Preparation method of hot-pressed block of biomass coal
The hot-pressing method solves the problem of low energy density of biomass coal in the ironmaking process, producing high-density biomass coal and improving the energy utilization efficiency and environmental performance of the coking process.
Patent Information
- Application Number
- CN202411056592.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
Existing technologies have not fully considered the characteristics of biomass coal, which limits its application in the ironmaking process, especially its low energy density, affecting its efficiency in the coking process.
A hot-pressing method is used to prepare high-density biomass coal through mixing, heating, hot pressing, and demolding steps. The specific steps include: mixing biomass char, coal, and coal tar; heating the hot pressing mold to 420-450℃ and applying pressure of 15-25MPa; and obtaining high-density biomass coal after demolding.
It increases the bulk density and heat output of biomass coal, reduces reliance on traditional coal, reduces pollutant emissions, optimizes ironmaking processes, and improves energy efficiency and resource recycling rates.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of coking, and in particular to a method for preparing hot pressed blocks of biomass coal. Background Art
[0002] As an alternative to fossil fuels, the use of biomass-based fuels in the steel industry is one of the key strategies to reduce resource depletion and environmental pressure. Biomass energy is not only environmentally friendly but also accounts for 10% to 14% of the global primary energy supply. In the context of global energy shortage, its development potential is huge. It is a renewable carbon source, and it is expected that by 2050, biomass energy may account for 30% to 40% of total energy consumption. Biomass can not only be used to capture carbon, but it is not derived from fossil fuels, which means it can be applied to fields such as electricity, heat and transportation. Compared with fossil fuels, biomass produces less CO2 when burned, which can theoretically reduce CO2 emissions by 58%. However, due to the disadvantages of low energy density, high water content and large volume of biomass, its application is limited to a certain extent.
[0003] From a chemical point of view, biomass has a higher oxygen-to-carbon ratio (O:C) and hydrogen-to-carbon ratio (H:C), which results in a lower calorific value than fossil fuels. Therefore, raw biomass cannot be directly used in a wide range of fields, but needs to be pretreated and modified to meet the requirements of use. Biomass energy is mainly converted into fuels in different states through physical conversion (such as solid molded fuel), chemical conversion (such as direct combustion, gasification, liquefaction) and biological conversion (such as fermentation to produce methane). At present, the output of biomass coal in industrial production is still very low, about 20%. Technologies for converting biomass into coal include direct combustion, thermochemical conversion and biological conversion, but the application of the produced biomass coal in the ironmaking process is still limited by its low energy density.
[0004] To overcome these limitations, a variety of methods have been explored to increase the bulk density of coal, including tamping coking, blended coal coking and preheating coking. Internationally, the bulk density of coal charged to the furnace is usually increased by means of graded crushing, heating, tamping and increasing the height of the carbonization chamber. Studies have also found that with the increase of bulk density, the porosity and specific surface area of coke decrease, thereby reducing the reactivity of coke. Stamping coking is an unconventional coking method that mechanically tamps blended coal into briquettes and then performs high-temperature dry distillation to meet the needs of coke for different purposes. Blended coal coking is to combine coking coals of different metamorphic degrees, mix them in proportion and then coke them. This method can expand the range of coking coal, improve the strength of coke and save high-quality coking coal. Preheating coking is to preheat the coking coal to about 200°C outside the furnace before coking, which can improve the quality of coke, increase the production capacity of coke ovens, and extend the life of coke ovens. However, the existing technology has not fully considered the characteristics of biomass coal. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for preparing hot pressed biomass coal briquette to improve the overall energy utilization efficiency.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing hot pressed biomass coal briquette, the specific steps comprising:
[0008] 1) Mixing: After crushing various coals, mix them with biochar and coal tar to form biocoal; the mass content of biochar is 40%-80%, the mass content of coal is 15%-50%, and the mass content of coal tar is 5-10%;
[0009] 2) placing biomass coal into a hot pressing mold;
[0010] 3) Heating: The hot pressing mold is placed in a heating device for heating at a temperature of 420-450°C for 20-30 minutes;
[0011] 4) Hot pressing: Take out the heated hot pressing mold and put it into the press to pressurize the upper and lower molds; the operating pressure is 15MPa-25MPa, and the holding time is 3-10 seconds;
[0012] 5) Demolding: After the hot pressing mold cools down, the biomass coal briquette is demoulded and taken out.
[0013] The biochar in step 1) is obtained by thermochemical conversion and biological conversion of biomass; the biomass includes organic waste and energy plants; the diameter of the biochar is less than 5 mm.
[0014] Step 1) The coal is crushed into particles smaller than 3 mm.
[0015] In step 5), the demoulding operation is performed by using an iron punch having a diameter smaller than the inner diameter of the hot pressing mold.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] The present invention increases the bulk density of biomass coal through hot briquetting, thereby increasing the heat output during combustion. By using biomass charcoal to replace part of the coking coal, steel companies can reduce their dependence on traditional coal and improve the recycling rate of resources. As a clean energy source, the carbon dioxide produced by the combustion of biomass can be absorbed by plants, reducing greenhouse gas emissions and having little impact on the environment. In the sintering of iron ore powder, replacing part of the coke powder or coal powder with biomass can reduce pollutant emissions. The properties of biomass, such as the calorific value, characteristic combustion temperature and rate, will affect the effect of mixed coal injection, thereby optimizing the ironmaking process. DETAILED DESCRIPTION
[0018] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0019] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the embodiments, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and the like are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, features defined as "first", "second", and the like may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means more than two.
[0020] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.
[0021] A method for preparing hot pressed biomass coal briquette, the specific steps comprising:
[0022] 1) Mixing: After crushing various coals, mix them with biochar and coal tar to form biocoal; the mass content of biochar is 40%-80%, the total mass content of coal is 15%-50%, and the mass content of coal tar is 5-10%;
[0023] 2) placing biomass coal into a hot pressing mold;
[0024] 3) Heating: The hot pressing mold is placed in a heating device for heating at a temperature of 420-450°C for 20-30 minutes. The biomass coal is heated evenly, softened, and colloids are precipitated. The heating temperature cannot be too low. If it is too low, the coal tar cannot be fully softened, the colloids have not reached the precipitation temperature, or the precipitation amount is small, that is, the liquid phase that binds the biomass is small, and the final solid hot pressed block has a small crushing strength, and the quality of the obtained coke is not significantly improved; the heating temperature cannot be too high. If it is too high, the coal tar begins to volatilize after softening and melting. At this time, if it is pressurized again, cracks will appear in the hot pressed block, and its crushing strength will also decrease, which will not improve the quality of the coke.
[0025] 4) Hot pressing: Take out the heated hot pressing mold and put it into the pressurizing machine to pressurize the upper and lower molds; the hot pressing operation pressure is 15MPa-25MPa, and the holding time is 3-10 seconds; if the hot pressing pressure is too small, the density of the sample will not change much, and the colloid of coal tar in the biomass coal sample cannot be effectively pressed around the biomass, and the bonding effect of the colloid is not maximized; if the hot pressing pressure is too large, although the bonding effect of the colloid is maximized, the bearing capacity of the mold is tested, or the wall thickness of the mold is appropriately increased, which also increases the investment cost of the mold.
[0026] 5) Demolding: After the hot pressing mold has cooled down, use an iron punch with a diameter smaller than the inner diameter of the hot pressing mold to perform the demolding operation; perform the demolding operation with continuous multiple impacts with small force. Do not remove the sample at once to avoid breaking the hot pressing block.
[0027] The biochar in step 1) is obtained by thermochemical conversion and biological conversion of biomass; the biomass includes organic waste and energy plants; the diameter of the biochar is less than 5 mm.
[0028] Step 1) Coal is crushed into particles smaller than 3 mm.
[0029] The preferred embodiments of the present invention are described in detail above in conjunction with the embodiments. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, and these simple modifications all belong to the protection scope of the present invention. It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further explain various possible combinations. In addition, the various different embodiments of the present invention can also be arbitrarily combined, as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
[0030] In order to make the purpose, technical scheme and technical effect of the present invention clearer, the technical scheme in the embodiment of the present invention is now clearly and completely described. However, the embodiments described below are only part of the embodiments of the present invention, not all of the embodiments. In combination with the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Example 1
[0032] A method for preparing hot pressed biomass coal briquette, the specific steps comprising:
[0033] 1) Mixing: Coal powder, biochar and coal tar are mixed; the particle size of coal powder is less than 3mm, and the biochar is the biomass hydrothermal carbonization after biomass hydrothermal carbonization. The particle size of biomass hydrothermal carbon is less than 5mm, and the mass percentage is: biomass hydrothermal carbon: 45%, coking coal: 20%, 1 / 3 coking coal: 10%, fat coal: 10%, lean coal: 10%, coal tar: 5%. Biomass hydrothermal carbonization process: the biomass raw material is put into a high-pressure reactor, argon is introduced, and the temperature is increased to 250℃ at a rate of 10℃ / min, and kept at this temperature for 3h, and then cooled naturally. During the process, it is stirred with a magnetic stirrer at 200rpm / min and the pressure is 15MPa. Cool, filter and dry to obtain biomass hydrothermal carbon.
[0034] 2) Place the mixture into the hot pressing mold
[0035] 3) Heating: The hot pressing mold is placed in a heating device for heating at a temperature of 430° C. for 25 min.
[0036] 4) Hot pressing: Take out the heated hot pressing mold and put it into the hydraulic press for pressurization operation. The operating pressure is 20MPa and the holding time is 5 seconds.
[0037] 5) Demolding: After the hot pressing mold has cooled down, use a punch to perform demoulding.
[0038] Example 2
[0039] A method for preparing hot pressed biomass coal briquette, the specific steps comprising:
[0040] 1) Mixing: coal powder, biochar and coal tar are mixed; coal powder is less than 3mm, biochar is biochar after biomass hydrothermal carbonization treatment, the particle size of biochar is less than 3mm, mass percentage: biomass hydrothermal carbon: 50%, coking coal: 15%, 1 / 3 coking coal: 10%, fat coal: 10%, lean coal: 10%, coal tar: 5%. ; Biomass hydrothermal carbonization process: biomass raw materials are put into a high-pressure reactor, argon is introduced, and the temperature is increased to 300℃ at a rate of 10℃ / min, and the temperature is kept at this temperature for 2h, followed by natural cooling. During the process, the magnetic stirring is stirred at 300rpm / min, and the pressure is 10MPa. Cool, filter and dry to obtain biomass hydrothermal carbon.
[0041] 2) placing the mixture into a hot pressing mold;
[0042] 3) Heating: The hot pressing mold is placed in a heating device for heating at a temperature of 430° C. for 25 minutes.
[0043] 4) Hot pressing: Take out the heated hot pressing mold and put it into a press for pressurization operation, with an operating pressure of 20 MPa and a holding time of 5 seconds;
[0044] 5) Demolding: After the hot pressing mold has cooled, use an iron punch with a diameter smaller than that of the hot pressing block to perform the demoulding operation.
[0045] The hot pressed briquettes were tested in a 300kg test coke oven of the coking plant with 20% hot pressed briquettes added to the blended coal, and the test results were compared with those of bulk materials without adding hot pressed briquettes. The hot test results of the obtained coke are shown in Table 1.
[0046] Table 1 Thermal strength index of coke
[0047]
[0048] It can be seen from the test results that without changing the coal blending ratio, the quality of coke can be significantly improved through the hot pressing operation process, which can reduce the reactivity of coke by 2-3 percentage points and increase the post-reaction strength by 5-6 percentage points.
[0049] By increasing the density of biomass coal piles, the volume of fuel can be reduced, and the transportation and storage costs can be reduced. At the same time, the heat output during combustion can be increased, and the overall energy utilization efficiency can be improved. The development and application of this technology has promoted the progress of related machinery, equipment and processes, and contributed to the upgrading and development of the entire industry. By increasing the density of biomass coal piles, the storage and transportation capacity of energy is increased, which can buffer the fluctuation of energy supply to a certain extent and enhance the stability of energy supply. The application of this technology can bring economic benefits to related enterprises, such as reducing production costs and improving product quality, and it may also become a new economic growth point. Implicit effect: The use of biomass resources can promote the optimization of the energy structure of steel enterprises, improve energy utilization efficiency and reduce energy consumption. The use of biomass energy can be combined with industries such as agriculture and forestry to provide additional sources of income for rural areas and promote the sustainable development of the rural economy. By adopting biomass energy, steel enterprises can demonstrate their commitment to environmental protection and sustainable development, and enhance their sense of social responsibility and image.
[0050] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and basic spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing hot pressed biomass coal briquette, characterized in that: The specific steps include: 1) Mixing: After crushing various coals, mix them with biochar and coal tar to form biocoal; the mass content of biochar is 40%-80%, the mass content of coal is 15%-50%, and the mass content of coal tar is 5-10%; 2) placing biomass coal into a hot pressing mold; 3) Heating: The hot pressing mold is placed in a heating device for heating at a temperature of 420-450°C for 20-30 minutes; 4) Hot pressing: Take out the heated hot pressing mold and put it into the press to pressurize the upper and lower molds; the operating pressure is 15MPa-25MPa, and the holding time is 3-10 seconds; 5) Demolding: After the hot pressing mold cools down, the biomass coal briquette is demoulded and taken out.
2. The method for preparing hot pressed biomass coal according to claim 1, characterized in that: The biochar in step 1) is obtained by thermochemical conversion and biological conversion of biomass; the biomass includes organic waste and energy plants; the diameter of the biochar is less than 5 mm.
3. The method for preparing hot pressed biomass coal according to claim 1, characterized in that: Step 1) The coal is crushed into particles smaller than 3 mm.