfonic acid; or R2 and R3 are each independently one of C1-C4 alkyl and acetonyl; or R2 is methyl, and R3 is ethyl; The general formula (II) is The R4 is hydrogen or methyl; The R5 is one of hydrogen, C1-C20 alkyl and isomers thereof, hydroxyethyl, ethyltrimethylammonium chloride, C1-C20 perfluoroalkyl, benzyl, phenyl, bornyl, and tetrahydrofuranyl.
2. The method for interfacial bonding and damage repair of soft matter materials according to claim 1, characterized in that: The adhesive liquid a and the adhesive liquid b also include a cross-linking agent.
3. The method for interfacial bonding and damage repair of soft materials according to claim 1, characterized in that: The oxidative initiator is at least one of ammonium persulfate, sodium persulfate, formic acid peroxide, calcium peroxyphosphate, potassium persulfate, and potassium peroxymonosulfate; the reducing initiator is at least one of ferrous chloride, ferrous sulfate, cuprous chloride, NaHSO3, Na2SO3, Na2S2O3, tartaric acid, and glucose; Or the oxidative initiator is at least one of dialkyl peroxide, cyclohexanone peroxide, isopropylbenzene hydroperoxide, tert-butyl hydroperoxide, acetone peroxide, tert-butyl ketone peroxide, benzophenone peroxide, di(2,4-dichlorobenzoyl) peroxide, and diisopropylbenzene peroxide, and the reducing initiator is at least one of formic acid, sulfonic acid, trialkyl boron, diisobutylonitrile hydrazine, tertiary amine, cyclopentane salt, thiol, and organic metal compound.
4. The method for interfacial bonding and damage repair of soft matter materials according to claim 1, characterized in that: The applied pressure is 0.04-1000 kPa.
5. The method for interfacial bonding and damage repair of soft materials according to claim 1, characterized in that: The bonding time is 1 min-12 h.
6. The method for interfacial bonding and damage repair of soft matter materials according to claim 1, characterized in that: The oxidative bonding solution includes the following components in concentrations: 0.5-7M monomer, 0.0005-0.14M oxidative initiator; The reduced bonding liquid comprises the following components in concentrations: 0.5-7M monomer, 0.0005-0.14M reduced initiator; The concentration of the monomer in the adhesive liquid b is 0.5-7M; The concentration of the oxidative initiator or the reduced initiator in the initiator solution is 0.1-0.7M.
7. The method for interfacial bonding and damage repair of soft materials as claimed in claim 2, characterized in that: The concentration of the cross-linking agent is 0.0005-0.7M.
8. The method for interfacial bonding and damage repair of soft materials according to claim 1, characterized in that: In the oxidized adhesive solution or the reduced adhesive solution, the molar concentration ratio of the crosslinking agent to the monomer is (0.01-0.02):
1.
9. The method for interfacial bonding and damage repair of soft matter materials as claimed in claim 1, characterized in that: In the oxidized adhesive solution or the reduced adhesive solution, the molar concentration ratio of the initiator to the monomer is (0.002-0.005):
1.
10. Use of the interface bonding and damage repair method of the soft matter material according to any one of claims 1 to 9 in repairing missing damage of gel materials, repairing damage of ion conductive gels and preparing interface coating composite materials.