AB glue applied to under-screen fingerprint unlocking mobile phone screen and preparation method thereof

By using AB glue composed of hydrophobic modified epoxy resin and antistatic modified PMMA in the under-screen fingerprint unlocking application of mobile phones, the problem of low light transmittance of traditional AB glue is solved, and the sensitivity and bonding strength of fingerprint recognition are improved. , ensuring high light transmittance and anti-static properties.

CN118978874APending Publication Date: 2024-11-19TAIHU JINZHANG TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410977953.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the application of under-screen fingerprint unlocking on mobile phones, the low light transmittance leads to weakening of reflected light intensity, affecting the collection of fingerprint recognition signals and resulting in insensitive unlocking.

Method used

AB glue composed of the first release film layer, a silicone layer, a high-transmittance anti-static substrate layer and an acrylic adhesive layer is adopted. The silicone layer contains a hydrophobic modified epoxy resin, and the high-transmittance anti-static substrate layer is Antistatically modified PMMA-coated PET films improve light transmittance and bond strength through these hierarchies.

Benefits of technology

It improves the sensitivity of fingerprint recognition, avoids the generation of bubbles during bonding, enhances the bonding strength and anti-static properties, and ensures high light transmittance and good anti-static properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978874A_ABST
    Figure CN118978874A_ABST
Patent Text Reader

Abstract

The invention discloses AB glue applied to an under-screen fingerprint unlocking mobile phone screen and a preparation method of the AB glue, and belongs to the technical field of AB glue, the prepared AB glue sequentially comprises a first release film layer, a silica gel layer, a high-light-transmittance anti-static base material layer, an acrylic acid glue layer and a second release film layer from top to bottom, hydrophobic modified epoxy resin is prepared through reaction of monoamino polysiloxane and epoxy resin. The high-light-transmittance anti-static base material layer is formed by coating the surface of a PET (Polyethylene Terephthalate) film with anti-static modified PMMA (Polymethyl Methacrylate), and the anti-static modified PMMA is prepared by reacting 3-sulfonic acid propyl potassium methacrylate and a methyl methacrylate monomer. The silica gel layer and the acrylic acid adhesive layer are coated on the surface of the high-light-transmittance anti-static base material layer, and the high-light-transmittance anti-static base material layer is attached to the release film to form the AB adhesive with a five-layer structure, so that the AB adhesive prepared by the invention has high light transmittance and good anti-static performance, is not easy to generate bubbles during attachment, and is flat in attachment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of AB glue, and specifically relates to AB glue used for under-screen fingerprint unlocking of a mobile phone screen and a preparation method thereof. Background Art

[0002] Fingerprint recognition unlocking has become the default function of most smartphones today. However, the fingerprint collection window required for traditional fingerprint unlocking affects the screen-to-body ratio of the phone to a certain extent. As full-screen smartphones become mainstream, more "invisible" under-screen fingerprint recognition has flooded the market. Mobile phones with under-screen fingerprint recognition capabilities can directly complete the fingerprint recognition process by pressing the specified area of ​​the phone screen. The principle is to use the refraction and reflection of light. When a finger presses the screen, the screen emits light to illuminate the finger area. The reflected light that illuminates the fingerprint passes through the gap between the screen pixels and returns to the sensor close to the screen. The acquired fingerprint image is compared with the image initially recorded by the phone, and finally the recognition judgment is made.

[0003] In addition, with the development of mobile phone protective films, there are many types of mobile phone screen protective films on the market, which are generally transparent thin film materials attached to the screen by static electricity and adhesives. Tempered glass film, also known as tempered glass film, diamond film, strengthened glass film, explosion-proof glass film, is a new type of screen protection material. Tempered film is mainly bonded to the mobile phone screen through AB glue. AB glue is a PET-based film with acrylic glue on one side and silicone on the other side. Acrylic glue is used to fit tempered glass, while silicone is used to fit the surface of the mobile phone because it can automatically exhaust. However, if used improperly or inappropriate AB glue is selected, the tempered film on the surface of the mobile phone screen may seriously affect the transmittance of light and reflected light, making the reflected light intensity weaker, causing the signal collected by the sensor to weaken, and the unlocking will be insensitive. Summary of the invention

[0004] The purpose of the present invention is to provide an AB glue for unlocking a mobile phone screen with fingerprint under the screen and a preparation method thereof, so as to improve the light transmittance of the AB glue.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] The present invention provides an AB glue for fingerprint unlocking of a mobile phone screen under the screen, which comprises, from top to bottom, a first release film layer, a silicone layer, a high-transmittance antistatic substrate layer, an acrylic glue layer, and a second release film layer;

[0007] The silica gel layer comprises the following raw materials by weight: 80-100 parts of organic silicone resin, 0.1-1 parts of cross-linking agent, 0.5-5 parts of catalyst, 0.1-3 parts of anchoring agent and 10-25 parts of hydrophobically modified epoxy resin;

[0008] Furthermore, the high-transmittance antistatic substrate layer is a PET film surface coated with antistatic modified PMMA.

[0009] Furthermore, the thickness of the PET film in the high-transmittance antistatic substrate layer is 5-20 μm, and the total thickness of the substrate layer is 10-50 μm.

[0010] Furthermore, the first release film layer is a silicon-free release film, and the second release film layer is a silicon-containing release film.

[0011] Furthermore, the cross-linking agent is hydrogen-containing silicone oil.

[0012] Furthermore, the catalyst is a platinum catalyst.

[0013] Furthermore, the anchoring agent is one of MSK-SC0929S and MSK-SC0930S-4.

[0014] Further, the preparation of the hydrophobically modified epoxy resin is as follows:

[0015] Add monoaminopolysiloxane and butyl acetate to the reaction kettle, mix and stir for 30 minutes, then add epoxy resin, stir for 10 minutes, evacuate and heat to 50°C, continue stirring and react for 1 hour, and obtain hydrophobically modified epoxy resin after removing the solvent. The amount of monoaminopolysiloxane added is 2% of the mass of the epoxy resin, and the amount of butyl acetate added is 30% of the mass of the epoxy resin;

[0016] The monoaminopolysiloxane is TEGO Phobe1505 functional polysiloxane solution.

[0017] Furthermore, the preparation of the antistatic modified PMMA is as follows:

[0018] Methyl methacrylate and azobisisoheptanenitrile are mixed to obtain solution A, in which the mass proportion of azobisisoheptanenitrile is 5%. 3-sulfonate propyl methacrylate potassium salt and 2-hydroxypropyl acrylate are ultrasonically dispersed to obtain solution B, in which the mass proportion of 3-sulfonate propyl methacrylate potassium salt is 8%. Solution A and solution B are mixed and ultrasonically treated for 120 minutes to obtain a mixed solution, in which the mass ratio of 2-hydroxypropyl acrylate to methyl methacrylate is 1:9. The reaction is continued at 80°C for 20 minutes, then cooled to -10°C, stirred for 10 minutes, vacuumed, reacted at 60°C for 3 hours, and then heated to 100°C for 1 hour to obtain antistatic modified PMMA.

[0019] The present invention also provides a method for preparing AB glue for unlocking a mobile phone screen with fingerprint under the screen, comprising the following steps:

[0020] S1, coating the antistatic modified PMMA on the surface of the PET film to obtain a high-transmittance antistatic substrate layer;

[0021] S2, mixing and stirring an organic silicone resin, a cross-linking agent, an anchoring agent, a catalyst and a hydrophobically modified epoxy resin to obtain a silicone layer raw material, coating the silicone layer raw material on the upper surface of the high-transmittance antistatic substrate layer, and obtaining a silicone layer after curing;

[0022] S3, coating acrylic glue on the lower surface of the high-transmittance antistatic substrate layer, and obtaining an acrylic glue layer after curing;

[0023] S4. Attach a release film on the silicone layer and attach a release film on the bottom of the acrylic adhesive layer to obtain AB adhesive.

[0024] Beneficial effects of the present invention:

[0025] (1) The addition of hydrophobically modified epoxy resin to the silicone layer in the AB glue prepared by the present invention can improve the bonding strength and hydrophobicity of the silicone layer, avoid the formation of bubbles when laminating on the surface of the mobile phone screen and affect the laminating flatness, and further improve the sensitivity of fingerprint recognition.

[0026] (2) The substrate layer of the AB glue prepared by the present invention is a PET film coated with antistatic modified PMMA. PMMA has high transparency, high mechanical strength and low price, but poor conductivity. Antistatic modification can suppress static electricity accumulation during long-term use and prevent the adsorption of dust, so that the substrate layer has high light transmittance and good antistatic performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The present invention will be further described below in conjunction with the accompanying drawings.

[0028] Figure 1 It is a schematic diagram of the structure of the AB glue prepared by the present invention. DETAILED DESCRIPTION

[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1

[0031] Preparation of hydrophobically modified epoxy resin: monoaminopolysiloxane and butyl acetate were added to the reaction kettle, and the epoxy resin was added after mixing and stirring for 30 minutes. After stirring for 10 minutes, the mixture was evacuated and heated to 50°C, and the stirring reaction was continued for 1 hour. After removing the solvent, the modified epoxy resin was obtained. The amount of monoaminopolysiloxane added was 2% of the mass of the epoxy resin, and the amount of butyl acetate added was 30% of the mass of the epoxy resin.

[0032] Preparation of antistatic modified PMMA: Methyl methacrylate and azobisisoheptanenitrile are mixed to obtain solution A, in which the mass proportion of azobisisoheptanenitrile is 5%. 3-sulfonate propyl methacrylate potassium salt and 2-hydroxypropyl acrylate are ultrasonically dispersed to obtain solution B, in which the mass proportion of 3-sulfonate propyl methacrylate potassium salt is 8%. Solution A and solution B are mixed and ultrasonically treated for 120 minutes to obtain a mixed solution, in which the mass ratio of 2-hydroxypropyl acrylate to methyl methacrylate is 1:9. The reaction is continued at 80°C for 20 minutes, then the temperature is lowered to -10°C, stirred for 10 minutes, and then vacuumed. The reaction is carried out at 60°C for 3 hours, and then heated to 100°C for 1 hour to obtain antistatic modified PMMA.

[0033] Preparation of AB glue:

[0034] S1, coating the antistatic modified PMMA on the surface of a PET film with a thickness of 5 μm to obtain a high-transmittance antistatic substrate layer with a total thickness of 10 μm;

[0035] S2, 100 parts of organic silicone resin, 1 part of hydrogen-containing silicone oil, 3 parts of MSK-SC0929S anchoring agent, 5 parts of platinum catalyst and 10 parts of hydrophobically modified epoxy resin are mixed and stirred to obtain a silica gel layer raw material, and the silica gel layer raw material is coated on the upper surface of the high-transmittance antistatic substrate layer, and the silica gel layer is obtained after curing;

[0036] S3, coating acrylic glue on the lower surface of the high-transmittance antistatic substrate layer, and obtaining an acrylic glue layer after curing;

[0037] S4. A PET non-silicone release film is laminated on the silicone layer, and a silicone-containing PET release film is laminated on the acrylic adhesive layer to obtain AB adhesive.

[0038] Example 2

[0039] The difference from Example 1 is that the amount of the hydrophobically modified epoxy resin in the silica gel layer is increased from 10 parts to 20 parts, and the other steps are the same as Example 1.

[0040] Example 3

[0041] The difference from Example 1 is that the hydrophobically modified epoxy resin in the silica gel layer is increased from 10 parts to 25 parts, and the other steps are the same as Example 1.

[0042] Example 4

[0043] The difference from Example 1 is that the antistatic modified PMMA is coated on the surface of a PET film with a thickness of 5 μm to obtain a high-transmittance antistatic substrate layer with a total thickness of 20 μm. The other steps are the same as Example 1.

[0044] Example 5

[0045] The difference from Example 1 is that the antistatic modified PMMA is coated on the surface of a PET film with a thickness of 5 μm to obtain a high-transmittance antistatic substrate layer with a total thickness of 25 μm. The other steps are the same as Example 1.

[0046] Example 6

[0047] Preparation of hydrophobically modified epoxy resin: monoaminopolysiloxane and butyl acetate were added to the reaction kettle, and the epoxy resin was added after mixing and stirring for 30 minutes. After stirring for 10 minutes, the mixture was evacuated and heated to 50°C, and the stirring reaction was continued for 1 hour. After removing the solvent, the modified epoxy resin was obtained. The amount of monoaminopolysiloxane added was 2% of the mass of the epoxy resin, and the amount of butyl acetate added was 30% of the mass of the epoxy resin.

[0048] Preparation of antistatic modified PMMA: Methyl methacrylate and azobisisoheptanenitrile are mixed to obtain solution A, in which the mass proportion of azobisisoheptanenitrile is 5%. 3-sulfonate propyl methacrylate potassium salt and 2-hydroxypropyl acrylate are ultrasonically dispersed to obtain solution B, in which the mass proportion of 3-sulfonate propyl methacrylate potassium salt is 8%. Solution A and solution B are mixed and ultrasonically treated for 120 minutes to obtain a mixed solution, in which the mass ratio of 2-hydroxypropyl acrylate to methyl methacrylate is 1:9. The reaction is continued at 80°C for 20 minutes, then the temperature is lowered to -10°C, stirred for 10 minutes, and then vacuumed. The reaction is carried out at 60°C for 3 hours, and then heated to 100°C for 1 hour to obtain antistatic modified PMMA.

[0049] Preparation of AB glue:

[0050] S1, coating the antistatic modified PMMA on the surface of a PET film with a thickness of 5 μm to obtain a high-transmittance antistatic substrate layer with a total thickness of 10 μm;

[0051] S2, 90 parts of organic silicone resin, 0.5 parts of hydrogen-containing silicone oil, 2 parts of MSK-SC0930S-4 anchoring agent, 3 parts of platinum catalyst and 10 parts of hydrophobically modified epoxy resin are mixed and stirred to obtain a silica gel layer raw material, and the silica gel layer raw material is coated on the upper surface of the high-transmittance antistatic substrate layer, and the silica gel layer is obtained after curing;

[0052] S3, coating acrylic glue on the lower surface of the high-transmittance antistatic substrate layer, and obtaining an acrylic glue layer after curing;

[0053] S4. A PET non-silicone release film is laminated on the silicone layer, and a silicone-containing PET release film is laminated on the acrylic adhesive layer to obtain AB adhesive.

[0054] Example 7

[0055] Preparation of hydrophobically modified epoxy resin: monoaminopolysiloxane and butyl acetate were added to the reaction kettle, and the epoxy resin was added after mixing and stirring for 30 minutes. After stirring for 10 minutes, the mixture was evacuated and heated to 50°C, and the stirring reaction was continued for 1 hour. After removing the solvent, the modified epoxy resin was obtained. The amount of monoaminopolysiloxane added was 2% of the mass of the epoxy resin, and the amount of butyl acetate added was 30% of the mass of the epoxy resin.

[0056] Preparation of antistatic modified PMMA: Methyl methacrylate and azobisisoheptanenitrile are mixed to obtain solution A, in which the mass proportion of azobisisoheptanenitrile is 5%. 3-sulfonate propyl methacrylate potassium salt and 2-hydroxypropyl acrylate are ultrasonically dispersed to obtain solution B, in which the mass proportion of 3-sulfonate propyl methacrylate potassium salt is 8%. Solution A and solution B are mixed and ultrasonically treated for 120 minutes to obtain a mixed solution, in which the mass ratio of 2-hydroxypropyl acrylate to methyl methacrylate is 1:9. The reaction is continued at 80°C for 20 minutes, then the temperature is lowered to -10°C, stirred for 10 minutes, and then vacuumed. The reaction is carried out at 60°C for 3 hours, and then heated to 100°C for 1 hour to obtain antistatic modified PMMA.

[0057] Preparation of AB glue:

[0058] S1, coating the antistatic modified PMMA on the surface of a PET film with a thickness of 5 μm to obtain a high-transmittance antistatic substrate layer with a total thickness of 10 μm;

[0059] S2, 80 parts of organic silicone resin, 0.1 parts of hydrogen-containing silicone oil, 0.1 parts of MSK-SC0929S anchoring agent, 0.5 parts of platinum catalyst and 10 parts of hydrophobically modified epoxy resin are mixed and stirred to obtain a silica gel layer raw material, and the silica gel layer raw material is coated on the upper surface of the high-transmittance antistatic substrate layer, and the silica gel layer is obtained after curing;

[0060] S3, coating acrylic glue on the lower surface of the high-transmittance antistatic substrate layer, and obtaining an acrylic glue layer after curing;

[0061] S4. A PET non-silicone release film is laminated on the silicone layer, and a silicone-containing PET release film is laminated on the acrylic adhesive layer to obtain AB adhesive.

[0062] Comparative Example 1

[0063] The difference between this comparative example and Example 1 is that no hydrophobic modified resin is added to the silica gel layer, and the other compositions and steps are the same as Example 1.

[0064] Comparative Example 2

[0065] The difference between this comparative example and Example 1 is that the hydrophobic modified resin in the silica gel layer is replaced by epoxy resin, and the other compositions and steps are the same as Example 1.

[0066] Comparative Example 3

[0067] The difference between this comparative example and Example 1 is that the high-transmittance antistatic substrate layer is replaced by a PET film with a film thickness of 10 μm, and the other compositions and steps are the same as Example 1.

[0068] Comparative Example 4

[0069] The difference between this comparative example and Example 1 is that the high-transmittance antistatic substrate layer is replaced by a PMMA-coated PET film, the PET film has a thickness of 5 μm, the total thickness of the substrate layer is 10 μm, and the other compositions and steps are the same as Example 1.

[0070] The AB glue prepared in Examples 1 to 7 and Comparative Examples 1 to 4 was used to adhere the tempered film to the surface of the under-screen fingerprint unlocking mobile phone screen, and performance tests were performed. The results are shown in Table 1.

[0071] The adhesion performance test refers to "GB / T 2792-2014 Test method for peel strength of adhesive tape".

[0072] Table 1

[0073]

[0074]

[0075] As can be seen from Table 1, the increase of the hydrophobically modified epoxy resin in the silicone layer of Example 3 can improve the adhesion of the silicone layer, and the improvement of the hydrophobic performance can also prevent the surface of the silicone layer from absorbing moisture, reducing the generation of bubbles. The AB glue prepared in Example 4 and Example 5 has better antistatic properties than Example 1, and can effectively reduce the bubbles caused by the adsorption of dust on the glue surface. In Example 6 and Example 7, the proportion of silicone resin is reduced, and its adhesion is slightly improved. Compared with Example 1, the residual bubbles in Comparative Example 1 and Comparative Example 2 are significantly increased, which is not conducive to the flatness of the AB glue prepared by the present invention, and the transmittance is slightly reduced. In Comparative Example 3, PET film is used as the substrate layer, and its antistatic performance and transmittance are significantly worse than those in Example 1. The PMMA in Comparative Example 4 is not antistatically modified, and the antistatic performance of the substrate layer is poor, which affects the discharge of bubbles during bonding.

[0076] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0077] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An AB glue used for fingerprint unlocking of mobile phone screen under the screen, characterized in that: From top to bottom, it includes a first release film layer, a silicone layer, a high-transmittance antistatic substrate layer, an acrylic adhesive layer, and a second release film layer; The silica gel layer comprises the following raw materials by weight: 80-100 parts of organic silicone resin, 0.1-1 parts of cross-linking agent, 0.5-5 parts of catalyst, 0.1-3 parts of anchoring agent and 10-25 parts of hydrophobically modified epoxy resin.

2. The AB glue for unlocking a mobile phone screen with fingerprint under the screen according to claim 1, characterized in that: The high-transmittance antistatic substrate layer is a PET film with antistatic modified PMMA coated on its surface.

3. The AB glue for unlocking a mobile phone screen with fingerprint under the screen according to claim 1, characterized in that: The thickness of the PET film in the high-transmittance antistatic substrate layer is 5-20 μm, and the total thickness of the substrate layer is 10-50 μm.

4. The AB glue for unlocking a mobile phone screen with fingerprint under the screen according to claim 1, characterized in that: The first release film layer is a silicon-free release film, and the second release film layer is a silicon-containing release film.

5. The AB glue for unlocking a mobile phone screen with fingerprint under the screen according to claim 1, characterized in that: The cross-linking agent is hydrogen-containing silicone oil.

6. The AB glue for unlocking a mobile phone screen with fingerprint under the screen according to claim 1, characterized in that: The catalyst is a platinum catalyst.

7. The AB glue for unlocking a mobile phone screen with fingerprint under the screen according to claim 1, characterized in that: The anchoring agent is one of MSK-SC0929S and MSK-SC0930S-4.

8. The AB glue for unlocking a mobile phone screen with fingerprint under the screen according to claim 1, characterized in that: The preparation of the hydrophobically modified epoxy resin is as follows: Add monoaminopolysiloxane and butyl acetate to the reaction kettle, mix and stir for 30 minutes, then add epoxy resin, stir for 10 minutes, evacuate and heat to 50°C, continue stirring and react for 1 hour, and obtain hydrophobically modified epoxy resin after removing the solvent. The amount of monoaminopolysiloxane added is 2% of the mass of the epoxy resin, and the amount of butyl acetate added is 30% of the mass of the epoxy resin; The monoaminopolysiloxane is Phobe1505 functional polysiloxane solution.

9. The AB glue for unlocking a mobile phone screen with fingerprint under the screen according to claim 1, characterized in that: The preparation of the antistatic modified PMMA is as follows: Methyl methacrylate and azobisisoheptanenitrile are mixed to obtain solution A, in which the mass proportion of azobisisoheptanenitrile is 5%. 3-sulfonate propyl methacrylate potassium salt and 2-hydroxypropyl acrylate are ultrasonically dispersed to obtain solution B, in which the mass proportion of 3-sulfonate propyl methacrylate potassium salt is 8%. Solution A and solution B are mixed and ultrasonically treated for 120 minutes to obtain a mixed solution, in which the mass ratio of 2-hydroxypropyl acrylate to methyl methacrylate is 1:

9. The reaction is continued at 80°C for 20 minutes, then cooled to -10°C, stirred for 10 minutes, vacuumed, reacted at 60°C for 3 hours, and then heated to 100°C for 1 hour to obtain antistatic modified PMMA.

10. A method for preparing AB glue for unlocking a mobile phone screen with fingerprint under the screen as described in claims 1-9, characterized in that: The following steps are involved: S1, coating the antistatic modified PMMA on the surface of the PET film to obtain a high-transmittance antistatic substrate layer; S2, mixing and stirring an organic silicone resin, a cross-linking agent, an anchoring agent, a catalyst and a hydrophobically modified epoxy resin to obtain a silicone layer raw material, coating the silicone layer raw material on the upper surface of the high-transmittance antistatic substrate layer, and obtaining a silicone layer after curing; S3, coating acrylic glue on the lower surface of the high-transmittance antistatic substrate layer, and obtaining an acrylic glue layer after curing; S4. Attach a release film on the silicone layer and attach a release film on the bottom of the acrylic adhesive layer to obtain AB adhesive.

Citation Information

Cited By

  • Protective film for mobile phone screen and preparation method thereof

    CN120399594A